A 355MPa grade hydrogen sulfide corrosion resistant steel plate and its production method
By adding a chromium carbide and titanium trisilide composition to the LF refining process, and combining it with specific process parameters and composition control, the corrosion resistance problem of 355MPa grade steel plates in hydrogen sulfide corrosive environments was solved, and the high strength and corrosion resistance of the steel plates were improved.
Patent Information
- Application Number
- CN202311538796.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-11-17
AI Technical Summary
Existing 355MPa grade steel plates have poor corrosion resistance in hydrogen sulfide corrosive environments, making containers prone to cracking. Existing solutions are costly and ineffective.
A chromium carbide and titanium trisilide composition is added during the LF refining process. Combined with specific heating, rolling and heat treatment processes, the composition and process parameters of the steel plate are controlled, including the addition of medium manganese and small amounts of chromium and niobium, to form a composite of high-hardness wear-resistant ceramic particles and steel plate, which enhances the mechanical properties and resistance to hydrogen sulfide corrosion of the steel plate.
It significantly improves the strength and resistance to hydrogen sulfide corrosion of steel plates, reduces production costs, and enhances the mechanical properties and corrosion resistance of steel plates.
Smart Images

Figure CN118064785B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of alloys, and in particular to a 355MPa grade hydrogen sulfide corrosion resistant steel plate and a production method thereof. Background Art
[0002] In petrochemical production, due to the long-term high-temperature use of pressure vessels and the generation of water deposited at the bottom of oil storage tanks, the pressure vessels will be severely corroded by hydrogen sulfide. The cracking of the container caused by hydrogen sulfide corrosion is not only related to the container material, but more importantly, the strength of the container. The material of the pressure vessel is mainly steel. The higher the strength of the steel, the more conducive it is for hydrogen to enter the steel, which in turn causes the steel to crack. High-strength steel is more likely to form sulfide stress cracking in a wet hydrogen sulfide environment. Therefore, in order to ensure the safety of the equipment, normalized steel plates with a yield strength of ≤355MPa are usually used as the main metal material of the container. However, the existing 355MPa grade steel plates still have the defect of hydrogen sulfide corrosion. At present, the means to eliminate hydrogen sulfide corrosion are mainly to use ordinary carbon steel, by adding stress-relieving post-weld heat treatment to the production method or lining the inner wall of the steel with a layer of corrosion-resistant metal, such as ferritic stainless steel, nickel alloy, etc.
[0003] In patent CN106086641B, a high-strength steel for extra-large oil storage tanks resistant to hydrogen sulfide corrosion and its manufacturing method, a carbon-manganese system with Cu and Nb micro-alloying components and a thermomechanical control and tempering process are used. However, the process has a high production cost and the steel has poor hydrogen sulfide corrosion resistance. Therefore, in order to solve the problem that steel containers are prone to cracking due to hydrogen sulfide, it is crucial for the petrochemical industry to develop a production method for hydrogen sulfide corrosion-resistant steel plates. Summary of the invention
[0004] The present invention provides a 355MPa grade hydrogen sulfide corrosion resistant steel plate and a production method thereof, which solves the problem that the 355MPa grade steel plate in the related art has poor hydrogen sulfide corrosion resistance.
[0005] The technical solution of the present invention is as follows:
[0006] The present invention provides a method for producing a 355MPa grade hydrogen sulfide corrosion resistant steel plate, comprising the following steps:
[0007] S1, molten iron pretreatment: pretreating the molten iron to obtain pretreated molten iron;
[0008] S2, converter smelting: adding scrap steel to the pretreated molten iron, smelting, tapping to obtain molten steel;
[0009] S3, LF refining: refining the molten steel, adding ferrotitanium after refining, feeding calcium wire, adding aluminum powder for deoxidation, and obtaining refined molten steel A;
[0010] S4, VD refining: vacuum refining the refined molten steel A to obtain refined molten steel B;
[0011] S5, continuous casting: the refined molten steel B is cast with full protection, cooled, and a continuous casting billet is obtained;
[0012] S6, heating: heating the continuous casting billet to obtain a heated slab;
[0013] S7, rolling: rolling the heated slab to obtain a rolled steel plate;
[0014] S8, cooling: cooling the rolled slab to obtain a cooled steel plate;
[0015] S9, slow cooling: stacking the cooled steel plates and slowly cooling them to obtain slowly cooled steel plates;
[0016] S10, heat treatment: heat treating the slowly cooled steel plate to obtain a hydrogen sulfide corrosion resistant steel plate;
[0017] In step S3, during the refining, a composition of chromium carbide and pentatitanium silicide is also added.
[0018] As a further technical solution, based on the added mass of the scrap steel, the added mass of the chromium carbide and titanium pentasilicon trisilicide composition is 0.1-0.3 kg / t, and the mass ratio of chromium carbide to titanium pentasilicon trisilicide is 5:5-7:3.
[0019] As a further technical solution, the molten iron pretreatment adopts KR desulfurization method for desulfurization, the thickness of the slag layer after desulfurization is ≤10mm, and the mass content is controlled to be S≤0.005%, P≤0.090%.
[0020] As a further technical solution, in step S2, the smelting also includes slag making treatment, and the slag making basicity is 3.0; the steel tapping temperature is 1590~1630℃, and the component target is mass content C 0.05%~0.08%, P≤0.008%, S≤0.005%.
[0021] As a further technical solution, in step S2, the refining also includes slag making treatment, and the slag making basicity is 6.0; the mass content of CaO in the refined slag is ≥55%, and Al2O3 is ≥8%; the LF refining inlet temperature is ≥1580°C, and the outlet temperature is 1615~1630°C; the vacuum degree of the VD vacuum refining is ≤60Pa, the vacuum refining time is 15~20min, and the outlet temperature is 1560~1570°C;
[0022] As a further technical solution, after the LF is refined, the calcium wire is fed ≥ 2m / t.
[0023] As a further technical solution, the cooling in step S5 includes secondary cooling, wherein the secondary cooling adopts weak cooling and electromagnetic stirring is performed in the secondary cooling; during the continuous casting, the superheat degree of the molten steel is 8-13°C.
[0024] As a further technical solution, the heating in step S6 includes heating treatment and soaking treatment, the heating treatment temperature is 1280±20°C, the heating treatment speed is 8~12min / cm, the soaking treatment temperature is 1260±20°C, and the soaking treatment time is ≥45min.
[0025] As a further technical solution, the rolling is divided into a first stage rolling and a second stage rolling, the first stage starting rolling temperature is ≥1150°C, and the final rolling temperature is 950~1000°C.
[0026] As a further technical solution, the reduction of the first stage rolling pass is ≥45mm, and the intermediate billet thickness is controlled 3.5h after the slab is widened; the starting rolling temperature of the second stage is 880~900℃, and the final rolling temperature is 760~880℃.
[0027] As a further technical solution, the reduction rate of each pass in the second stage of rolling is ≥16%, and the cumulative reduction rate is ≥60%.
[0028] As a further technical solution, during cooling in step S8, the red-returning temperature is 700±10°C; in step S9, the stacking slow cooling temperature is ≥250°C, and the stacking slow cooling time is ≥24h; in step S10, the heat treatment includes annealing, quenching, and tempering, and the tempering temperature is 630±10°C.
[0029] The present invention also proposes a 355MPa grade hydrogen sulfide corrosion resistant steel plate produced by the production method, which comprises the following components in weight percentage: C 0.10%~0.14%, Si 0.20%~0.35%, Mn 1.20%~1.40%, Cr 0.20%~0.30%, Mo≤0.010%, Ni≤0.020%, Cu≤0.030%, Alt 0.020%~0.035%, Ti 0.010%~0.020%, Nb0.020%~0.045%, S≤0.002%, P≤0.010%, Ca≥0.0010%, and the balance is Fe.
[0030] The working principle and beneficial effects of the present invention are:
[0031] 1. In the present invention, a composition of chromium carbide and titanium pentasilicon is added during LF refining, and chromium carbide and titanium pentasilicon are high-hardness wear-resistant ceramic particles, which are compounded with the metal material in the steel plate to enhance the mechanical properties and hydrogen sulfide corrosion resistance of the steel plate.
[0032] 2. In the present invention, the mechanical properties of the steel plate are further improved by controlling the heating and rolling process conditions of the continuous casting billet.
[0033] 3. In the present invention, the addition of medium manganese and a small amount of chromium and niobium elements further improves the strength, hardness and corrosion resistance of the steel. The addition of niobium elements also reduces the quenching temperature of heat treatment, and there is no need to add a large amount of precious Mo elements to the steel. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0035] Figure 1 This is the metallographic structure diagram of the hydrogen sulfide corrosion resistant steel plate 100X of Example 1;
[0036] Figure 2 This is the metallographic structure diagram of the hydrogen sulfide corrosion resistant steel plate 500X of Example 1;
[0037] Figure 3 This is the metallographic structure diagram of austenite 500X of hydrogen sulfide corrosion resistant steel plate in Example 1. DETAILED DESCRIPTION
[0038] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] In the following examples, by mass content, the iron content of the scrap steel is ≥65%, the titanium content of the ferrotitanium is ≥35%, and the aluminum content of the aluminum powder is ≥99%;
[0040] Example 1
[0041] A method for producing a 355MPa grade hydrogen sulfide corrosion resistant steel plate comprises the following steps:
[0042] S1. KR hot metal pretreatment: The hot metal is desulfurized by KR desulfurization method to obtain pretreated hot metal. The thickness of the slag layer after desulfurization is 8 mm, and S is controlled to be 0.003% and P to be 0.060%;
[0043] S2. Converter smelting: put 150t of pretreated molten iron into the converter, add 15t of scrap steel, the tapping temperature is 1593℃, and smelting molten steel is obtained, the slag basicity is 3.0, and the composition targets are: C: 0.06%, P: 0.006%, S: 0.003%;
[0044] S3, LF refining: add molten steel into the refining furnace, the basicity is 6.0, enter the station at 1587℃, add 0.75kg chromium carbide and 0.75kg titanium trisilicide, add 30kg ferrotitanium, feed 3m / t calcium wire, add 125kg aluminum powder for deoxidation, exit the station at 1618℃ to obtain refined molten steel A, the refining slag contains CaO: 58%, Al2O3: 10%, and obtains refined molten steel A;
[0045] S4, VD refining: add the refined molten steel into a vacuum refining furnace at 57Pa, keep it for 15min, and get refined molten steel B at 1563℃;
[0046] S5, continuous casting: the refined molten steel B is cast with full protection, the superheat of the molten steel during continuous casting is controlled to be 10°C, and secondary cooling is performed, the secondary cooling adopts weak cooling, and electromagnetic stirring is performed during the secondary cooling to obtain a continuously cast billet;
[0047] S6, heating: heating the continuous casting billet at 1265° C., the heating speed is 8 min / cm, and performing soaking treatment at 1246° C. for 48 min to obtain a heated slab;
[0048] S7, rolling: the heated slab is subjected to the first stage of opening rolling at 1156°C, the first stage of final rolling at 964°C, the pass reduction is 48mm, the intermediate slab thickness is controlled 3.5h after the slab is widened, the second stage of opening rolling is carried out at 887°C, the second stage of final rolling is carried out at 773°C, the reduction rate of each pass is 18%, and the rolled steel plate is obtained;
[0049] S8, cooling: after rolling, weak ACC cooling is performed, and the red-return temperature is 698°C to obtain a cooled steel plate;
[0050] S9, slow cooling: slowly cooling the stack at 261° C. for 31 hours to obtain a slowly cooled steel plate;
[0051] S10, heat treatment: the slowly cooled steel plate is subjected to tempering heat treatment at 629°C to obtain a hydrogen sulfide corrosion resistant steel plate, wherein the metallographic structure diagrams of the hydrogen sulfide corrosion resistant steel plate are as follows: Figure 1-3 shown.
[0052] Example 2
[0053] A method for producing a 355MPa grade hydrogen sulfide corrosion resistant steel plate comprises the following steps:
[0054] S1. KR hot metal pretreatment: The hot metal is desulfurized by KR desulfurization method to obtain pretreated hot metal. The thickness of the slag layer after desulfurization is 10 mm, and S is controlled to be 0.005% and P to be 0.040%;
[0055] S2. Converter smelting: put 120t of pre-treated molten iron into the converter, add 12t of scrap steel, the tapping temperature is 1593℃, and smelting molten steel is obtained, the slag basicity is 3.0, and the composition targets are: C: 0.05%, P: 0.007%, S: 0.005%;
[0056] S3, LF refining: add molten steel into the refining furnace, the basicity is 6.0, enter the station at 1597℃, add 1.4kg chromium carbide and 1.0kg titanium trisilicide, add 25kg ferrotitanium, feed 5m / t calcium wire, add 100kg aluminum powder for deoxidation, exit the station at 1621℃, and obtain refined molten steel A, with CaO: 63% and Al2O3: 13% in the refining slag, and obtain refined molten steel A;
[0057] S4, VD refining: add the refined molten steel into a vacuum refining furnace at 55Pa, keep it for 15min, and leave the furnace at 1568℃ to obtain refined molten steel B;
[0058] S5, continuous casting: the refined molten steel B is cast with full protection, the superheat of the molten steel during continuous casting is controlled to be 15°C, and secondary cooling is performed, the secondary cooling adopts weak cooling, and electromagnetic stirring is performed during the secondary cooling to obtain a continuously cast billet;
[0059] S6, heating: heating the continuous casting billet at 1276° C. at a heating rate of 10 min / cm, and performing soaking treatment at 1254° C. for 53 min to obtain a heated slab;
[0060] S7, rolling: the heated slab is subjected to the first stage of opening rolling at 1213°C, and the final rolling is carried out at 987°C, with a pass reduction of 51 mm, and the intermediate slab thickness is controlled 3.5 hours after the slab is widened, and the second stage of opening rolling is carried out at 894°C, and the final rolling is carried out at 781°C, with a pass reduction of 20%, to obtain the rolled steel plate;
[0061] S8, cooling: after rolling, weak ACC cooling is performed, and the red-return temperature is 703°C to obtain a cooled steel plate;
[0062] S9, slow cooling: slowly cooling the stack at 274° C. for 28 hours to obtain a slowly cooled steel plate;
[0063] S10, heat treatment: the slowly cooled steel plate is subjected to tempering heat treatment at 633°C to obtain a hydrogen sulfide corrosion resistant steel plate.
[0064] Example 3
[0065] A method for producing a 355MPa grade hydrogen sulfide corrosion resistant steel plate comprises the following steps:
[0066] S1. KR hot metal pretreatment: The hot metal is desulfurized by KR desulfurization method to obtain pretreated hot metal. The thickness of the slag layer after desulfurization is 10 mm, and S is controlled to be 0.003% and P to be 0.060%.
[0067] S2. Converter smelting: 100t of pretreated molten iron is put into the converter, 10t of scrap steel is added, the tapping temperature is 1628℃, and smelting molten steel is obtained, the slag basicity is 3.0, the composition target is: C: 0.08%, P: 0.008%, S: 0.005%, and refined molten steel A is obtained;
[0068] S3, LF refining: add molten steel into the refining furnace, the basicity is 6.0, enter the station at 1711℃, add 2.1kg chromium carbide and 0.9kg titanium trisilicide, add 20kg ferrotitanium, feed 7m / t calcium wire, add 85kg aluminum powder for deoxidation, exit the station at 1638℃, obtain refined molten steel A, the refining slag contains CaO: 67%, Al2O3: 16%, and obtain refined molten steel B;
[0069] S4, VD refining: add the refined molten steel into a vacuum refining furnace at 53Pa, keep it for 15min, and leave the furnace at 1570℃ to obtain refined molten steel B;
[0070] S5. Continuous casting: Continuous casting: The refined molten steel B is cast with full protection, the superheat of the molten steel in the casting is controlled to be 18°C, and the secondary cooling is weak cooling, and electromagnetic stirring is performed during the secondary cooling to obtain a continuously cast billet;
[0071] S6, heating: heating the continuous casting billet at 1293° C. at a heating rate of 12 min / cm, and performing soaking treatment at 1271° C. for 55 min to obtain a heated slab;
[0072] S7, rolling: the heated slab is subjected to the first stage of opening rolling at 1219°C, and the final rolling is carried out at 996°C, with a pass reduction of 53mm, and the intermediate slab thickness is controlled 3.5h after the slab is widened, and the second stage of opening rolling is carried out at 898°C, and the final rolling is carried out at 876°C, with a pass reduction of 26%, to obtain the rolled steel plate;
[0073] S8, cooling: after rolling, weak ACC cooling is performed, and the red-return temperature is 708°C to obtain a cooled steel plate;
[0074] S9, slow cooling: slowly cooling the stack at 281° C. for 30 hours to obtain a slowly cooled steel plate;
[0075] S10, heat treatment: the slowly cooled steel plate is subjected to tempering heat treatment at 639° C. to obtain a hydrogen sulfide corrosion resistant steel plate.
[0076] Example 4
[0077] The difference between this embodiment and embodiment 1 is only that the weight percentage of manganese is 0.98%.
[0078] Example 5
[0079] The only difference between this embodiment and embodiment 1 is that the weight percentage of chromium is 0.35%.
[0080] Example 6
[0081] The only difference between this embodiment and embodiment 1 is that the weight percentage of niobium is 0.048%.
[0082] The difference between Examples 7 to 11 and Example 1 is only that the heating and rolling processes are different, as shown in the following table:
[0083]
[0084] Comparative Example 1
[0085] The difference between this comparative example and Example 1 is that pentatitanium trisilicide is replaced by chromium carbide in step S3.
[0086] Comparative Example 2
[0087] The difference between this comparative example and Example 1 is that chromium carbide is replaced by pentatitanium trisilicide in step S3.
[0088] Comparative Example 3
[0089] The difference between this comparative example and Example 1 is that the mass ratio of chromium carbide to pentatitanium silicide in step S3 is 4:6.
[0090] Comparative Example 4
[0091] The difference between this comparative example and Example 1 is that the mass ratio of chromium carbide to pentatitanium silicide in step S3 is 8:2.
[0092] The raw materials used in the embodiments and comparative examples are shown in the following table:
[0093]
[0094] The weight percentages (%) of the components of the 355MPa grade hydrogen sulfide corrosion resistant steel plates prepared in Examples 1 to 11 and Comparative Examples 1 to 4 are shown in the following table:
[0095]
[0096] The 355MPa grade hydrogen sulfide corrosion resistant steel plates prepared in Examples 1 to 11 and Comparative Examples 1 to 4 were tested for performance using Solution A in accordance with GB / T 4157-2017, with a loading stress of 188MPa and a test time of 720h, as shown in the following table:
[0097]
[0098] The 355MPa grade hydrogen sulfide corrosion resistant steel plates prepared in Examples 1 to 11 and Comparative Examples 1 to 4 were subjected to mechanical property tests according to GB / T 3531-2014, as shown in the following table:
[0099]
[0100] According to the data of Example 1 and Comparative Examples 1 to 4, it can be seen that the present invention significantly improves the strength and hydrogen sulfide corrosion resistance of the steel plate by adding a composition of chromium carbide and pentatitanium silicide during LF refining.
[0101] According to the data of Example 1 and Examples 7 to 11, it can be seen that the present invention further improves the mechanical properties of the steel plate by controlling the heating and rolling process conditions of the continuous casting billet.
[0102] According to the data of Examples 1 and 4 to 6, the present invention further improves the strength and hydrogen sulfide corrosion resistance of the 355MPa grade hydrogen sulfide corrosion resistant steel plate by adding medium manganese and a small amount of chromium and niobium elements.
[0103] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for producing a 355MPa grade hydrogen sulfide corrosion resistant steel plate, It is characterized in that The following steps are involved: S1, molten iron pretreatment: pretreating the molten iron to obtain pretreated molten iron; S2, converter smelting: adding scrap steel to the pretreated molten iron, smelting, tapping to obtain smelted steel; S3, LF refining: refining the molten steel, adding ferrotitanium after refining, feeding calcium wire, adding aluminum powder for deoxidation, and obtaining refined molten steel A; S4, VD refining: vacuum refining the refined molten steel A to obtain refined molten steel B; S5, continuous casting: the refined molten steel B is cast with full protection, cooled, and a continuous casting billet is obtained; S6, heating: heating the continuous casting billet to obtain a heated slab; S7, rolling: rolling the heated slab to obtain a rolled steel plate; S8, cooling: cooling the rolled slab to obtain a cooled steel plate; S9, slow cooling: stacking the cooled steel plates and slowly cooling them to obtain slowly cooled steel plates; S10, heat treatment: heat treating the slowly cooled steel plate to obtain a hydrogen sulfide corrosion resistant steel plate; In step S3, during the refining, a composition of chromium carbide and pentatitanium silicide is also added; The particle size of chromium carbide is 100 mesh, and the particle size of titanium trisilicide is 200 mesh; The mass ratio of chromium carbide to titanium pentasilicon is 5:5~7:3; The added mass of the chromium carbide and titanium pentasilicon trisilicide composition is 0.1-0.3 kg / t based on the added mass of the scrap steel; The heating in step S6 includes heating treatment and soaking treatment, the heating treatment temperature is 1280±20°C, the heating treatment speed is 8-12min / cm, the soaking treatment temperature is 1260±20°C, and the soaking treatment time is ≥45min; The rolling is divided into a first stage rolling and a second stage rolling, wherein the first stage rolling has a starting rolling temperature of ≥1150°C and a final rolling temperature of 950-1000°C; the second stage rolling has a starting rolling temperature of 880-900°C and a final rolling temperature of 760-880°C; The hydrogen sulfide corrosion resistant steel plate is composed of the following components in weight percentage: C 0.10%~0.14%, Si 0.20%~0.35%, Mn 1.20%~1.40%, Cr 0.20%~0.30%, Mo≤0.010%, Ni≤0.020%, Cu≤0.030%, Alt0.020%~0.035%, Ti 0.010%~0.020%, Nb 0.020%~0.045%, S≤0.002%, P≤0.010%, Ca≥0.0010%, and the balance is Fe.
2. The method for producing a 355MPa grade hydrogen sulfide corrosion resistant steel plate according to claim 1, It is characterized in that The molten iron pretreatment adopts KR desulfurization method for desulfurization, the thickness of the slag layer after desulfurization is ≤10mm, and the mass content S is controlled to be ≤0.005%, and P is ≤0.090%.
3. The method for producing a 355MPa grade hydrogen sulfide corrosion resistant steel plate according to claim 1, It is characterized in that In step S2, the smelting also includes slag making treatment, and the slag making basicity is 3.0; the temperature of the steel tapping is 1590~1630℃, and the target component mass content is C 0.05%~0.08%, P≤0.008%, and S≤0.005%.
4. The method for producing a 355MPa grade hydrogen sulfide corrosion resistant steel plate according to claim 1, It is characterized in that In step S3, the refining process also includes slag making, and the slag basicity is 6.0; the mass content of CaO in the refined slag is ≥55%, and the Al 2 O 3 ≥8%; the inlet temperature of the refining is ≥1580℃, and the outlet temperature is 1615~1630℃; in step S4, the vacuum degree of the vacuum refining is ≤60Pa, the vacuum refining time is 15~20min, and the outlet temperature is 1560~1570℃.
5. The method for producing a 355MPa grade hydrogen sulfide corrosion resistant steel plate according to claim 1, It is characterized in that The cooling in step S5 includes secondary cooling, wherein the secondary cooling adopts a weak cooling method and electromagnetic stirring is performed during the secondary cooling; during the continuous casting, the superheat degree of the molten steel is 8-13°C.
6. The method for producing a 355MPa grade hydrogen sulfide corrosion resistant steel plate according to claim 1, It is characterized in that During cooling in step S8, the red-returning temperature is 700±10°C; in step S9, the stacking slow cooling temperature is ≥250°C, and the stacking slow cooling time is ≥24h; in step S10, the heat treatment includes annealing, quenching, and tempering, and the tempering temperature is 630±10°C.