A kind of PET laser transfer film and preparation method thereof

By using water-based polyurethane acrylate emulsion and microencapsulated anti-shrinkage agent in PET laser transfer film, the pollution and safety hazard problems of organic solvent-based transfer coatings are solved, the mechanical properties and adhesion of the laser transfer film are improved, and high-end Packaging application requirements.

CN118082400BActive Publication Date: 2024-10-15HUNAN TAILI HENGYOU TECH DEV CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410199238.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-22
Publication Date
2024-10-15
Estimated Expiration
2044-02-22

AI Technical Summary

Technical Problem

Existing laser transfer films use organic solvent-based transfer coatings, which endangers the health of operators and pollutes the environment. During the curing process, the shrinkage stress of the resin cannot be released in time, reducing the mechanical properties of the material, resulting in reduced adhesion and deformation of the coating.

Method used

Water-based polyurethane acrylate emulsion and microencapsulated anti-shrinkage agent are used to prepare the PET laser transfer film through a combination of photoinitiator and leveling agent. The microencapsulated anti-shrinkage agent is used to rupture during high-temperature molding and buffer the resin curing shrinkage stress. Improve mechanical properties.

Benefits of technology

It effectively overcomes the pollution and safety hazards of solvent-based transfer coatings, improves the mechanical properties of the coating, meets the molding requirements of high-end packaging, reduces the shrinkage stress of the coating, and improves adhesion and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118082400B_ABST
    Figure CN118082400B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of laser transfer films, in particular to a PET laser transfer film and a preparation method thereof, comprising a PET base film, a laser mold layer and an aluminum-plated layer; the laser mold layer is prepared from the following raw materials in parts by weight: 60-80 parts of aqueous polyurethane acrylate emulsion, 15-25 parts of acrylate monomers, 5-10 parts of microencapsulated anti-shrinkage agents, 1-3 parts of photoinitiators, and 0.1-0.5 parts of leveling agents; the addition of the microencapsulated anti-shrinkage agent plays a positive role in reducing the shrinkage stress of the coating and improving the mechanical properties thereof; and the prepared PET laser transfer film can be widely used in various high-end packages.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of laser transfer films, in particular to a PET laser transfer film and a preparation method thereof. Background Art

[0002] A polymer coating is applied on the surface of the film, and then a bright laser pattern is pressed on the coating according to different needs. After vacuum aluminum plating, a laser transfer film is formed. It is beautiful and easy to identify, and has a good anti-counterfeiting effect. It is widely used in various high-end packaging. Among them, transfer coating is an important component material of laser transfer film.

[0003] Currently, organic solvent-based transfer coatings are mostly used, which not only endanger the health of operators, but also pollute the environment and bring safety hazards to production. During the curing process of the transfer coating, the monomer molecules polymerize into a linear or cross-linked network structure, and the distance between molecules is rapidly shortened, causing polymerization shrinkage in the resin system. The shrinkage stress cannot be released in time, which will reduce the mechanical properties of the material, resulting in reduced adhesion of the coating, and even deformation and cracking. Summary of the invention

[0004] Purpose of the invention: In view of the above technical problems, the present invention proposes a PET laser transfer film and a preparation method thereof.

[0005] The technical solutions adopted are as follows:

[0006] A PET laser transfer film, comprising a PET base film, a laser molding layer and an aluminum plating layer;

[0007] The laser molding layer is made of the following raw materials in parts by weight:

[0008] 60-80 parts of waterborne polyurethane acrylate emulsion, 15-25 parts of acrylate monomer, 5-10 parts of microencapsulated anti-shrinkage agent, 1-3 parts of photoinitiator, and 0.1-0.5 parts of leveling agent.

[0009] Furthermore, the preparation method of the aqueous polyurethane acrylate emulsion is as follows:

[0010] Under nitrogen protection, diol, diisocyanate, dimethylol propionic acid and organic tin catalyst are mixed and reacted for 1-3 hours, and then pentaerythritol triallyl ether and acetone are added, and the reaction is continued for 10-60 minutes to obtain a prepolymer. The prepolymer is dropped into water and triethylamine is added. After stirring for 10-60 minutes, ethylenediamine is added to extend the chain, and finally the acetone is removed by reduced pressure distillation.

[0011] Furthermore, the diol is polycaprolactone diol.

[0012] Furthermore, the diisocyanate is any one or more combinations of isophorone diisocyanate, dicyclohexylmethane diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, and hexamethylene diisocyanate.

[0013] Furthermore, the acrylate monomer is any one or more combinations of bisphenol A propylene glycol dimethacrylate, glycerol 1,3-diglycerol alcohol diacrylate, pentaerythritol triacrylate, and ethoxylated trimethylolpropane triacrylate.

[0014] Furthermore, the microencapsulated anti-shrinkage agent uses urea as a core material.

[0015] Furthermore, the preparation method of the microencapsulated anti-shrinkage agent is as follows:

[0016] Dissolve chitosan in acetic acid solution, add urea and mix to obtain an aqueous phase, mix paraffin and petroleum ether to obtain an oil phase, disperse the aqueous phase into the oil phase, add an emulsifier and glutaraldehyde, stir to react for 1-5 hours, filter out the precipitate, wash and dry.

[0017] Further, the photoinitiator is a combination of TPO and 184;

[0018] The weight ratio of TPO to 184 is 1-5:1-5.

[0019] Furthermore, the leveling agent is any one or more combinations of BYK-333, BYK-347, BYK-358N, and BYK-378.

[0020] The present invention provides a method for preparing a PET laser transfer film:

[0021] Aqueous polyurethane acrylate emulsion, acrylate monomer, microencapsulated anti-shrinkage agent, photoinitiator and leveling agent are mixed and coated on a PET base film, dried and cured by ultraviolet light to obtain a coating, the mold plate is heated to 150-180°C, the laser information on the mold plate is hot stamped onto the coating under high temperature to obtain a laser molded layer, and finally vacuum aluminum is plated to obtain an aluminum-plated layer.

[0022] Beneficial effects of the present invention:

[0023] The present invention provides a PET laser transfer film. The water-based transfer coating used not only takes into account various performance characteristics that the transfer coating should have, but also overcomes the problems of environmental pollution, health hazards and safety hazards during the production of solvent-based transfer coatings. The wall material of the microencapsulated anti-shrinkage agent is an organic polymer with a certain deformation ability. It deforms under the tensile force of surrounding resin polymerization to compensate for the shrunken volume, and has a certain elasticity, which can effectively buffer the shrinkage stress during curing. During high-temperature molding, the microcapsules are broken, and microbubbles generated by the pyrolysis of the core material can further compensate for the shrinkage volume of the resin curing and reduce the shrinkage stress of the coating, so that it can meet the molding requirements. After testing, the addition of the microencapsulated anti-shrinkage agent plays a positive role in reducing the shrinkage stress of the coating and improving its mechanical properties. The prepared PET laser transfer film can be widely used in various high-end packages. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The structure diagram of the PET laser transfer film of the present invention is shown in the figure, and the reference numerals in the figure represent:

[0025] 1-PET base film, 2-laser molded layer, 3-aluminum coating layer;

[0026] Figure 2 This is the SEM image of the microencapsulated anti-shrinkage agent prepared in Example 1. DETAILED DESCRIPTION

[0027] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.

[0028] Embodiment 1:

[0029] A PET laser transfer film comprises a PET base film 1, a laser molding layer 2 and an aluminum plating layer 3;

[0030] The laser molding layer 2 is made of the following raw materials in parts by weight:

[0031] 75 parts of waterborne polyurethane acrylate emulsion, 20 parts of pentaerythritol triacrylate, 8 parts of microencapsulated anti-shrinkage agent, 1 part of photoinitiator TPO, 1 part of photoinitiator 184, and 0.5 part of leveling agent BYK-333.

[0032] The preparation method of waterborne polyurethane acrylate emulsion is as follows:

[0033] Under nitrogen protection, 10g polycaprolactone diol (molecular weight 1000), 2.33g isophorone diisocyanate, 0.94g dihydroxymethylpropionic acid and 0.05g dibutyltin dilaurate were mixed and reacted at 55°C for 3h, and then 2.56g pentaerythritol triallyl ether and 50ml acetone were added, and the reaction was continued for 40min to obtain a prepolymer. The prepolymer was dripped into 25ml water and 0.25g triethylamine was added. After stirring for 60min, 1.05g ethylenediamine was added to extend the chain, and finally the acetone was removed by reduced pressure distillation.

[0034] The preparation method of microencapsulated anti-shrinkage agent is as follows:

[0035] Dissolve 1g chitosan in 20ml 1% acetic acid solution, add 2g urea and mix to obtain an aqueous phase, mix 30ml paraffin and 10ml petroleum ether to obtain an oil phase, disperse the aqueous phase into the oil phase, add 0.1g emulsifier Span-80 and 0.5g glutaraldehyde, stir at room temperature for 3h, filter out the precipitate, wash with petroleum ether and dry.

[0036] Preparation method of the above PET laser transfer film:

[0037] Aqueous polyurethane acrylate emulsion, pentaerythritol triacrylate, microencapsulated anti-shrinkage agent, photoinitiator TPO, photoinitiator 184 and leveling agent BYK-333 are mixed to obtain a transfer coating, which is applied on a PET base film 1, dried and cured by ultraviolet irradiation for 10 minutes to obtain a coating with a thickness of about 5 μm, the mold plate is heated to 160°C, and the laser information on the mold plate is hot stamped onto the coating at high temperature to obtain a laser molded layer 2, and the vacuum aluminum plating machine heats the aluminum wire to 1400°C under a vacuum condition of 0.05 Pa to vaporize it, and then adheres to the laser molded layer 2 to form an aluminum plating layer 3 with a thickness of about 100 nm.

[0038] Embodiment 2:

[0039] A PET laser transfer film comprises a PET base film 1, a laser molding layer 2 and an aluminum plating layer 3;

[0040] The laser molding layer 2 is made of the following raw materials in parts by weight:

[0041] 80 parts of waterborne polyurethane acrylate emulsion, 25 parts of ethoxylated trimethylolpropane triacrylate, 10 parts of microencapsulated anti-shrinkage agent, 1 part of photoinitiator TPO, 1 part of photoinitiator 184, and 0.5 parts of leveling agent BYK-333.

[0042] The preparation method of the aqueous polyurethane acrylate emulsion and the microencapsulated anti-shrinkage agent is the same as that of Example 1;

[0043] Preparation method of the above PET laser transfer film:

[0044] Aqueous polyurethane acrylate emulsion, ethoxylated trimethylolpropane triacrylate, microencapsulated anti-shrinkage agent, photoinitiator TPO, photoinitiator 184 and leveling agent BYK-333 are mixed to obtain a transfer coating, which is applied on a PET base film 1, dried and cured by ultraviolet irradiation for 10 minutes to obtain a coating with a thickness of about 5 μm, the mold plate is heated to 180°C, and the laser information on the mold plate is hot stamped onto the coating at high temperature to obtain a laser molded layer 2, and the vacuum aluminum plating machine heats the aluminum wire to 1400°C under a vacuum condition of 0.05 Pa to vaporize it, and then adheres to the laser molded layer 2 to form an aluminum plating layer 3 with a thickness of about 100 nm.

[0045] Embodiment 3:

[0046] A PET laser transfer film comprises a PET base film 1, a laser molding layer 2 and an aluminum plating layer 3;

[0047] The laser molding layer 2 is made of the following raw materials in parts by weight:

[0048] 70 parts of waterborne polyurethane acrylate emulsion, 15 parts of pentaerythritol triacrylate, 5 parts of microencapsulated anti-shrinkage agent, 1 part of photoinitiator TPO, 1 part of photoinitiator 184, and 0.25 parts of leveling agent BYK-333.

[0049] The preparation method of the aqueous polyurethane acrylate emulsion and the microencapsulated anti-shrinkage agent is the same as that of Example 1;

[0050] Preparation method of the above PET laser transfer film:

[0051] Aqueous polyurethane acrylate emulsion, pentaerythritol triacrylate, microencapsulated anti-shrinkage agent, photoinitiator TPO, photoinitiator 184 and leveling agent BYK-333 are mixed to obtain a transfer coating, which is applied on a PET base film 1, dried and cured by ultraviolet irradiation for 10 minutes to obtain a coating with a thickness of about 5 μm, the mold plate is heated to 150°C, and the laser information on the mold plate is hot stamped onto the coating under high temperature to obtain a laser molded layer 2, and the vacuum aluminum plating machine heats the aluminum wire to 1400°C under a vacuum condition of 0.05 Pa to vaporize it, and then adheres to the laser molded layer 2 to form an aluminum plating layer 3 with a thickness of about 100 nm.

[0052] Comparative Example 1:

[0053] The method is substantially the same as Example 1, except that no microencapsulated anti-shrinkage agent is added.

[0054] Comparative Example 2:

[0055] The method is basically the same as Example 1, except that urea is directly added without microencapsulation treatment.

[0056] Performance Test:

[0057] The transfer coatings prepared in Examples 1-3 of the present invention and Comparative Examples 1-2 were used as samples for performance testing. The samples were evenly coated on a PET release film at room temperature using a 60 μm wire rod, and then cured for 300 seconds using a 395 nm ultraviolet light to obtain a coating with a thickness of 30±1 μm. During the curing, a real-time infrared-optical rheology instrument was used to measure the shrinkage stress of the coating, and the obtained coating was used to test pencil hardness, adhesion and impact strength.

[0058] The pencil hardness of the coating was measured using a PPH-750 pencil hardness tester from Shanghai Tianchen Modern Environmental Technology Co., Ltd. in accordance with GB / T6739-2006;

[0059] The adhesion of the coating was measured using the HGQ paint film cross-cutting device produced by Shanghai Pushen Chemical Machinery Co., Ltd. in accordance with GB / T9268-1998;

[0060] The impact resistance of the coating was measured using the BGD304 paint film impactor produced by Guangzhou Biaogeda Precision Instrument Co., Ltd. in accordance with GB / T1732-1993.

[0061] The test results are shown in Table 1 below:

[0062] Table 1:

[0063]

[0064] It can be seen from Table 1 above that the addition of microencapsulated anti-shrinkage agent plays a positive role in reducing the shrinkage stress of the coating and improving its mechanical properties.

[0065] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A PET laser transfer film, It is characterized in that Including PET base film, laser molding layer and aluminum plating layer; The laser molding layer is made of the following raw materials in parts by weight: 70-80 parts of waterborne polyurethane acrylate emulsion, 15-25 parts of acrylate monomer, 5-10 parts of microencapsulated anti-shrinkage agent, 2 parts of photoinitiator, 0.25-0.5 parts of leveling agent; The preparation method of the aqueous polyurethane acrylate emulsion is as follows: Under nitrogen protection, diol, diisocyanate, dimethylol propionic acid and organic tin catalyst were mixed and reacted for 3 hours, and then pentaerythritol triallyl ether and acetone were added, and the reaction was continued for 40 minutes to obtain a prepolymer, and the prepolymer was dropped into water and triethylamine was added, and after stirring for 60 minutes, ethylenediamine was added to extend the chain, and finally the acetone was removed by reduced pressure distillation; The diol is polycaprolactone diol; The diisocyanate is any one or more combinations of isophorone diisocyanate, dicyclohexylmethane diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, and hexamethylene diisocyanate; The acrylate monomer is any one or more combinations of bisphenol A propylene glycol dimethacrylate, glycerol 1,3-diglycerol alcohol diacrylate, pentaerythritol triacrylate, and ethoxylated trimethylolpropane triacrylate; The microencapsulated anti-shrinkage agent uses urea as a core material; The preparation method of the microencapsulated anti-shrinkage agent is as follows: Dissolve chitosan in acetic acid solution, add urea and mix to obtain an aqueous phase, mix paraffin and petroleum ether to obtain an oil phase, disperse the aqueous phase into the oil phase, add an emulsifier and glutaraldehyde, stir to react for 3 hours, filter out the precipitate, wash and dry.

2. The PET laser transfer film according to claim 1, It is characterized in that The photoinitiator is a composition of TPO and 184; The weight ratio of TPO to 184 is 1-5:1-5.

3. The PET laser transfer film according to claim 1, It is characterized in that The leveling agent is any one or more combinations of BYK-333, BYK-347, BYK-358N and BYK-378.

4. A method for preparing a PET laser transfer film as claimed in any one of claims 1 to 3, It is characterized in that Aqueous polyurethane acrylate emulsion, acrylate monomer, microencapsulated anti-shrinkage agent, photoinitiator and leveling agent are mixed and coated on a PET base film, dried and cured by ultraviolet light to obtain a coating, the mold plate is heated to 150-180°C, the laser information on the mold plate is hot stamped onto the coating under high temperature to obtain a laser molded layer, and finally vacuum aluminum is plated to obtain an aluminum-plated layer.

Citation Information

Cited By

  • Laser transfer film capable of being repeatedly bonded and preparation method thereof

    CN122481381A