A method for integrating carbon dioxide capture and hydrogenation to methanol using Cu-based catalysts
By doping elements such as C and P in the Cu/Al2O3 catalyst, combined with liquid phase treatment and carbon dioxide capture in the ammonia solution, the problem of deactivation of traditional copper-based catalysts due to water adsorption is solved, and the methanol yield and catalyst are improved. activity, achieving efficient CO2 utilization.
Patent Information
- Application Number
- CN202410369095.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-03-28
AI Technical Summary
The competitive adsorption of water in traditional copper-based catalysts during the hydrogenation of carbon dioxide to methanol causes catalyst deactivation and reduces the methanol yield.
By doping elements such as C and P into the Cu/Al2O3 catalyst, the structure of the copper-based catalyst is adjusted, and combined with liquid phase treatment and carbon dioxide capture in the ammonia solution, the adsorption of water is reduced and the catalyst activity is improved.
The activity of the catalyst is improved, the yield of methanol is increased, the reaction temperature and energy consumption are reduced, and the utilization process of CO2 is simplified.
Smart Images

Figure CN118059905B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of chemical engineering, and relates to a catalytic conversion technology integrating carbon dioxide capture and hydrogenation to produce methanol, and belongs to the technical field of carbon dioxide resource utilization. Background Art
[0002] In recent decades, CO2 has attracted research interest due to its greenhouse effect on global climate change. Since the 1950s, global atmospheric CO2 levels have risen rapidly and have now doubled (212ppm in 1958, 445ppm in 2021). According to relevant model calculations, CO2 levels are expected to double again by 2100. As the highest oxidation state of carbon, CO2 has a formation enthalpy of 396kJ / mol and has significant thermodynamic stability. Therefore, converting CO2 into more thermodynamically stable chemicals, such as Na2CO3, NaHCO3, NH4HCO3, and salicylic acid, provides a feasible way for production companies to deal with large amounts of CO2 emissions.
[0003] Methanol is not only an efficient energy carrier, but also a bulk chemical and an alternative fuel. Nobel Prize winner George A. Olah proposed in the early years that the synthesis of methanol from carbon dioxide resources is in line with the concept of "methanol economy". Methanol is widely used as a basic chemical raw material, and its downstream chemical products are as many as hundreds of kinds, among which formaldehyde, acetic acid and dimethyl ether are its main derivatives. In recent years, with the reduction of oil reserves, the application of methanol has gradually expanded to the field of olefin synthesis. The preparation of catalysts with excellent performance is one of the important factors for realizing the industrialization of CO2 hydrogenation to methanol. In the past 20 years, the development of CO2 hydrogenation to methanol catalysts has become a research hotspot in the field of carbon-one chemistry, and the research focuses on the selection of catalyst composition, improvement and innovation of preparation methods, optimization of reaction conditions and reaction mechanism (Chem. Rev. 2017, 117, 9804–9838). In 1960, ICI first used Cu / ZnO / Al2O3 catalyst to synthesize methanol from synthesis gas under relatively mild reaction conditions (220-300℃, 5-10MPa). Cu / ZnO / Al2O3 catalyst has become a commercial catalyst for synthesizing methanol from syngas. At present, copper-based catalysts are still the most widely used catalysts for hydrogenation of carbon dioxide to methanol in industry (ChemSusChem2020,13,6141–6159). Due to the abundance of copper resources on the earth, copper-based catalysts are economical and sustainable in catalysis.
[0004] The integration of CO2 capture and conversion can reduce the cost of CO2 utilization because it can reduce the cost of energy-consuming desorption and compression steps (ACS Sustain. Chem. Eng. 2019, 7, 12270–12280). Therefore, methanol can be directly obtained by directly using a catalyst to catalyze the hydrogenation of captured CO2 in an amine solution. After CO2 is captured, the presence of amines can change the chemical bonds of CO2, and the activated CO2 can be more efficiently hydrogenated, which reduces the reaction temperature for producing methanol (J. Catal. 2020, 389, 247–258). Directly converting CO2 active species in amine solutions into value-added chemicals can eliminate the CO2 separation process, simplify the CO2 utilization process, reduce the reaction temperature, and achieve high efficiency and energy saving (Nat. Rev. Chem. 2021, 5, 564–579; ACS Catal. 2021, 11, 12682–12691; Chem Sus Chem 2021, 14, 4812–4819).
[0005] However, traditional copper-based catalysts, such as Cu / ZnO / Al2O3, will be deactivated due to the competitive adsorption of water on the catalyst due to the formation of byproduct water during the reaction (Catal. Sci. Technol. 2018, 8, 5098–5103). By adjusting the surface properties of the catalyst, for example, by doping with inert elements such as C, the hydrophilicity of the catalyst can be reduced, thereby reducing the adsorption of water on the catalyst. By doping with elements such as P to adsorb byproduct water, the adsorption of water on Al2O3 can be reduced, and the competitive adsorption of water can also be reduced, thereby maintaining the activity of the catalyst. We adjust the structure of the copper-based catalyst by doping Cu / Al2O3 with elements such as C and P, thereby improving its catalytic performance. Summary of the invention
[0006] The main purpose of the present invention is to integrate carbon dioxide capture and hydrogenation to produce methanol in the liquid phase using a Cu-based catalyst, and to adjust the structure of the copper-based catalyst by doping elements such as C and P, in order to solve the technical problem that traditional copper-based catalysts are deactivated during the reaction, resulting in low methanol yield.
[0007] To achieve the above purpose, the present invention adopts the following two technical solutions:
[0008] 1. A method for integrating carbon dioxide capture and hydrogenation to produce methanol using a Cu-based catalyst, characterized in that it comprises the following steps:
[0009] 1) Mix a metal copper salt and a metal aluminum salt and dissolve them in deionized water by stirring, and the solution is recorded as solution a; add ammonia water to deionized water to obtain diluted ammonia water, and dissolve a soluble sugar (one of sucrose, glucose, and fructose) as a carbon source in the diluted ammonia water, and the obtained solution is recorded as solution b; add solution a dropwise to solution b, age in a beaker for 2 hours, place in an oil bath, stir and dry at 50-70° C., and then transfer to a 90-100° C. oven for drying for 12 hours to obtain a dried material; the dried material is transferred to a muffle furnace, calcined at 300-600° C. for 3-14 hours, ground, and then reduced in a tubular furnace, and reduced at 300-600° C. for 1-12 hours under hydrogen to obtain three carbon-doped copper-based catalysts, namely Cu / Al2O3-sucrose, Cu / Al2O3-glucose, and Cu / Al2O3-fructose, where sucrose, glucose, and fructose represent sucrose, glucose, and fructose, respectively;
[0010] 2) adding anhydrous ethanol to a reaction kettle; then adding a catalyst mixture equivalent to 0.1 to 10 wt % of anhydrous ethanol to the reaction kettle, wherein the catalyst may be one or more of Cu / Al2O3-sucrose, Cu / Al2O3-glucose, and Cu / Al2O3-fructose; then filling with 0.1 to 1 MPa of carbon dioxide and 2 to 20 MPa of hydrogen; then the reaction kettle is reacted at 150 to 250° C. and a rotation speed of 600 to 1000 rpm for 2 to 24 hours; after cooling, a reaction solution containing methanol can be obtained, and the yield of methanol is analyzed by gas chromatography.
[0011] 2. A method for integrating carbon dioxide capture and hydrogenation to produce methanol using a Cu-based catalyst, characterized in that it comprises the following steps:
[0012] 1) Mix a metal copper salt and a metal aluminum salt and dissolve them in deionized water by stirring, and the solution is recorded as solution a; add ammonia water to deionized water to obtain diluted ammonia water, and dissolve a soluble sugar (one of sucrose, glucose, and fructose) as a carbon source in the diluted ammonia water, and the obtained solution is recorded as solution b; add solution a dropwise to solution b, age in a beaker for 2 hours, place in an oil bath, stir and dry at 50-70° C., and then transfer to a 90-100° C. oven for drying for 12 hours to obtain a dried material; the dried material is transferred to a muffle furnace, calcined at 300-600° C. for 3-14 hours, ground, and then reduced in a tubular furnace, and reduced at 300-600° C. for 1-12 hours under hydrogen to obtain three carbon-doped copper-based catalysts, namely Cu / Al2O3-sucrose, Cu / Al2O3-glucose, and Cu / Al2O3-fructose, where sucrose, glucose, and fructose represent sucrose, glucose, and fructose, respectively;
[0013] 2) adding triethylamine equivalent to 0.5-20% of anhydrous ethanol to anhydrous ethanol to obtain an ethanol solution of amine; placing the ethanol solution of amine in a reaction kettle, adding a catalyst equivalent to 0.1-10wt% of the ethanol solution of amine to the ethanol solution of amine in the reaction kettle, wherein the catalyst may be one or more of Cu / Al2O3-sucrose, Cu / Al2O3-glucose, and Cu / Al2O3-fructose; then charging with 0.1-1MPa carbon dioxide and 2-20MPa hydrogen; then reacting the reaction kettle at 150-250°C and a rotation speed of 600-1000rpm for 2-24 hours; after cooling, a reaction solution containing methanol can be obtained, and the yield of methanol is analyzed by gas chromatography.
[0014] 3. A method for integrating carbon dioxide capture and hydrogenation to produce methanol using a Cu-based catalyst, characterized in that it comprises the following steps:
[0015] 1) Mix a metal copper salt and a metal aluminum salt and dissolve them in deionized water by stirring, and the solution is recorded as solution a; add ammonia water to deionized water to obtain diluted ammonia water, and dissolve phosphoric acid as a phosphorus source in the diluted ammonia water, and the obtained solution is recorded as solution b; add solution a dropwise to solution b, age in a beaker for 2 hours, place in an oil bath, stir and dry at 50-70° C., and then transfer to a 90-100° C. oven for drying for 12 hours to obtain a dried material; transfer the dried material to a muffle furnace, calcine at 300-600° C. for 3-14 hours, grind, and then reduce in a tubular furnace, and reduce at 300-600° C. for 1-12 hours under hydrogen to obtain Cu / Al2O3-phosphoric, a copper-based catalyst doped with phosphorus, where phosphoric represents phosphoric acid;
[0016] 2) adding anhydrous ethanol to a reaction kettle; then adding a catalyst mixture equivalent to 0.1 to 10 wt% of anhydrous ethanol to the reaction kettle, wherein the catalyst is Cu / Al2O3-phosphoric; then filling with 0.1 to 1 MPa of carbon dioxide and 2 to 20 MPa of hydrogen; then the reaction kettle is reacted at 150 to 250° C. and 600 to 1000 rpm for 2 to 24 hours; after cooling, a reaction liquid containing methanol can be obtained, and the yield of methanol is analyzed by gas chromatography.
[0017] 4. A method for integrating carbon dioxide capture and hydrogenation to produce methanol using a Cu-based catalyst, characterized in that it comprises the following steps:
[0018] 1) Mix a metal copper salt and a metal aluminum salt and dissolve them in deionized water by stirring, and the solution is recorded as solution a; add ammonia water to deionized water to obtain diluted ammonia water, and dissolve phosphoric acid as a phosphorus source in the diluted ammonia water, and the obtained solution is recorded as solution b; add solution a dropwise to solution b, age in a beaker for 2 hours, place in an oil bath, stir and dry at 50-70° C., and then transfer to a 90-100° C. oven for drying for 12 hours to obtain a dried material; transfer the dried material to a muffle furnace, calcine at 300-600° C. for 3-14 hours, grind, and then reduce in a tubular furnace, and reduce at 300-600° C. for 1-12 hours under hydrogen to obtain Cu / Al2O3-phosphoric, a copper-based catalyst doped with phosphorus, where phosphoric represents phosphoric acid;
[0019] 2) adding triethylamine equivalent to 0.5-20% of anhydrous ethanol to anhydrous ethanol to obtain an ethanol solution of amine; placing the ethanol solution of amine in a reaction kettle, adding a catalyst equivalent to 0.1-10wt% of the ethanol solution of amine to the ethanol solution of amine in the reaction kettle, wherein the catalyst is Cu / Al2O3-phosphoric; then charging 0.1-1MPa of carbon dioxide and 2-20MPa of hydrogen; then reacting the reaction kettle at 150-250°C and a rotation speed of 600-1000rpm for 2-24 hours; after cooling, a reaction solution containing methanol can be obtained, and the yield of methanol is analyzed by gas chromatography.
[0020] The present invention adopts the above technical solution, which has the following advantages:
[0021] In view of the high energy consumption of industrial production of methanol by hydrogenation of carbon dioxide in the gas phase, we proposed to use Cu-based catalysts to integrate carbon dioxide capture and hydrogenation to produce methanol in the liquid phase. We have developed a new catalyst preparation method, which reduces the competitive adsorption of water formed during the hydrogenation of carbon dioxide by doping C and P on the supported copper-based catalyst, so that the doped copper-based catalyst has better activity and the yield of methanol is also improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 : Methanol yield obtained by catalytic conversion of carbon dioxide in pure ethanol solvent using different catalysts.
[0023] Figure 2 : Methanol yield obtained by catalytic conversion of carbon dioxide with different catalysts in ethanol solvent with added triethylamine. DETAILED DESCRIPTION
[0024] The present invention is described in detail below by way of examples.
[0025] Example 1
[0026] There are four steps to prepare 20wt% Cu / Al2O3 catalyst:
[0027] In the first step, 2.94 g Al(NO3)3·9H2O and 0.38 g Cu(NO3)2·3H2O were mixed and dissolved in 20 mL deionized water, and stirred at 500 rpm to dissolve.
[0028] In the second step, 4.2 mL of ammonia water was taken, and then deionized water was added to 20 mL, and the mixture was stirred and dissolved at 500 rpm to obtain an ammonia solution. The solution of the first step was then added dropwise to the ammonia solution and aged for 2 h.
[0029] In the third step, the solution from the second step was placed in an oil bath and stirred at 50-70°C until dry, and then transferred to a 90°C oven for drying for 12 hours.
[0030] The fourth step is to place the sample obtained in the third step in a muffle furnace and calcine it at 400°C for 3 hours, and then reduce it in a tubular furnace at 400°C for 2 hours in a hydrogen atmosphere to obtain a 20wt% Cu / Al2O3 catalyst.
[0031] Reaction part:
[0032] First, 20 mL of ethanol was added into the reactor, and then 0.3 g of 20 wt% Cu / Al2O3 catalyst was placed into the reactor, and 0.5 MPa CO2 and 3.5 MPa H2 were filled into the reactor. The reaction was carried out at 200°C for 6 hours, and a reaction solution containing methanol was obtained.
[0033] Example 2
[0034] There are four steps to prepare 20wt% Cu / Al2O3-sucrose catalyst:
[0035] In the first step, 2.94 g Al(NO3)3·9H2O and 0.38 g Cu(NO3)2·3H2O were mixed and dissolved in 20 mL deionized water, and stirred at 500 rpm to dissolve.
[0036] In the second step, take 4.2 mL of ammonia water, then add deionized water to 20 mL, then add 2 g of fructose (sucrose), stir and dissolve at 500 rpm to obtain an aqueous solution of sucrose, then add the solution of the first step dropwise into the aqueous solution of sucrose, and then age for 2 hours.
[0037] In the third step, the solution from the second step was placed in an oil bath and stirred at 50-70°C until dry, and then transferred to a 90°C oven for drying for 12 hours.
[0038] The fourth step is to place the sample obtained in the third step in a muffle furnace and calcine it at 400°C for 3 hours, and then reduce it in a tubular furnace at 400°C for 2 hours in a hydrogen atmosphere to obtain a 20wt% Cu / Al2O3-sucrose catalyst.
[0039] Reaction part:
[0040] First, 20 mL of ethanol was added into the reactor, and 0.3 g of 20 wt% Cu / Al2O3-sucrose catalyst was placed into the reactor, and 0.5 MPa CO2 and 3.5 MPa H2 were charged into the reactor. The reaction was carried out at 200°C for 6 hours, and a reaction solution containing methanol was obtained.
[0041] Example 3
[0042] There are four steps to prepare 20wt% Cu / Al2O3-glucose catalyst:
[0043] In the first step, 2.94 g Al(NO3)3·9H2O and 0.38 g Cu(NO3)2·3H2O were mixed and dissolved in 20 mL deionized water, and stirred at 500 rpm to dissolve.
[0044] In the second step, take 4.2 mL of ammonia water, then add deionized water to 20 mL, then add 2 g of glucose, stir and dissolve at 500 rpm to obtain an aqueous solution of glucosamine, then add the solution of the first step dropwise to the aqueous solution of glucosamine, and then age for 2 hours.
[0045] In the third step, the solution from the second step was placed in an oil bath and stirred at 50-70°C until dry, and then transferred to a 90°C oven for drying for 12 hours.
[0046] In the fourth step, the sample obtained in the third step was placed in a muffle furnace and calcined at 400°C for 3 hours, and then reduced in a tubular furnace at 400°C for 2 hours in a hydrogen atmosphere to obtain a 20wt% Cu / Al2O3-glucose catalyst.
[0047] Reaction part:
[0048] First, 20 mL of ethanol was added into the reactor, and 0.3 g of 20 wt% Cu / Al2O3-glucose catalyst was placed into the reactor, and 0.5 MPa CO2 and 3.5 MPa H2 were charged into the reactor. The reaction was carried out at 200°C for 6 hours, and a reaction solution containing methanol was obtained.
[0049] Example 4
[0050] There are four steps to prepare 20wt% Cu / Al2O3-fructose catalyst:
[0051] In the first step, 2.94 g Al(NO3)3·9H2O and 0.38 g Cu(NO3)2·3H2O were mixed and dissolved in 20 mL deionized water, and stirred at 500 rpm to dissolve.
[0052] In the second step, take 4.2 mL of ammonia water, then add deionized water to 20 mL, then add 2 g of fructose, stir and dissolve at 500 rpm to obtain an aqueous solution of glucosamine, then add the solution of the first step dropwise to the aqueous solution of glucosamine, and then age for 2 hours.
[0053] In the third step, the solution from the second step was placed in an oil bath and stirred at 50-70°C until dry, and then transferred to a 90°C oven for drying for 12 hours.
[0054] In the fourth step, the sample obtained in the third step was placed in a muffle furnace and calcined at 400°C for 3 hours, and then reduced in a tubular furnace at 400°C for 2 hours in a hydrogen atmosphere to obtain a 20wt% Cu / Al2O3-fructose catalyst.
[0055] Reaction part:
[0056] First, 20 mL of ethanol was added into the reactor, and 0.3 g of 20 wt% Cu / Al2O3-fructose catalyst was placed into the reactor, and 0.5 MPa CO2 and 3.5 MPa H2 were filled into the reactor. The reaction was carried out at 200°C for 6 hours to obtain a reaction solution containing methanol.
[0057] Example 5
[0058] There are four steps to prepare 20wt% Cu / Al2O3-phosphoric catalyst:
[0059] In the first step, 2.94 g Al(NO3)3·9H2O and 0.38 g Cu(NO3)2·3H2O were mixed and dissolved in 20 mL deionized water, and stirred at 500 rpm to dissolve.
[0060] In the second step, take 4.2 mL of ammonia water, then add deionized water to 20 mL, then add 0.0309 g of phosphoric acid, stir and dissolve at 500 rpm to obtain an ammonia phosphoric acid aqueous solution, then add the solution of the first step dropwise to the ammonia phosphoric acid aqueous solution, and then age for 2 hours.
[0061] In the third step, the solution from the second step was placed in an oil bath and stirred at 50-70°C until dry, and then transferred to a 90°C oven for drying for 12 hours.
[0062] In the fourth step, the sample obtained in the third step was placed in a muffle furnace and calcined at 400°C for 3 hours, and then reduced in a tubular furnace at 400°C for 2 hours in a hydrogen atmosphere to obtain a 20wt% Cu / Al2O3-phosphoric catalyst.
[0063] Reaction part:
[0064] First, 20 mL of ethanol was added into a reactor, and 0.3 g of 20 wt% Cu / Al2O3-phosphoric catalyst was placed into the reactor, and 0.5 MPa CO2 and 3.5 MPa H2 were charged into the reactor. The reaction was carried out at 200° C. for 6 hours, and a reaction liquid containing methanol was obtained.
[0065] The yield of methanol is expressed as the molar amount of methanol divided by the molar amount of carbon dioxide as the reaction raw material. The yields of methanol obtained in Examples 1-5 are as follows: Figure 1 shown.
[0066] Example 6
[0067] There are four steps to prepare 20wt% Cu / Al2O3 catalyst:
[0068] In the first step, 2.94 g Al(NO3)3·9H2O and 0.38 g Cu(NO3)2·3H2O were mixed and dissolved in 20 mL deionized water, and stirred at 500 rpm to dissolve.
[0069] In the second step, 4.2 mL of ammonia water was taken, and then deionized water was added to 20 mL, and the mixture was stirred and dissolved at 500 rpm to obtain an ammonia solution. The solution of the first step was then added dropwise to the ammonia solution and aged for 2 h.
[0070] In the third step, the solution from the second step was placed in an oil bath and stirred at 50-70°C until dry, and then transferred to a 90°C oven for drying for 12 hours.
[0071] The fourth step is to place the sample obtained in the third step in a muffle furnace and calcine it at 400°C for 3 hours, and then reduce it in a tubular furnace at 400°C for 2 hours in a hydrogen atmosphere to obtain a 20wt% Cu / Al2O3 catalyst.
[0072] Reaction part:
[0073] First, 19 mL of ethanol and 1 mL of triethylamine were mixed and added to a reactor, 0.3 g of 20 wt% Cu / Al2O3 catalyst was added to the reactor, 0.5 MPa CO2 and 3.5 MPa H2 were introduced, and the reaction was carried out at 200°C for 6 hours to obtain a reaction solution containing methanol.
[0074] Example 7
[0075] There are four steps to prepare 20wt% Cu / Al2O3-sucrose catalyst:
[0076] In the first step, 2.94 g Al(NO3)3·9H2O and 0.38 g Cu(NO3)2·3H2O were mixed and dissolved in 20 mL deionized water, and stirred at 500 rpm to dissolve.
[0077] In the second step, take 4.2 mL of ammonia water, then add deionized water to 20 mL, then add 2 g of fructose (sucrose), stir and dissolve at 500 rpm to obtain an aqueous solution of sucrose, then add the solution of the first step dropwise into the aqueous solution of sucrose, and then age for 2 hours.
[0078] In the third step, the solution from the second step was placed in an oil bath and stirred at 50-70°C until dry, and then transferred to a 90°C oven for drying for 12 hours.
[0079] The fourth step is to place the sample obtained in the third step in a muffle furnace and calcine it at 400°C for 3 hours, and then reduce it in a tubular furnace at 400°C for 2 hours in a hydrogen atmosphere to obtain a 20wt% Cu / Al2O3-sucrose catalyst.
[0080] Reaction part:
[0081] First, 19 mL of ethanol and 1 mL of triethylamine were mixed and added to a reactor, 0.3 g of 20 wt% Cu / Al2O3-sucrose catalyst was added to the reactor, 0.5 MPa CO2 and 3.5 MPa H2 were charged, and the reaction was carried out at 200°C for 6 hours to obtain a reaction solution containing methanol.
[0082] Example 8
[0083] There are four steps to prepare 20wt% Cu / Al2O3-glucose catalyst:
[0084] In the first step, 2.94 g Al(NO3)3·9H2O and 0.38 g Cu(NO3)2·3H2O were mixed and dissolved in 20 mL deionized water, and stirred at 500 rpm to dissolve.
[0085] In the second step, take 4.2 mL of ammonia water, then add deionized water to 20 mL, then add 2 g of glucose, stir and dissolve at 500 rpm to obtain an aqueous solution of glucosamine, then add the solution of the first step dropwise to the aqueous solution of glucosamine, and then age for 2 hours.
[0086] In the third step, the solution from the second step was placed in an oil bath and stirred at 50-70°C until dry, and then transferred to a 90°C oven for drying for 12 hours.
[0087] In the fourth step, the sample obtained in the third step was placed in a muffle furnace and calcined at 400°C for 3 hours, and then reduced in a tubular furnace at 400°C for 2 hours in a hydrogen atmosphere to obtain a 20wt% Cu / Al2O3-glucose catalyst.
[0088] Reaction part:
[0089] First, 19 mL of ethanol and 1 mL of triethylamine were mixed and added to a reactor, 0.3 g of 20 wt% Cu / Al2O3-glucose catalyst was added to the reactor, 0.5 MPa CO2 and 3.5 MPa H2 were introduced, and the reaction was carried out at 200°C for 6 hours to obtain a reaction solution containing methanol.
[0090] Example 9
[0091] There are four steps to prepare 20wt% Cu / Al2O3-fructose catalyst:
[0092] In the first step, 2.94 g Al(NO3)3·9H2O and 0.38 g Cu(NO3)2·3H2O were mixed and dissolved in 20 mL deionized water, and stirred at 500 rpm to dissolve.
[0093] In the second step, take 4.2 mL of ammonia water, then add deionized water to 20 mL, then add 2 g of fructose, stir and dissolve at 500 rpm to obtain an aqueous solution of glucosamine, then add the solution of the first step dropwise to the aqueous solution of glucosamine, and then age for 2 hours.
[0094] In the third step, the solution from the second step was placed in an oil bath and stirred at 50-70°C until dry, and then transferred to a 90°C oven for drying for 12 hours.
[0095] In the fourth step, the sample obtained in the third step was placed in a muffle furnace and calcined at 400°C for 3 hours, and then reduced in a tubular furnace at 400°C for 2 hours in a hydrogen atmosphere to obtain a 20wt% Cu / Al2O3-fructose catalyst.
[0096] Reaction part:
[0097] First, 19 mL of ethanol and 1 mL of triethylamine were mixed and added to a reactor, 0.3 g of 20 wt% Cu / Al2O3-fructose catalyst was added to the reactor, 0.5 MPa CO2 and 3.5 MPa H2 were charged, and the reaction was carried out at 200°C for 6 hours to obtain a reaction solution containing methanol.
[0098] Example 10
[0099] There are four steps to prepare 20wt% Cu / Al2O3-phosphoric catalyst:
[0100] In the first step, 2.94 g Al(NO3)3·9H2O and 0.38 g Cu(NO3)2·3H2O were mixed and dissolved in 20 mL deionized water, and stirred at 500 rpm to dissolve.
[0101] In the second step, take 4.2 mL of ammonia water, then add deionized water to 20 mL, then add 0.0309 g of phosphoric acid, stir and dissolve at 500 rpm to obtain an ammonia phosphoric acid aqueous solution, then add the solution of the first step dropwise to the ammonia phosphoric acid aqueous solution, and then age for 2 hours.
[0102] In the third step, the solution from the second step was placed in an oil bath and stirred at 50-70°C until dry, and then transferred to a 90°C oven for drying for 12 hours.
[0103] In the fourth step, the sample obtained in the third step was placed in a muffle furnace and calcined at 400°C for 3 hours, and then reduced in a tubular furnace at 400°C for 2 hours in a hydrogen atmosphere to obtain a 20wt% Cu / Al2O3-phosphoric catalyst.
[0104] Reaction part:
[0105] First, 1 mL of triethylamine and 19 mL of ethanol were mixed and added to a reactor, 0.3 g of 20 wt% Cu / Al2O3-phosphoric catalyst was added to the reactor, 0.5 MPa CO2 and 3.5 MPa H2 were introduced, and the reaction was carried out at 200°C for 6 hours to obtain a reaction solution containing methanol.
[0106] The yield of methanol is expressed as the molar amount of methanol divided by the molar amount of carbon dioxide as the reaction raw material. The yields of methanol obtained in Examples 6-10 are as follows: Figure 2 shown.
Claims
1. A method for integrating carbon dioxide capture and hydrogenation to produce methanol using a Cu-based catalyst, characterized in that: The following steps are involved: 1) Mix a metal copper salt and a metal aluminum salt and dissolve them in deionized water by stirring, and the solution is recorded as solution a; add ammonia water to deionized water to obtain diluted ammonia water, dissolve soluble sugar as a carbon source in the diluted ammonia water, and the obtained solution is recorded as solution b; add solution a dropwise to solution b, age for 1 to 12 hours, stir and dry at 30 to 90° C., and then transfer to 90 to 120° C. and dry for 1 to 12 hours to obtain a dried material; transfer the dried material to a muffle furnace, calcine at 300 to 600° C. for 3 to 14 hours, grind it, and then reduce it in a tubular furnace, and reduce it at 300 to 600° C. for 1 to 12 hours under hydrogen to obtain a carbon-doped copper-based catalyst; 2) adding anhydrous alcohol into a reaction kettle; then adding a carbon-doped copper-based catalyst equivalent to 0.1-10 wt% of anhydrous alcohol into the reaction kettle; then charging 0.1-1 MPa of carbon dioxide and 2-20 MPa of hydrogen into the reaction kettle; then reacting the reaction kettle at 150-250° C. and 600-1000 rpm for 2-24 hours; after cooling, a reaction solution containing methanol can be obtained.
2. A method for integrating carbon dioxide capture and hydrogenation to produce methanol using a Cu-based catalyst, characterized in that: The following steps are involved: 1) Mix a metal copper salt and a metal aluminum salt and dissolve them in deionized water by stirring, and the solution is recorded as solution a; add ammonia water to deionized water to obtain diluted ammonia water, dissolve soluble sugar as a carbon source in the diluted ammonia water, and the obtained solution is recorded as solution b; add solution a dropwise to solution b, age for 1 to 12 hours, stir and dry at 30 to 90° C., and then transfer to 90 to 120° C. and dry for 1 to 12 hours to obtain a dried material; transfer the dried material to a muffle furnace, calcine at 300 to 600° C. for 3 to 14 hours, grind it, and then reduce it in a tubular furnace, and reduce it at 300 to 600° C. for 1 to 12 hours under hydrogen to obtain a carbon-doped copper-based catalyst; 2) adding an amine equivalent to 0.5-20 wt% of anhydrous alcohol to anhydrous alcohol to obtain an alcohol solution of the amine; placing the alcohol solution of the amine in a reaction kettle, and then adding a carbon-doped copper-based catalyst equivalent to 0.1-10 wt% of the alcohol solution of the amine to the alcohol solution of the amine in the reaction kettle to mix; then filling the reaction kettle with 0.1-1 MPa of carbon dioxide and 2-20 MPa of hydrogen; then reacting the reaction kettle at 150-250° C. and a rotation speed of 600-1000 rpm for 2-24 hours; after cooling, a reaction solution containing methanol can be obtained.
3. A method for integrating carbon dioxide capture and hydrogenation to produce methanol using a Cu-based catalyst, characterized in that: The following steps are involved: 1) Mix a metal copper salt and a metal aluminum salt and dissolve them in deionized water by stirring, and the solution is recorded as solution a; add ammonia water to deionized water to obtain diluted ammonia water, and dissolve phosphoric acid as a phosphorus source in the diluted ammonia water, and the obtained solution is recorded as solution b; add solution a dropwise to solution b, age for 1 to 12 hours, stir and dry at 30 to 90° C., and then transfer to 90 to 120° C. and dry for 1 to 12 hours to obtain a dried material; transfer the dried material to a muffle furnace, calcine at 300 to 600° C. for 3 to 14 hours, grind it, and then reduce it in a tubular furnace, and reduce it at 300 to 600° C. for 1 to 12 hours under hydrogen to obtain Cu / Al2O3-phosphoric, a copper-based catalyst doped with phosphorus, where phosphoric represents phosphoric acid; 2) adding anhydrous alcohol into a reaction kettle; then adding a catalyst mixture equivalent to 0.1-10 wt% of anhydrous alcohol into the reaction kettle, wherein the catalyst is Cu / Al2O3-phosphoric; then charging the reaction kettle with 0.1-1 MPa of carbon dioxide and 2-20 MPa of hydrogen; then reacting the reaction kettle at 150-250° C. and 600-1000 rpm for 2-24 hours; after cooling, a reaction solution containing methanol can be obtained.
4. A method for integrating carbon dioxide capture and hydrogenation to produce methanol using a Cu-based catalyst, characterized in that: The following steps are involved: 1) Mix a metal copper salt and a metal aluminum salt and dissolve them in deionized water by stirring, and the solution is recorded as solution a; add ammonia water to deionized water to obtain diluted ammonia water, and dissolve phosphoric acid as a phosphorus source in the diluted ammonia water, and the obtained solution is recorded as solution b; add solution a dropwise to solution b, age for 1 to 12 hours, stir and dry at 30 to 90° C., and then transfer to 90 to 120° C. and dry for 1 to 12 hours to obtain a dried material; transfer the dried material to a muffle furnace, calcine at 300 to 600° C. for 3 to 14 hours, grind it, and then reduce it in a tubular furnace, and reduce it at 300 to 600° C. for 1 to 12 hours under hydrogen to obtain Cu / Al2O3-phosphoric, a copper-based catalyst doped with phosphorus, where phosphoric represents phosphoric acid; 2) adding an amine equivalent to 0.5-20% of anhydrous alcohol to anhydrous alcohol to obtain an alcohol solution of the amine; placing the alcohol solution of the amine in a reaction kettle, and then adding a catalyst equivalent to 0.1-10wt% of the alcohol solution of the amine to the alcohol solution of the amine in the reaction kettle, wherein the catalyst is Cu / Al2O3-phosphoric; then charging the reaction kettle with 0.1-1MPa of carbon dioxide and 2-20MPa of hydrogen; then reacting the reaction kettle at 150-250°C and a rotation speed of 600-1000rpm for 2-24 hours; after cooling, a reaction solution containing methanol can be obtained.
5. The method according to any one of claims 1 to 4, characterized in that: The metal copper salt is one or more of copper nitrate, copper acetate, copper sulfate, copper phosphate, copper carbonate, copper aluminate, and copper chloride; the metal aluminum salt is one or more of aluminum nitrate, aluminum acetate, aluminum sulfate, aluminum phosphate, and aluminum chloride; and the concentration of the obtained diluted ammonia water is 1-20wt%.
6. The method according to claim 1 or 2, characterized in that: The soluble sugars are one or more of sucrose, glucose, fructose, mannose, lactose, galactose, ribose, xylose, arabinose, mannose, maltose and deoxyribose.
7. The method according to claim 3 or 4, characterized in that: The mass ratio of phosphoric acid to diluted ammonia water is 1:100 to 100:
1.
8. The method according to claim 1 or 2, characterized in that: The carbon-doped copper-based catalyst is one or more of Cu / Al2O3-sucrose, Cu / Al2O3-glucose, Cu / Al2O3-fructose, Cu / Al2O3-mannose, Cu / Al2O3-lactose, Cu / Al2O3-galactose, Cu / Al2O3-ribose, Cu / Al2O3-xylose, Cu / Al2O3-arabinose, Cu / Al2O3-mannose, Cu / Al2O3-maltose, and Cu / Al2O3-deoxyribose, where sucrose, glucose, fructose, mannose, lactose, galactose, ribose, xylose, arabinose, mannose, maltose and deoxyribose represent sucrose, glucose, fructose, mannose, lactose, galactose, ribose, ribose, xylose, arabinose, mannose, maltose and deoxyribose, respectively.
9. The method according to any one of claims 1 or 3, wherein the volume of the anhydrous alcohol added is 10 to 80% of the volume of the reactor; the type of the anhydrous alcohol is one or more of methanol, ethanol, propanol, butanol, pentanol, hexanol, ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, 1,4-butylene glycol, 1,3-butylene glycol, 2,3-butylene glycol, 1,5-pentanediol, and glycerol.
10. The method according to any one of claims 2 or 4, wherein the volume of the alcohol solution of the amine added is 10-80% of the volume of the reactor; the type of anhydrous alcohol is one or more of methanol, ethanol, propanol, butanol, pentanol, hexanol, ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, 1,4-butanediol, 1,3-butanediol, 2,3-butanediol, 1,5-pentanediol, and glycerol; the type of amine is one or more of trimethylamine, triethylamine, tripropylamine, tributylamine, trimethylolamine, triethanolamine, tripropanolamine, tributanolamine, N-methylpiperidine, N-ethylpiperidine, N-propylpiperidine, N-methylpiperidine, N-ethanolpiperidine, N-propanolpiperidine, N-methylpyrrolidine, N-ethylpyrrolidine, N-propylpyrrolidine, N-methylpyrrolidine, N-ethanolpyrrolidine, and N-propanolpyrrolidine.