A low temperature sintered ultra-low magnetic permeability NiCuZn material and preparation method thereof
Through low-temperature sintering process and specific component ratio design, ultra-low magnetic permeability NiCuZn ferrite material is prepared, which solves the cost and performance problems caused by high-temperature sintering of traditional materials and achieves the comprehensive performance of low magnetic permeability and high mechanical strength. Excellent.
Patent Information
- Application Number
- CN202410299574.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-03-15
AI Technical Summary
Traditional NiCuZn ferrite materials require high-temperature sintering during the preparation process, resulting in increased production costs and changes in magnetic properties. They have high magnetic permeability, large magnetic losses, and low mechanical strength, and cannot meet the low magnetic permeability requirements in specific applications.
Using a low-temperature sintering process and through specific ingredient ratio and additive design, ultra-low magnetic permeability NiCuZn materials are prepared, including Fe2O3, ZnO, NiO and additives SiO2, CaCO3, WO3, Bi2O3, to control the magnetic domain structure and oxygen defects, and reduce the magnetic permeability efficiency and improve mechanical strength.
It achieves superior sintering performance, good current saturation performance, ultra-low magnetic permeability and high mechanical strength, reduces magnetic loss, is suitable for high-frequency applications, has uniform appearance and color, and is suitable for industrial production.
Smart Images

Figure BDA0004743386700000051 
Figure BDA0004743386700000061 
Figure BDA0004743386700000121
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of soft ferrite materials, and in particular to a low-temperature sintered ultra-low magnetic permeability NiCuZn material and a preparation method thereof. Background Art
[0002] Ferrite is a ferromagnetic ceramic material that is widely used in electronics, communications, energy, environmental protection and other fields. Among ferrite materials, NiCuZn ferrite is regarded as an important soft magnetic material due to its excellent magnetic properties and good sintering performance.
[0003] However, the traditional NiCuZn ferrite materials usually need to be sintered at a higher temperature during the preparation process, which not only increases the production cost, but also may cause changes in the crystal structure inside the material, affecting its magnetic properties. In addition, the magnetic permeability of the NiCuZn ferrite materials currently prepared is generally high, while the magnetic loss is high and the mechanical strength is low, which cannot meet the demand for low magnetic permeability materials in certain specific applications.
[0004] For example, in some magnetic field measurement or magnetic induction sensor applications, low magnetic permeability materials are needed to reduce the impact of magnetic interference and improve measurement accuracy and stability; in the field of electromagnetic interference suppression, the problem of electromagnetic interference in electronic equipment and systems is becoming increasingly serious. Low magnetic permeability materials can be used for electromagnetic shielding and interference suppression, effectively reducing the impact of electromagnetic radiation and interference; in the field of energy conversion, in energy conversion technologies such as magnetic power generation and magnetohydrodynamic power generation, low magnetic permeability materials are needed to reduce magnetic losses and improve energy conversion efficiency; and in the field of biomedicine, in biomedical technologies such as nuclear magnetic resonance imaging and magnetic separation, low magnetic permeability materials are needed to reduce the impact on the organism and improve imaging quality and separation effect.
[0005] Therefore, there is an urgent need to prepare a NiCuZn ferrite material with ultra-low magnetic permeability and high mechanical strength to meet the needs in specific applications. Summary of the invention
[0006] In order to solve at least one of the above technical problems, a NiCuZn ferrite material with ultra-low magnetic permeability and high mechanical strength is developed. The present application provides a low-temperature sintered ultra-low magnetic permeability NiCuZn material and a preparation method thereof.
[0007] On the one hand, the present application provides a low-temperature sintered ultra-low magnetic permeability NiCuZn material, comprising a main component and an additive; wherein the main component comprises the following molar percentage raw materials: Fe2O3 40.0-48.0mol%, ZnO 1-10mol%, NiO35-45mol%, and the remainder is CuO; based on the weight of the main component, the additive comprises the following mass percentage raw materials: SiO2 1.0-5.0wt%, CaCO3 1.5-7.5wt%, WO3 0.5-1.5wt% and Bi2O3 0.1-0.5wt% One or more.
[0008] By adopting the above technical solution, the NiCuZn ferrite material prepared by the present application has good sintering performance, excellent current saturation performance, ultra-low magnetic permeability and excellent mechanical strength through unique composition and ratio design and selection of additives, and at the same time has a high Q value in high frequency, effectively reducing magnetic loss, and the prepared NiCuZn ferrite material has uniform appearance and color;
[0009] The application uses a specific ratio of Fe2O3 to control the magnetic properties of the material; the use of a specific ratio of ZnO can promote the formation of oxygen defects in the material, and these oxygen defects can serve as pinning centers for the movement of magnetic domain walls, hindering the rotation of magnetic domains, thereby reducing magnetic permeability; and the use of a specific ratio of NiO has strong magnetism and can significantly affect the magnetic domain structure and magnetic properties of the material. By controlling the content of NiO, excessive magnetic domains are generated in the material, hindering the rotation of magnetic domains, thereby reducing magnetic permeability;
[0010] The application uses a specific ratio of the additive SiO2 to improve the insulation performance and mechanical strength of the material. At the same time, SiO2 can also work together with other additives to further optimize the magnetic properties of the material. The interaction between the specific ratio of CaCO3, WO3, and Bi2O3 and the main components affects the magnetic properties and sintering performance of the material, and can improve the microstructure and magnetic domain structure of the material, thereby improving the magnetic properties and current saturation capacity.
[0011] Optionally, the additive includes the following raw materials in mass percentage: CaCO3 1.5-7.5wt% and WO3 0.5-1.5wt%.
[0012] Preferably, the additive comprises the following raw materials in mass percentage: CaCO3 4.5wt% and WO3 1wt%.
[0013] By adopting the above technical solution, the present application adopts specific CaCO3 and WO3 that can work together to promote the formation of lattice defects in the material. These defects can pin the movement of magnetic domains and further reduce the magnetic permeability.
[0014] Preferably, the additive comprises the following raw materials in mass percentage: SiO2 3wt%, WO3 1wt% and Bi2O3 0.3wt%.
[0015] Preferably, the additive comprises the following raw materials in mass percentage: SiO2 3wt%, CaCO3 4.5wt% and Bi2O3 0.3wt%.
[0016] Preferably, the additive comprises the following raw materials in mass percentage: SiO2 3wt%, CaCO3 4.5wt%, WO3 1wt% and Bi2O3 0.3wt%.
[0017] By adopting the above technical solution and using a specific additive system, the NiCuZn ferrite material prepared in this application has better comprehensive performance.
[0018] Optionally, the main component includes the following raw materials in molar percentage: Fe2O3 42.2-45.6mol%, ZnO 3.5-6.3mol%, NiO 38.4-40.5mol%, and the balance is CuO.
[0019] Preferably, the main component includes the following raw materials in molar percentage: Fe2O3 43.5mol%, ZnO 4.1mol%, NiO 39.2mol%, and the balance is CuO.
[0020] By adopting the above technical solution, the present application adopts a more optimal ratio of main component raw materials, and the comprehensive performance of the prepared NiCuZn ferrite material is more excellent.
[0021] Optionally, the additive further comprises one or both of Y2O3 0.1-0.6wt% and Ga2O3 1.0-2.2wt%.
[0022] Preferably, the additive further comprises Y2O3 0.1-0.6wt% and Ga2O3 1.0-2.2wt%.
[0023] Preferably, the additive further comprises 0.4 wt% of Y2O3 and 1.8 wt% of Ga2O3.
[0024] By adopting the above technical solution, adding a specific amount of Y2O3 and Ga2O3 to the additive of the present application can effectively improve the crystallinity of ferrite, reduce impurities and defects, improve magnetic properties, and improve mechanical strength and high-frequency impedance characteristics.
[0025] On the other hand, the present application provides a method for preparing a low temperature sintered ultra-low magnetic permeability NiCuZn material, comprising the following steps:
[0026] S1, mixing the main components and additives, ball milling and spray granulation, and then pre-calcining to prepare a pre-calcined material;
[0027] S2, mixing and stirring the pre-burned material with a binder, deionized water, a defoamer and a dispersant, and then performing a first ball milling and screening process and a second ball milling and screening process to prepare a mixed material;
[0028] S3, taking the mixed material and performing spray granulation to obtain granular material;
[0029] S4, placing the granular material into a mold for compression molding to prepare a green body;
[0030] S5. Sintering the green body to prepare the low-temperature sintered ultra-low magnetic permeability NiCuZn material.
[0031] By adopting the above technical scheme, the preparation method of the low-temperature sintered ultra-low magnetic permeability NiCuZn material of the present application is simple and efficient to operate, environmentally friendly, and can be industrially produced; at the same time, the prepared NiCuZn material has excellent comprehensive performance.
[0032] Optionally, in S1, the pre-firing temperature is 850-950° C., and the holding time is 150-200 min.
[0033] Optionally, in S2, the average particle size D50 of the mixture is 0.4-0.8 μm.
[0034] Preferably, in S2, the average particle size D50 of the mixture is 0.4-0.6 μm.
[0035] Optionally, in S3, the adhesive is selected from a polyvinyl alcohol solution, and the weight of the polyvinyl alcohol is 0.8-1.5wt% of the weight of the mixture.
[0036] Optionally, in S5, the sintering temperature is 1000-1150° C., and the holding time is 150-200 min.
[0037] Preferably, in S5, the sintering temperature is 1050-1100°C.
[0038] In summary, the present invention includes at least one of the following beneficial technical effects:
[0039] 1. The NiCuZn ferrite material prepared by the present application has good sintering performance, excellent current saturation performance, ultra-low magnetic permeability and excellent mechanical strength through unique composition and ratio design and selection of additives. At the same time, it has a high Q value in high frequency, which effectively reduces magnetic loss;
[0040] 2. The application uses a specific ratio of Fe2O3 to control the magnetic properties of the material; the use of a specific ratio of ZnO can promote the formation of oxygen defects in the material, which can serve as pinning centers for the movement of magnetic domain walls, hindering the rotation of magnetic domains, thereby reducing magnetic permeability; and the use of a specific ratio of NiO has strong magnetism and can significantly affect the magnetic domain structure and magnetic properties of the material. By controlling the content of NiO, excessive magnetic domains are generated in the material, hindering the rotation of magnetic domains, thereby reducing magnetic permeability;
[0041] 3. The application uses a specific ratio of additive SiO2 to improve the insulation performance and mechanical strength of the material. At the same time, SiO2 can also work together with other additives to further optimize the magnetic properties of the material; the interaction between the specific ratio of CaCO3, WO3, Bi2O3 and the main component affects the magnetic properties and sintering properties of the material, and can improve the microstructure and magnetic domain structure of the material, thereby improving the magnetic properties and current saturation capacity;
[0042] 4. The preparation method of the low-temperature sintered ultra-low magnetic permeability NiCuZn material of the present application is simple and efficient to operate, environmentally friendly, and can be industrially produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 The frequency-impedance characteristic curve of the NiCuZn material prepared in Example 4;
[0044] Figure 2 This is the appearance picture of the NiCuZn material prepared in Example 24. DETAILED DESCRIPTION
[0045] The present application is further described in detail below with reference to the accompanying drawings and embodiments.
[0046] The present application designs a low-temperature sintered ultra-low magnetic permeability NiCuZn material, comprising a main component and an additive; wherein the main component comprises the following raw materials in molar percentage: Fe2O3 40.0-48.0mol%, ZnO 1-10mol%, NiO 35-45mol%, and the remainder is CuO; based on the weight of the main component, the additive comprises the following raw materials in mass percentage: one or more of SiO2 1.0-5.0wt%, CaCO3 1.5-7.5wt%, WO3 0.5-1.5wt% and Bi2O3 0.1-0.5wt%.
[0047] The present invention provides a method for preparing a low temperature sintered ultra-low magnetic permeability NiCuZn material, comprising the following steps:
[0048] S1, mixing the main components and additives, ball milling and spray granulation, and then pre-calcining to prepare a pre-calcined material;
[0049] S2, mixing and stirring the pre-burned material with a binder, deionized water, a defoamer and a dispersant, and then performing a first ball milling and screening process and a second ball milling and screening process to prepare a mixed material;
[0050] S3, spray granulating the mixture to obtain granular material;
[0051] S4, placing the granular material into a mold for compression molding to prepare a green body;
[0052] S5. Sintering the green body to prepare the low-temperature sintered ultra-low magnetic permeability NiCuZn material. Specific embodiments
[0054] The raw material models of this application are as follows. Unless otherwise specified, the raw materials of this application are all commercially available:
[0055] Fe2O3: purity 99%;
[0056] ZnO: purity 99%;
[0057] NiO: purity 98.5-99%;
[0058] CuO: purity 99.9%;
[0059] SiO2: purity 99.9%;
[0060] CaCO3: purity 99%;
[0061] WO3: purity 99.9%;
[0062] Bi2O3: purity 99.9%;
[0063] Y2O3: purity 99.9%;
[0064] Ga2O3: purity 99%;
[0065] Polyvinyl alcohol: purity 99.99%;
[0066] Defoamer: BYK-024 silicone defoamer;
[0067] Polycarboxylic acid amine salt dispersant 5029: Weifang Dadong Chemical Co., Ltd.
[0068] Test items and test methods Saturation current: When current passes through a ferrite ring, magnetic saturation of the magnetic body will occur, and the inductance will decrease. This characteristic is called the DC superposition characteristic. When testing the sample of the embodiment, the number of coils is 10. The HP4284A-LCR tester is used to continuously pass a DC current through the sample, resulting in a decrease in inductance. The current value corresponding to a decrease in inductance of 30% is defined as the saturation current;
[0069] Initial magnetic permeability: Use E4991B impedance analyzer to test the sample, set the frequency to 4MHz, input the sample outer diameter, inner diameter, height parameters, and read the panel data to obtain the initial magnetic permeability value of the sample;
[0070] Q value at 20MHz: 20 turns of insulated copper wire were evenly wound on the surface of the sintered magnetic ring sample, and its Q value at 20MHz was tested using Agilent (Agilent Technologies, USA) equipment E4991+16192;
[0071] Hardness: Tested according to GB / T9097-2016 Apparent Hardness and Microhardness of Sintered Metal Materials;
[0072] Impedance: The impedance of the samples was measured using an E4991B impedance analyzer.
[0073] Examples 1-15
[0074] The specific raw material weights of the NiCuZn materials of Examples 1-15 are shown in Table 1.
[0075] Table 1
[0076]
[0077]
[0078] The balance of the main component is CuO.
[0079] Example 1
[0080] A method for preparing a low temperature sintered ultra-low magnetic permeability NiCuZn material comprises the following steps:
[0081] S1. The main components and additives are mixed, ball-milled and spray-granulated respectively, and then pre-calcined at a temperature of 850° C. for a holding time of 200 min to prepare pre-calcined material 1 and pre-calcined material 2;
[0082] S2, after mixing and stirring the pre-sintered material 1 and the pre-sintered material 2, a ball milling and screening process is performed once and a second ball milling and screening process is performed to prepare a mixture with an average particle size D50 of 0.6 μm; wherein the weight ratio of the raw material, deionized water and steel balls in the two ball milling processes is 2:1:6, the first ball milling time is 3 hours, and the second ball milling time is 1 hour
[0083] S3, taking the mixed material and the binder, defoamer and dispersant, mixing and stirring to obtain a slurry, spray granulation, and obtaining a granular material with a water content of 0.2wt%, wherein the defoamer is added in an amount of 2mL / kg and the dispersant is added in an amount of 1mL / kg;
[0084] S4, placing the granular material into a mold for compression molding to prepare a green body, the specification of the green body is φ25×φ15×7.5mm;
[0085] S5, sintering the green body at a sintering temperature of 1050° C. for a holding time of 200 min to obtain the low-temperature sintered ultra-low magnetic permeability NiCuZn material;
[0086] Among them, in S3, the defoamer is BYK-024 silicone defoamer; the dispersant is polycarboxylic acid amine salt dispersant 5029; the adhesive is a polyvinyl alcohol solution with a concentration of 10wt%; and the weight of the polyvinyl alcohol is 0.8wt% of the weight of the mixture.
[0087] Example 2
[0088] A method for preparing a low temperature sintered ultra-low magnetic permeability NiCuZn material comprises the following steps:
[0089] S1. The main components and additives are mixed, ball-milled and spray-granulated respectively, and then pre-calcined at a temperature of 880° C. for a holding time of 170 min to prepare pre-calcined materials 1 and 2;
[0090] S2, after mixing and stirring the pre-sintered material 1 and the pre-sintered material 2, perform a first ball milling and screening process and a second ball milling and screening process to prepare a mixture with an average particle size D50 of 0.5 μm; wherein the weight ratio of the raw material, deionized water and steel balls during the two ball milling processes is 2:1:6, the first ball milling time is 3 hours, and the second ball milling time is 1 hour;
[0091] S3, taking the mixed material binder, defoamer and dispersant, mixing and stirring to obtain a slurry, spray granulation, and obtaining a granular material with a water content of 0.2wt%; wherein the amount of defoamer added is 2mL / kg, and the amount of dispersant added is 1mL / kg;
[0092] S4, placing the granular material into a mold for compression molding to prepare a green body, the specification of the green body is φ25×φ15×7.5mm;
[0093] S5. Sintering the green body at a sintering temperature of 1070°C and a holding time of 180 min to obtain the low-temperature sintered ultra-low magnetic permeability NiCuZn material; wherein, in S3, the defoaming agent is BYK-024 silicone defoaming agent; the dispersant is polycarboxylic acid amine salt dispersant 5029; the binder is a polyvinyl alcohol solution with a concentration of 10wt%; and the weight of the polyvinyl alcohol is 1wt% of the weight of the mixture.
[0094] Example 3
[0095] A method for preparing a low temperature sintered ultra-low magnetic permeability NiCuZn material comprises the following steps:
[0096] S1. The main components and additives are mixed, ball-milled and dried respectively, and then pre-fired at a temperature of 910° C. for a holding time of 160 min to prepare pre-fired material 1 and pre-fired material 2;
[0097] S2, after mixing and stirring the pre-sintered material 1 and the pre-sintered material 2, a ball milling and screening process is performed once and a second ball milling and screening process is performed to prepare a mixture with an average particle size D50 of 0.4 μm; wherein the weight ratio of the raw material, deionized water and steel balls during the two ball milling processes is 2:1:6, the first ball milling time is 3 h, and the second ball milling time is 1 h;
[0098] S3, taking the mixed material binder, defoamer and dispersant, mixing and stirring to obtain a slurry, spray granulation, and obtaining a granular material with a water content of 0.2wt%; wherein the amount of defoamer added is 2mL / kg, and the amount of dispersant added is 1mL / kg;
[0099] S4, placing the granular material into a mold for compression molding to prepare a green body, the specification of the green body is φ25×φ15×7.5mm;
[0100] S5, sintering the green body at a sintering temperature of 1090° C. for a holding time of 160 min to obtain the low-temperature sintered ultra-low magnetic permeability NiCuZn material;
[0101] Among them, in S3, the defoamer is BYK-024 silicone defoamer; the dispersant is polycarboxylic acid amine salt dispersant 5029; the adhesive is a polyvinyl alcohol solution with a concentration of 10wt%; and the weight of the polyvinyl alcohol is 1.5wt% of the weight of the mixture.
[0102] Example 4
[0103] A method for preparing a low temperature sintered ultra-low magnetic permeability NiCuZn material comprises the following steps:
[0104] S1. The main components and additives are mixed, ball-milled and spray-granulated respectively, and then pre-calcined at a temperature of 950° C. for a holding time of 150 min to prepare pre-calcined material 1 and pre-calcined material 2;
[0105] S2, after mixing and stirring the pre-sintered material 1 and the pre-sintered material 2, a ball milling and screening process is performed once and a second ball milling and screening process is performed to prepare a mixture with an average particle size D50 of 0.8 μm; wherein the weight ratio of the raw material, deionized water and steel balls during the two ball milling processes is 2:1:6, the first ball milling time is 3 hours, and the second ball milling time is 1 hour;
[0106] S3, taking the mixed material binder, defoamer and dispersant, mixing and stirring to obtain a slurry, spray granulation, and obtaining a granular material with a water content of 0.2wt%; wherein the amount of defoamer added is 2mL / kg, and the amount of dispersant added is 1mL / kg;
[0107] S4, placing the granular material into a mold for compression molding to prepare a green body, the specification of the green body is φ25×φ15×7.5mm;
[0108] S5, sintering the green body at a sintering temperature of 1100° C. for a holding time of 150 min to obtain the low-temperature sintered ultra-low magnetic permeability NiCuZn material;
[0109] Among them, in S3, the defoamer is BYK-024 silicone defoamer; the dispersant is polycarboxylic acid amine salt dispersant 5029; the adhesive is a polyvinyl alcohol solution with a concentration of 10wt%; the weight of the polyvinyl alcohol is 0.1.3wt% of the weight of the mixture.
[0110] Embodiment 5-7
[0111] The preparation method of a low-temperature sintered ultra-low magnetic permeability NiCuZn material in Examples 5-7 is consistent with the preparation method in Example 1.
[0112] Embodiment 8-15
[0113] The preparation method of a low-temperature sintered ultra-low magnetic permeability NiCuZn material of Examples 8-15 is consistent with the preparation method of Example 2.
[0114] Example 16
[0115] Based on Example 14, except that the D50 of the mixture in S2 is 0.8 μm, the other components and preparation methods are consistent with Example 14.
[0116] Embodiment 17
[0117] Based on Example 14, except that the sintering temperature in S5 is 1000° C., the other components and preparation methods are consistent with Example 14.
[0118] Embodiment 18
[0119] Based on Example 14, except that the sintering temperature in S5 is 1150°C, the other components and preparation methods are consistent with Example 14.
[0120] Embodiment 19
[0121] Based on Example 14, except that the additive further includes 0.1wt% Y2O3, the rest of the preparation methods are consistent with Example 14; wherein, a preparation method of a low temperature sintered ultra-low magnetic permeability NiCuZn material comprises the following steps:
[0122] S1. The main components and additives are mixed, ball-milled and spray-granulated respectively, and then pre-calcined at a temperature of 880° C. for a holding time of 170 min to prepare pre-calcined materials 1 and 2;
[0123] S2, after mixing and stirring the pre-sintered material 1 and the pre-sintered material 2, a ball milling and screening process is performed once and a second ball milling and screening process is performed to prepare a mixture with an average particle size D50 of 0.5 μm; wherein, the weight ratio of the raw material, deionized water and steel balls in the two ball milling processes is 2:1:6, the first ball milling time is 3 hours, and the second ball milling time is 1 hour;
[0124] S3, taking the mixed material binder, defoamer and dispersant, mixing and stirring to obtain a slurry, spray granulation, and obtaining a granular material with a water content of 0.2wt%; wherein the amount of defoamer added is 2mL / kg, and the amount of dispersant added is 1mL / kg;
[0125] S4, placing the granular material into a mold for compression molding to prepare a green body, the specification of the green body is φ25×φ15×7.5mm;
[0126] S5, sintering the green body at a sintering temperature of 1070° C. for a holding time of 180 min to prepare the low-temperature sintered ultra-low magnetic permeability NiCuZn material;
[0127] Among them, in S3, the defoamer is BYK-024 silicone defoamer; the dispersant is polycarboxylic acid amine salt dispersant 5029; the adhesive is a polyvinyl alcohol solution with a concentration of 10wt%; and the weight of the polyvinyl alcohol is 1wt% of the weight of the mixture.
[0128] Embodiment 20
[0129] Based on Example 14, except that the additive further includes 1.0wt% of Ga2O3, the rest of the preparation methods are consistent with Example 14; wherein, a preparation method of a low-temperature sintered ultra-low magnetic permeability NiCuZn material comprises the following steps:
[0130] S1, respectively mixing the main component and the additive, ball milling and drying, ball milling and spray granulation, and then pre-calcining, the pre-calcining temperature is 880° C., the heat preservation time is 170 min, to prepare pre-calcined material 1 and pre-calcined material 2;
[0131] S2, after mixing and stirring the pre-sintered material 1 and the pre-sintered material 2, the pre-sintered material 1 and the pre-sintered material 2 are subjected to a primary ball milling and screening process and a secondary ball milling and screening process to prepare a mixture with an average particle size D50 of 0.5 μm; wherein the weight ratio of the raw material, deionized water and steel balls in the two ball milling processes is 2:1:6, the primary ball milling time is 3 h, and the secondary ball milling time is 1 h;
[0132] S3, taking the mixed material and the binder, defoamer and dispersant, mixing and stirring to obtain a slurry, spray granulation, and obtaining a granular material with a water content of 0.2wt%; wherein the amount of the defoamer added is 2mL / kg, and the amount of the dispersant added is 1mL / kg;
[0133] S4, placing the granular material into a mold for compression molding to prepare a green body, the specification of the green body is φ25×φ15×7.5mm;
[0134] S5, sintering the green body at a sintering temperature of 1070° C. for a holding time of 180 min to prepare the low-temperature sintered ultra-low magnetic permeability NiCuZn material;
[0135] Among them, in S3, the defoamer is BYK-024 silicone defoamer; the dispersant is polycarboxylic acid amine salt dispersant 5029; the adhesive is a polyvinyl alcohol solution with a concentration of 10wt%; and the weight of the polyvinyl alcohol is 1wt% of the weight of the mixture.
[0136] Examples 21-23
[0137] Based on Example 14, except that the additives also include Y2O3 and Ga2O3, the rest of the preparation methods are consistent with Example 14; wherein, a preparation method of a low-temperature sintered ultra-low magnetic permeability NiCuZn material comprises the following steps:
[0138] S1, respectively mixing the main component and the additive, ball milling and drying, ball milling and spray granulation, and then pre-calcining, the pre-calcining temperature is 880° C., the heat preservation time is 170 min, to prepare pre-calcined material 1 and pre-calcined material 2;
[0139] S2, after mixing and stirring the pre-sintered material 1 and the pre-sintered material 2, the pre-sintered material 1 and the pre-sintered material 2 are subjected to a primary ball milling and screening process and a secondary ball milling and screening process to prepare a mixture with an average particle size D50 of 0.5 μm; wherein the weight ratio of the raw material, deionized water and steel balls in the two ball milling processes is 2:1:6, the primary ball milling time is 3 h, and the secondary ball milling time is 1 h;
[0140] S3, taking the mixed material and the binder, defoamer and dispersant, mixing and stirring to obtain a slurry, spray granulation, and obtaining a granular material with a water content of 0.2wt%; wherein the amount of the defoamer added is 2mL / kg, and the amount of the dispersant added is 1mL / kg;
[0141] S4, placing the granular material into a mold for compression molding to prepare a green body, the specification of the green body is φ25×φ15×7.5mm;
[0142] S5, sintering the green body at a sintering temperature of 1070° C. for a holding time of 180 min to prepare the low-temperature sintered ultra-low magnetic permeability NiCuZn material;
[0143] Among them, in S3, the defoamer is BYK-024 silicone defoamer; the dispersant is polycarboxylic acid amine salt dispersant 5029; the adhesive is a polyvinyl alcohol solution with a concentration of 10wt%; and the weight of the polyvinyl alcohol is 1wt% of the weight of the mixture.
[0144] Embodiment 21
[0145] Y2O3 0.1wt% and Ga2O3 1.0wt%.
[0146] Embodiment 22
[0147] Y2O3 0.4wt% and Ga2O3 1.8wt%.
[0148] Embodiment 23
[0149] Y2O3 0.6wt% and Ga2O3 2.2wt%.
[0150] Embodiment 24
[0151] Based on Example 22, except for S1 and S2, the rest of the preparation methods are consistent with Example 22;
[0152] Among them, a preparation method of low temperature sintered ultra-low magnetic permeability NiCuZn material is as follows:
[0153] S1. After mixing and stirring the main component and the additive, ball milling and spray granulation are performed, and then pre-calcination is performed at a pre-calcination temperature of 880° C. and a heat preservation time of 170 min to prepare a pre-calcined material;
[0154] S2, the pre-sintered material is subjected to a first ball milling and screening process and a second ball milling and screening process to prepare a mixture with an average particle size D50 of 0.5 μm; wherein the weight ratio of the raw material, deionized water and steel balls in the two ball milling processes is 2:1:6, the first ball milling time is 3 hours, and the second ball milling time is 1 hour;
[0155] S3, taking the mixed material and the binder, defoamer and dispersant, mixing and stirring to obtain a slurry, spray granulation, and obtaining a granular material with a water content of 0.2wt%; wherein the amount of the defoamer added is 2mL / kg, and the amount of the dispersant added is 1mL / kg;
[0156] S4, placing the granular material into a mold for compression molding to prepare a green body, the specification of the green body is φ25×φ15×7.5mm;
[0157] S5, sintering the green body at a sintering temperature of 1070° C. for a holding time of 180 min to prepare the low-temperature sintered ultra-low magnetic permeability NiCuZn material;
[0158] Among them, in S3, the defoamer is BYK-024 silicone defoamer; the dispersant is polycarboxylic acid amine salt dispersant 5029; the adhesive is a polyvinyl alcohol solution with a concentration of 10wt%; and the weight of the polyvinyl alcohol is 1wt% of the weight of the mixture.
[0159] Embodiment 25
[0160] Based on Example 24, except for S2 and S3, the rest of the preparation methods are the same as those of Example 24;
[0161] Among them, a preparation method of low temperature sintered ultra-low magnetic permeability NiCuZn material is as follows:
[0162] S1. After mixing and stirring the main component and the additive, ball milling and spray granulation are performed, and then pre-calcination is performed at a pre-calcination temperature of 880° C. and a heat preservation time of 170 min to prepare a pre-calcined material;
[0163] S2, the pre-sintered material is mixed with a binder, deionized water, a defoamer and a dispersant to obtain a slurry, and a ball milling and screening process is performed once and twice to prepare a mixture with an average particle size D50 of 0.5 μm, wherein the weight ratio of the raw material, deionized water and steel balls during the two ball milling processes is 2:1:6, the first ball milling time is 3h, and the second ball milling time is 1h; the amount of the defoamer added is 2mL / kg, and the amount of the dispersant added is 1mL / kg;
[0164] S3, taking the mixed material and spray granulating it to obtain granules with a water content of 0.2wt%; S4, putting the granules into a mold and pressing it to prepare a green body, the specification of the green body is φ25×φ15×7.5mm;
[0165] S5, sintering the green body at a sintering temperature of 1070° C. for a holding time of 180 min to prepare the low-temperature sintered ultra-low magnetic permeability NiCuZn material;
[0166] Among them, in S3, the defoamer is BYK-024 silicone defoamer; the dispersant is polycarboxylic acid amine salt dispersant 5029; the adhesive is a polyvinyl alcohol solution with a concentration of 10wt%; and the weight of the polyvinyl alcohol is 1wt% of the weight of the mixture.
[0167] Comparative Examples 1-6
[0168] Comparative Example 1
[0169] Based on Example 2, except that the molar percentage of Fe2O3 in the main component is 35% and the molar percentage of CuO is 23.1%, the other components and preparation methods are consistent with those of Example 2.
[0170] Comparative Example 2
[0171] Based on Example 2, except that the molar percentage of Fe2O3 in the main component is 50% and the molar percentage of CuO is 8.1%, the other components and preparation methods are consistent with those of Example 2.
[0172] Comparative Example 3
[0173] Based on Example 2, except that the molar percentage of ZnO in the main component is 12% and the molar percentage of CuO is 7.4%, the other components and the preparation method are consistent with those in Example 2.
[0174] Comparative Example 4
[0175] Based on Example 2, except that the molar percentage of ZnO in the main component is 0.5% and the molar percentage of CuO is 18.9%, the other components and the preparation method are consistent with those in Example 2.
[0176] Comparative Example 5
[0177] Based on Example 2, except that the molar percentage of NiO in the main component is 30% and the molar percentage of CuO is 24.3%, the other components and the preparation method are consistent with those in Example 2.
[0178] Comparative Example 6
[0179] Based on Example 2, except that the molar percentage of NiO in the main component is 48% and the molar percentage of CuO is 6.3%, the other components and the preparation method are consistent with those of Example 2.
[0180] The NiCuZn materials prepared in Examples 1-21 and Comparative Examples 1-6 were subjected to performance testing, and the test results are shown in Table 2.
[0181] Table 2
[0182]
[0183]
[0184] It can be seen from Examples 1-4, Comparative Examples 1-6 and Table 2 that the NiCuZn ferrite material prepared by the present application using specific components, ratio design and additive selection has excellent current saturation performance, ultra-low magnetic permeability, high Q value, excellent hardness and high-frequency impedance characteristics; at the same time, Figure 1 It can be seen that the NiCuZn ferrite material prepared in Example 4 of the present application has excellent high-frequency impedance characteristics, and the impedance is 1682Ω at 1000MHz;
[0185] It can be seen from Examples 5-7, 1 and Table 2 that the NiCuZn ferrite material prepared by using SiO2 and Bi2O3 as additives of the present application has better comprehensive performance than the NiCuZn ferrite material prepared by adding SiO2 or Bi2O3 alone; it can be seen from Examples 8-10, 2 and Table 2 that the additives of the present application using CaCO3 and WO3 at the same time can work together to promote the formation of lattice defects in the material, and these defects can pin the movement of magnetic domains and further reduce the magnetic permeability;
[0186] It can be seen from Examples 11-13, 9 and Table 2 that the additives of the present application simultaneously using specific contents of SiO2, CaCO3, WO3 and Bi2O3 are more conducive to reducing the magnetic permeability and improving the current saturation performance, and the comprehensive performance of the prepared NiCuZn ferrite material is more excellent;
[0187] It can be seen from Examples 13-15 and Table 2 that the present application adopts a more optimal ratio of main components, and the comprehensive performance of the prepared NiCuZn ferrite material is more excellent;
[0188] It can be seen from Examples 16, 14 and Table 2 that although the saturation current is better and the magnetic permeability is lower when the D50 of the mixture in S2 is higher than the value range, the prepared NiCuZn ferrite material has poor mechanical properties, high brittleness, and reduced contact area between particles, which is not conducive to sintering.
[0189] It can be seen from Examples 17-18, 14 and Table 2 that when the sintering temperature in S5 is too high or too low, although the saturation performance and magnetic permeability of the prepared NiCuZn ferrite material are good, it will cause the lattice structure inside the material to be unstable, thereby reducing the mechanical strength; It can be seen from Examples 19-23, 14 and Table 2 that Y2O3 and Ga2O3 are also added to the additives of the present application, which can effectively improve the crystallinity of the ferrite, reduce impurities and defects, improve magnetic properties, and improve mechanical strength;
[0190] It can be seen from Examples 22, 24, 25 and Table 2 that in S1 of the present application, the main component and the additive are mixed and stirred, and then ball milled, spray granulated and pre-calcined. The prepared pre-calcined material has higher dispersibility and is more conducive to improving the comprehensive performance of the ferrite material; and in the grinding stage in S2, a binder, deionized water, a defoamer and a dispersant are added to perform ball milling and screening, and secondary ball milling and screening, which further promotes the dispersion uniformity of the mixture, and the comprehensive performance of the prepared ferrite material is excellent; at the same time, Figure 2 It can be seen that the NiCuZn ferrite material prepared in this application has a uniform black appearance;
[0191] It can be seen from Comparative Examples 1-6, Example 2 and Table 2 that the NiCuZn ferrite material prepared by the present application using specific molar percentages of Fe2O3, NiO and ZnO has excellent current saturation performance and ultra-low magnetic permeability.
[0192] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, all equivalent changes made according to the principles of the present application should be included in the protection scope of the present application.
Claims
1. A low temperature sintered ultra-low magnetic permeability NiCuZn material, characterized in that: It includes a main component and additives; wherein the main component includes the following raw materials in molar percentage: Fe2O3 40.0-48.0mol%, ZnO 1-10mol%, NiO 35-45mol%, and the balance is CuO; based on the weight of the main component, the additive includes the following raw materials in mass percentage: SiO2 1.0-5.0wt%, CaCO3 1.5-7.5wt%, WO3 0.5-1.5wt% and Bi2O3 0.1-0.5wt%.
2. A low temperature sintered ultra-low magnetic permeability NiCuZn material according to claim 1, characterized in that: The additive includes the following raw materials in mass percentage: SiO2 3wt%, CaCO3 4.5wt%, WO3 1wt% and Bi2O3 0.3wt%.
3. The low temperature sintered ultra-low magnetic permeability NiCuZn material according to claim 1, characterized in that: The main component includes the following raw materials in molar percentage: Fe2O3 42.2-45.6 mol%, ZnO 3.5-6.3 mol%, NiO 38.4-40.5 mol%, and the balance is CuO.
4. The low temperature sintered ultra-low magnetic permeability NiCuZn material according to claim 1, characterized in that: The additives also include one or both of Y2O3 0.1-0.6wt% and Ga2O3 1.0-2.2wt%.
5. A method for preparing the low temperature sintered ultra-low magnetic permeability NiCuZn material according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, mixing the main components and additives, ball milling and spray granulation, and then pre-calcining to prepare a pre-calcined material; S2, mixing and stirring the pre-burned material with a binder, deionized water, a defoamer and a dispersant, and then performing a first ball milling and screening process and a second ball milling and screening process to prepare a mixed material; S3, spray granulating the mixture to obtain granular material; S4, placing the granular material into a mold for compression molding to prepare a green body; S5. Sintering the green body to obtain the low-temperature sintered ultra-low magnetic permeability NiCuZn material.
6. The method for preparing the low temperature sintered ultra-low magnetic permeability NiCuZn material according to claim 5, characterized in that: In S1, the pre-firing temperature is 850-950° C., and the holding time is 150-200 min.
7. The method for preparing the low temperature sintered ultra-low magnetic permeability NiCuZn material according to claim 5, characterized in that: In the S2, the average particle size D50 of the mixture is 0.4-0.8 μm.
8. The method for preparing the low temperature sintered ultra-low magnetic permeability NiCuZn material according to claim 5, characterized in that: In S2, the binder is selected from a polyvinyl alcohol solution, and the weight of the polyvinyl alcohol is 0.8-1.5wt% of the weight of the mixture.
9. The method for preparing the low temperature sintered ultra-low magnetic permeability NiCuZn material according to claim 5, characterized in that: In the step S5, the sintering temperature is 1000-1150° C. and the holding time is 150-200 min.