A carbon fiber composite material and its preparation method and application
By combining polydopamine and octaaminopropylsilsesquioxane to modify carbon fiber and epoxy resin, and adding modified ammonium polyphosphate to the composite, the thermal stability and flammability problems of carbon fiber composites at high temperatures are solved. , achieving the preparation of carbon fiber composite materials with high mechanical properties and good flame retardant properties.
Patent Information
- Application Number
- CN202410314892.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-03-19
AI Technical Summary
Carbon fiber composite materials have poor thermal stability in high-temperature environments, and organic resin-based materials are easy to burn, which limits their application in certain fields.
Polydopamine is used to pre-modify carbon fiber and combined with octaaminopropylsilsesquioxane to form POSS-modified carbon fiber, which is added to epoxy resin, and halogen-free flame retardant modified ammonium polyphosphate is added to the resin glue. Preparation of carbon fiber composite materials by hot press molding.
It improves the mechanical properties and thermal stability of composite materials, maintains a high oxygen index and UL-94 rating, and significantly improves flame retardant properties, making it suitable for the field of building materials.
Smart Images

Figure BDA0004748617230000061 
Figure BDA0004748617230000071
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of composite materials, and in particular relates to a carbon fiber composite material and a preparation method and application thereof. Background Art
[0002] Carbon fiber composites are made of carbon fiber and resin-based composite materials. Carbon fiber is a fibrous material composed of carbon elements, which has high strength and stiffness. The modulus of carbon fiber is higher than that of traditional metal materials. The weight of carbon fiber composites is only about 1 / 4 of that of traditional metal materials, but its strength is more than twice that of traditional metal materials. Therefore, carbon fiber composites have better resistance to deformation and load-bearing capacity, and have the advantages of light weight, high strength, high modulus, and corrosion resistance.
[0003] Carbon fiber composites are increasingly used in this field due to their advantages such as high strength, low thermal expansion coefficient, small heat capacity and small specific gravity. However, carbon fiber composites also have some disadvantages. First, the performance of carbon fiber composites will be affected at high temperatures, and they are prone to softening and failure. Therefore, their application in high temperature environments needs further improvement. Secondly, the flammable nature of organic resin-based materials limits their application in many fields. The development of high-performance flame-retardant carbon fiber composites is of great significance.
[0004] As one of the raw materials of resin-based composite materials, epoxy resin is widely used in engineering construction bonding, building gap filling and building reinforcement and repair, but its flammable properties limit its application. Therefore, it is of great significance to develop high-performance flame-retardant carbon fiber reinforced epoxy resin composites. Summary of the invention
[0005] The object of the present invention is to provide a carbon fiber composite material and a preparation method thereof to solve the problem of poor thermal stability of the carbon fiber composite material.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A method for preparing a carbon fiber composite material comprises the following steps:
[0008] Adding octaaminopropyl silsesquioxane to a Tris buffer having a pH value of 8.5, and stirring, washing with water, and drying to obtain POSS-modified carbon fiber, wherein the amount of octaaminopropyl silsesquioxane added to the Tris buffer is 2-5 mg / L;
[0009] The POSS-modified carbon fiber is added into epoxy resin glue for immersion to obtain prepreg, and multiple layers of prepreg are laid and hot-pressed to obtain a carbon fiber composite material.
[0010] Furthermore, the resin glue includes epoxy resin and curing agent, and the mass ratio of epoxy resin to curing agent in the epoxy resin glue is 10:1; the epoxy resin is E51, the epoxy value is 0.52 mol / 100g, and the density is 1.2g / cm 3 , curing agent diethyltoluenediamine.
[0011] Furthermore, the resin glue liquid also includes a halogen-free flame retardant, and the added amount of the halogen-free flame retardant is 10% of the mass of the resin liquid.
[0012] Furthermore, the pressure of the hot pressing molding is 0.5-0.6 MPa, and the temperature of the hot pressing molding is 180-200°C.
[0013] Furthermore, the halogen-free flame retardant is modified ammonium polyphosphate, which is prepared by the following steps:
[0014] Adding an alkyl silane coupling agent into an ethanol aqueous solution, adjusting the system to be weakly acidic, and stirring to obtain a hydrolyzate;
[0015] Add ammonium polyphosphate to ethanol, then add γ-aminopropyltriethoxysilane, heat and stir to react, add the above hydrolyzate, keep the temperature unchanged after adding, continue stirring, after stirring, centrifuge, wash and dry to obtain modified ammonium polyphosphate.
[0016] Furthermore, the alkylsilane coupling agent is one of n-hexyltrimethoxysilane, octyltrimethoxysilane, tetradecyltrimethoxysilane, and hexadecyltrimethoxysilane. Different alkylsilane coupling agents are combined with ammonium polyphosphate modified with γ-aminopropyltriethoxysilane through hydrolysis, thereby improving the hydrolysis resistance of ammonium polyphosphate, improving the compatibility of ammonium polyphosphate in composite materials, and further improving the application of ammonium polyphosphate as a flame retardant in composite materials.
[0017] Further, the polydopamine pre-modified carbon fiber is prepared by the following steps:
[0018] The oxidized carbon fiber is added to a Tris buffer with a pH value of 8.5, dopamine is added, and the mixture is stirred at room temperature. After the stirring is completed, the mixture is centrifuged, washed, and filtered to obtain polydopamine pre-modified carbon fiber; the content of dopamine in the buffer is 2-5 mg / mL.
[0019] Furthermore, the oxidized carbon fiber is a carbon fiber oxidized by soaking in concentrated nitric acid, and is prepared by the following steps:
[0020] Soak the carbon fiber in acetone to wash the surface impurities, and then soak it in concentrated nitric acid solution for 100-120 minutes after drying. After taking it out, wash it with water and dry it to obtain oxidized carbon fiber. After oxidation treatment with concentrated nitric acid, the surface of the carbon fiber will be oxidized and etched, and grooves will be left after etching, which not only increases the roughness of the carbon fiber surface, but also increases the area of subsequent reactions.
[0021] A carbon fiber composite material is prepared by the above preparation method.
[0022] The above carbon fiber composite materials are used in building materials.
[0023] Beneficial effects of the present invention:
[0024] The invention provides a carbon fiber composite material, which is composed of POSS-modified carbon fiber and epoxy resin and has good mechanical properties and thermal stability. When a low content of halogen-free flame retardant is added to the composite material, the UL-94 grade can maintain a V-0 grade and a high oxygen index, and the mechanical properties of the composite material after adding the flame retardant can be maintained at a high level, and the composite material has high mechanical properties and stability.
[0025] The POSS-modified carbon fiber used in the carbon fiber composite material of the present invention is composed of polydopamine pre-modified carbon fiber and octaaminopropyl silsesquioxane, and the octaaminopropyl silsesquioxane can react with the polydopamine pre-modified carbon fiber to improve the roughness of the fiber surface as a modifier to further modify and improve the interface bonding of the composite material. The increase in the roughness of the fiber surface is conducive to the interface bonding between the fiber and the epoxy resin, and reduces the probability of the carbon fiber being peeled off and falling off from the resin matrix.
[0026] Ammonium polyphosphate is a universal low-cost halogen-free flame retardant, but it is hygroscopic and has poor compatibility with organic polymers. Adding it to a composite material will lead to a decrease in mechanical properties. In the present invention, by using modified carbon fiber as a raw material, it is less affected by the flame retardant and can maintain good stability in the test; in addition, the flame retardant elements such as nitrogen and silicon (derived from polydopamine and octaaminopropylsilsesquioxane) introduced into the treated carbon fiber have a synergistic flame retardant effect with the added halogen-free flame retardant, which can effectively improve the thermal stability (residual carbon rate) of the material and the strength of the expanded carbon layer, thereby making the carbon layer have better heat insulation and oxygen isolation properties, thereby improving the flame retardant properties, and can be well applied to the field of building materials. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] A method for preparing a carbon fiber composite material comprises the following steps:
[0030] Prepare Tris buffer according to the following ratio: add 1.21 g of tris(hydroxymethylaminomethane) to 1000 mL of water and adjust the pH to 8.5 with hydrochloric acid;
[0031] The T700 carbon fiber was added to a Tris buffer with a pH value of 8.5, dopamine was added, and the content of dopamine in the buffer was 5 mg / mL. The mixture was stirred for 12 hours at room temperature. After the stirring was completed, the mixture was centrifuged, washed, and filtered to obtain a polydopamine pre-modified carbon fiber.
[0032] The polydopamine pre-modified carbon fiber is added to a Tris buffer and octaaminopropyl silsesquioxane is added, and the mixture is stirred for 12 hours. After the stirring is completed, the carbon fiber is washed with water and dried to obtain POSS-modified carbon fiber; the amount of octaaminopropyl silsesquioxane added to the Tris buffer is 5 mg / L.
[0033] The POSS-modified carbon fiber is added to the epoxy resin glue for soaking to obtain a prepreg, and multiple layers of prepreg are laid and hot-pressed: the pressure of hot-pressing is 0.5MPa, and the temperature of hot-pressing is 200℃ to obtain a carbon fiber composite material; the mass ratio of resin to fiber is 2:3; the resin glue includes epoxy resin and curing agent, and the mass ratio of epoxy resin to curing agent in the epoxy resin glue is 10:1. Epoxy resin: E51, epoxy value is 0.52mol / 100g, density is 1.2g / cm 3 , curing agent diethyltoluenediamine.
[0034] Example 2
[0035] A method for preparing a carbon fiber composite material comprises the following steps:
[0036] Prepare Tris buffer according to the following ratio: add 1.21 g of tris(hydroxymethylaminomethane) to 1000 mL of water and adjust the pH to 8.5 with hydrochloric acid;
[0037] Soak the T700 carbon fiber in acetone for 24 hours, wash the surface impurities, dry at 120°C, and then soak in a concentrated nitric acid solution with a mass fraction of 68% for 110 minutes. Take it out and wash it with water and dry it to obtain oxidized carbon fiber. Add the oxidized carbon fiber to a Tris buffer with a pH value of 8.5, add dopamine, the content of dopamine in the buffer is 5 mg / mL, stir at room temperature for 12 hours, and after stirring, centrifuge, wash, and filter to obtain polydopamine pre-modified carbon fiber;
[0038] The polydopamine pre-modified carbon fiber is added to a Tris buffer and octaaminopropyl silsesquioxane is added, and the mixture is stirred for 12 hours. After the stirring is completed, the carbon fiber is washed with water and dried to obtain POSS-modified carbon fiber; the amount of octaaminopropyl silsesquioxane added to the Tris buffer is 5 mg / L.
[0039] The POSS-modified carbon fiber is added to the epoxy resin glue for soaking to obtain a prepreg, and multiple layers of prepreg are laid and hot-pressed: the pressure of hot-pressing is 0.6MPa, and the temperature of hot-pressing is 180℃ to obtain a carbon fiber composite material; the mass ratio of resin to fiber is 2:3; the resin glue includes epoxy resin and curing agent, and the mass ratio of epoxy resin to curing agent in the epoxy resin glue is 10:1. Epoxy resin: E51, epoxy value is 0.52mol / 100g, density is 1.2g / cm 3 , curing agent diethyltoluenediamine.
[0040] Example 3
[0041] A method for preparing a carbon fiber composite material comprises the following steps:
[0042] Compared with Example 2, the dopamine content in this example is 3 mg / mL, and the other steps are the same.
[0043] The polydopamine pre-modified carbon fiber is added to a Tris buffer and octaaminopropyl silsesquioxane is added, and the mixture is stirred for 12 hours. After the stirring is completed, the carbon fiber is washed with water and dried to obtain POSS-modified carbon fiber; the amount of octaaminopropyl silsesquioxane added to the Tris buffer is 5 mg / L.
[0044] POSS modified carbon fiber is soaked in epoxy resin glue to obtain prepreg, and multiple layers of prepreg are laid and hot pressed: the pressure of hot pressing is 0.6MPa, and the temperature of hot pressing is 180℃ to obtain carbon fiber composite material; the mass ratio of resin to fiber is 2:3; the resin glue includes epoxy resin and curing agent, and the mass ratio of epoxy resin to curing agent in the epoxy resin glue is 10:1. Epoxy resin: E51, epoxy value is 0.52mol / 100g, density is 1.2g / cm 3 , curing agent diethyltoluenediamine.
[0045] Example 4
[0046] Compared with Example 2, the addition amount of octaaminopropyl silsesquioxane in this example is 4 mg / L, and the other steps are the same.
[0047] Example 5
[0048] Compared with Example 2, the addition amount of octaaminopropyl silsesquioxane in this example is 2 mg / L, and the other steps are the same.
[0049] Comparative Example 1
[0050] Compared with Example 2, this embodiment uses untreated T700 carbon fiber, and the carbon fiber is immersed in epoxy resin glue to obtain a prepreg. Multiple layers of prepreg are laid and hot pressed: the pressure of hot pressing is 0.6 MPa, and the temperature of hot pressing is 180°C to obtain a carbon fiber composite material; the mass ratio of resin to fiber is 2:3; the resin glue includes epoxy resin and curing agent, and the mass ratio of epoxy resin to curing agent in the epoxy resin glue is 10:1, and the remaining steps are the same.
[0051] The samples prepared in Examples 1 to 5 and Comparative Example 1 were tested;
[0052] Bending performance test: according to the three-point bending test in ASTMD7264 standard; Thermal stability test: the test temperature range is 30-900℃, nitrogen is selected as the protective atmosphere, and the given temperature increase rate is 8℃ / min to record the carbon residue rate. The test results are shown in Table 1 below:
[0053] Table 1
[0054]
[0055]
[0056] It can be seen from Table 1 that the interface bonding strength between the fiber and the resin matrix in the treated composite material is large, and the sample does not suffer destructive damage, the difficulty of crack transmission increases, and the composite material prepared by the present invention has good bending performance. From the test results of thermal stability, it can be seen that the composite material prepared by the present invention has a high carbon residue rate and good thermal stability.
[0057] Example 6
[0058] Compared with Example 2, in this example, a halogen-free flame retardant is added to the resin liquid, and the amount of the halogen-free flame retardant added is 10% of the mass of the resin liquid. The halogen-free flame retardant is modified ammonium polyphosphate, which is prepared by the following steps:
[0059] 3 mL of alkyl silane coupling agent was added to 100 mL of 80% ethanol aqueous solution, the pH value was adjusted to 5 with acetic acid, and the hydrolyzate was obtained after stirring for 2 hours; the alkyl silane coupling agent was n-hexyltrimethoxysilane
[0060] Add 50g of ammonium polyphosphate to 100mL of ethanol, then add 3mL of γ-aminopropyltriethoxysilane and stir the reaction at 70°C for 2h, add the hydrolyzate, keep the temperature unchanged after adding, continue stirring for 1h, and after stirring, centrifuge, wash and dry to obtain modified ammonium polyphosphate.
[0061] Example 7
[0062] Compared with Example 2, in this example, a halogen-free flame retardant is added to the resin liquid, and the amount of the halogen-free flame retardant added is 10% of the mass of the resin liquid. The halogen-free flame retardant is modified ammonium polyphosphate, which is prepared by the following steps:
[0063] 4 mL of an alkyl silane coupling agent was added to 100 mL of an ethanol aqueous solution having a mass fraction of 80%, and the pH value was adjusted to 5 with acetic acid. The mixture was stirred for 2 hours to obtain a hydrolyzate; the alkyl silane coupling agent was octyltrimethoxysilane;
[0064] Add 50g of ammonium polyphosphate to 100mL of ethanol, then add 3mL of γ-aminopropyltriethoxysilane and stir the reaction at 70°C for 2h, add the hydrolyzate, keep the temperature unchanged after adding, continue stirring for 1h, and after stirring, centrifuge, wash and dry to obtain modified ammonium polyphosphate.
[0065] Example 8
[0066] Compared with Example 2, in this example, a halogen-free flame retardant is added to the resin liquid, and the amount of the halogen-free flame retardant added is 10% of the mass of the resin liquid. The halogen-free flame retardant is ammonium polyphosphate.
[0067] Comparative Example 2
[0068] Compared with Example 8, this comparative example uses untreated T700 carbon fiber, and the carbon fiber is immersed in epoxy resin glue to obtain a prepreg. Multiple layers of prepreg are laid and hot pressed: the pressure of hot pressing is 0.6 MPa, and the temperature of hot pressing is 180°C to obtain a carbon fiber composite material; the resin glue includes epoxy resin and curing agent, and the mass ratio of resin to fiber is 2:3; the mass ratio of epoxy resin to curing agent in the epoxy resin glue is 10:1.
[0069] The samples prepared in Examples 6 to 8 and Comparative Example 2 were subjected to performance tests;
[0070] The test standard for the limiting oxygen index (LOI) performance test is ASTM D2863-2012, the standard size of the test specimen is 130 mm × 6.5 mm × 3.2 mm, and the ignition method is central top ignition.
[0071] The test standard of the vertical burning test (UL-94) performance test is ASTMD3801-2010, with 5 vertical burning test specimens in each group, and the standard size is 130mm×12.7mm×3.2mm. During the test, each specimen is subjected to a flame of 10 seconds twice; the results are shown in Table 2:
[0072] Table 2
[0073] project Limiting oxygen index Flame retardant grade Bending strength / MPa Example 6 32.1 V-0 1002.6 Example 7 32.5 V-0 1002.4 Example 8 32.1 V-0 987.6 Comparative Example 2 27.6 V-1 465.8
[0074] It can be seen from Table 2 that the composite material prepared by the present invention has good flame retardant properties, and the UL-94 grade can maintain V-0 level at a lower flame retardant. Moreover, the mechanical properties of the composite material after adding the flame retardant can be maintained at a high level, and the mechanical properties and stability of the composite material are high.
[0075] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0076] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a carbon fiber composite material, characterized in that: The steps include: Adding octaaminopropyl silsesquioxane to a Tris buffer having a pH value of 8.5, and stirring, washing with water, and drying to obtain POSS-modified carbon fiber, wherein the amount of octaaminopropyl silsesquioxane added to the Tris buffer is 2-5 mg / L; The POSS-modified carbon fiber is added into epoxy resin glue for immersion to obtain prepreg, and multiple layers of prepreg are laid and hot-pressed to obtain a carbon fiber composite material.
2. The method for preparing a carbon fiber composite material according to claim 1, characterized in that: The resin glue includes epoxy resin and curing agent, wherein the mass ratio of epoxy resin to curing agent in the epoxy resin glue is 10:1; the epoxy resin is E51, the epoxy value is 0.52 mol / 100 g, and the density is 1.2 g / cm 3 , curing agent diethyltoluenediamine.
3. The method for preparing a carbon fiber composite material according to claim 2, characterized in that: The resin glue liquid also includes a halogen-free flame retardant, and the added amount of the halogen-free flame retardant is 10% of the mass of the resin liquid.
4. The method for preparing a carbon fiber composite material according to claim 1, characterized in that: The pressure of hot pressing is 0.5-0.6MPa, and the temperature of hot pressing is 180-200℃.
5. The method for preparing a carbon fiber composite material according to claim 3, characterized in that: The halogen-free flame retardant is modified ammonium polyphosphate, which is prepared by the following steps: Adding an alkyl silane coupling agent into an ethanol aqueous solution, adjusting the system to be weakly acidic, and stirring to obtain a hydrolyzate; Add ammonium polyphosphate to ethanol, then add γ-aminopropyltriethoxysilane, heat and stir to react, add the above hydrolyzate, keep the temperature unchanged after adding, continue stirring, after stirring, centrifuge, wash and dry to obtain modified ammonium polyphosphate.
6. The method for preparing a carbon fiber composite material according to claim 5, characterized in that: The alkylsilane coupling agent is one of n-hexyltrimethoxysilane, octyltrimethoxysilane, tetradecyltrimethoxysilane and hexadecyltrimethoxysilane.
7. The method for preparing a carbon fiber composite material according to claim 1, characterized in that: Polydopamine pre-modified carbon fibers were prepared by the following steps: The oxidized carbon fiber is added to a Tris buffer with a pH value of 8.5, dopamine is added, and the mixture is stirred at room temperature. After the stirring is completed, the mixture is centrifuged, washed, and filtered to obtain polydopamine pre-modified carbon fiber; the content of dopamine in the buffer is 2-5 mg / mL.
8. The method for preparing a carbon fiber composite material according to claim 7, characterized in that: The oxidized carbon fiber is a carbon fiber that has been oxidized by soaking in concentrated nitric acid and is prepared by the following steps: The carbon fiber is soaked in acetone to wash the surface impurities, and then dried and soaked in a concentrated nitric acid solution for 100-120 minutes. After being taken out, it is washed with water and dried to obtain an oxidized carbon fiber.
9. A carbon fiber composite material, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 8.
10. The carbon fiber composite material according to claim 9, characterized in that: Application in building materials.