A double network sodium hyaluronate / silk fibroin gel bridged by aminated silk fibroin and preparation method thereof
By introducing aminated silk fibroin bridges into the sodium hyaluronate/silk fibroin gel to form a double network structure, the problems of gel collapse and biosafety risks in the existing technology are solved, and a stable antibacterial agent is achieved. Degradation and strong cell adhesion ability.
Patent Information
- Application Number
- CN202410185645.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-20
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-02-20
AI Technical Summary
Existing hyaluronic acid gel degrades quickly in the body and is easy to collapse. It has weak cell adhesion ability and is difficult to guide tissue regeneration. Silk fibroin gel, although biodegradable slowly, has insufficient water retention and shaping ability, and the whole body is easy to form after mixing. Collapse and cross-linker residue pose biosafety risks.
Aminated silk fibroin is used as a bridging molecule, and a double network structure of sodium hyaluronate/silk fibroin gel is formed through rapid freezing-low-temperature thawing and low-temperature dialysis processes, and EDC is used to activate silk fibroin side chains and hyaluronic acid Sodium molecules form stable aminated silk fibroin bridges, enhancing the gel's resistance to biodegradation and cell adhesion.
The generated gel has a stable network structure, strong resistance to biodegradation, and is not easy to collapse and disintegrate. The use of low-toxicity EDC as an activator avoids the adverse effects of cross-linking agent residues on biocompatibility and achieves controllable results. Degradation characteristics and strong cell adhesion ability.
Smart Images

Figure CN118085336B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomedical natural polymer gel materials, and specifically relates to a double-network sodium hyaluronate / silk fibroin gel bridged by amino-modified silk fibroin and a preparation method thereof. Background Art
[0002] As a soft tissue filling material, hyaluronic acid gel has the advantages of strong water retention and shaping ability, and has been widely used in the field of medical and plastic surgery. However, it has a fast biodegradation rate and a short retention time in the body; and its adhesion to cells is weak, making it difficult to guide tissue regeneration.
[0003] Silk fibroin has good biocompatibility, slow biodegradation, strong cell adhesion, and can guide tissue regeneration, but its water retention and shaping abilities are insufficient. Blending silk fibroin with hyaluronic acid to prepare a composite component gel can, to a certain extent, utilize the advantages of silk fibroin and hyaluronic acid and overcome their respective shortcomings.
[0004] Prior to the present invention, patent CN114989621A mixed hyaluronic acid, silk fibroin and polyvinyl alcohol, and then cross-linked them with 1-ethyl-3-dimethylaminopropylcarbodiimide and N-hydroxysuccinimide to produce a medical beauty filling gel. However, because it is a mixed network structure between different components, the gel as a whole is prone to collapse when the hyaluronic acid component is degraded; and polyvinyl alcohol, as a synthetic polymer, has a biosafety risk if it remains in the body for a long time.
[0005] Patent CN102836465A mixes silk fibroin microspheres with hyaluronate, and then crosslinks them with divinyl sulfone, ethylene glycol diglycidyl ether, butanediol diglycidyl ether or polypropylene glycol diglycidyl ether to prepare a silk fibroin / hyaluronic acid composite gel. When the hyaluronic acid component is degraded, the gel as a whole is also prone to collapse, and silk fibroin is easily hydrolyzed to a large extent under alkaline conditions.
[0006] Patent CN114601958A uses dopamine to graft aldehyde-modified hyaluronic acid, and then mixes it with silk fibroin and gelatin to react with Schiff base; at the same time, it uses the coordination of trivalent iron ions to prepare hyaluronic acid / silk fibroin double cross-linked injectable hydrogel. The inside of the hydrogel is a mixed network between different components. When the hyaluronic acid component is degraded, the gel as a whole is also prone to collapse; and the addition of the gelatin component will accelerate the degradation of the hydrogel. Summary of the invention
[0007] The purpose of the present invention is to provide a double-network sodium hyaluronate / silk fibroin gel bridged by amino-modified silk fibroin and a preparation method thereof. The gel has the advantages of a firm network structure, strong resistance to biodegradation, and is not easy to collapse and disintegrate.
[0008] The technical solution adopted by the present invention to solve the above problems is: a method for preparing a double-network sodium hyaluronate / silk fibroin gel bridged by aminated silk fibroin, degumming, dissolving and dialyzing mulberry silk to obtain a silk fibroin solution, diluting the silk fibroin solution with purified water to obtain a silk fibroin aqueous solution, wherein the silk fibroin aqueous solution is a non-aminated silk fibroin aqueous solution, and then performing the following processing steps:
[0009] P1: 4-Morpholine Ethanesulfonic acid (MES), spermine, N-hydroxysuccinimide (NHS), and 1-Ethyl-3- (3-Dimethylaminopropyl) -Carbodiimide hydrochloride (EDC) were added to the unaminated silk fibroin aqueous solution in sequence, and after stirring, the solution was subjected to rapid freezing-low temperature thawing, low temperature dialysis-freeze drying in sequence, and then post-processed to obtain aminated silk fibroin solid;
[0010] P2: Mixing sodium hyaluronate aqueous solution, MES, NHS and aminated silk fibroin to obtain a sodium hyaluronate network precursor with aminated silk fibroin as a bridging molecule;
[0011] P3: Mixing the unaminated silk fibroin aqueous solution, MES, NHS, EDC and the aminated silk fibroin to obtain a silk fibroin network prepolymer with the aminated silk fibroin as a bridging molecule;
[0012] P4: The sodium hyaluronate network precursor and the silk fibroin network prepolymer are mixed and reacted to obtain block gel, and then after granulation, washing and balancing, double-network sodium hyaluronate / silk fibroin gel particles bridged by amino-modified silk fibroin are obtained.
[0013] Preferably, the step P1 is as follows:
[0014] A1: Prepare an aqueous solution of unaminated silk fibroin with a mass fraction of 0.1-3%, add MES to the aqueous solution of unaminated silk fibroin, and stir to mix;
[0015] A2: Add spermine, NHS and EDC to the solution in step A1;
[0016] A3: placing the solution in step A2 in a low-temperature refrigerator for rapid freezing, and then thawing at +2 to +8°C to obtain a crude amino-modified silk fibroin solution;
[0017] A4: The crude product of the aminated silk fibroin solution in step A3 is subjected to low-temperature dialysis, and the solution obtained after dialysis is freeze-dried to obtain an aminated silk fibroin solid.
[0018] Preferably, the step P2 is as follows:
[0019] B1: dissolving sodium hyaluronate solid in purified water or water for injection to obtain a sodium hyaluronate solution;
[0020] B2: dissolving the aminated silk fibroin solid in purified water or water for injection to obtain an aminated silk fibroin solution;
[0021] B3: Under ice bath conditions, MES and NHS are dissolved in an aminated silk fibroin solution, and then mixed with a sodium hyaluronate solution to obtain a sodium hyaluronate / aminated silk fibroin mixed solution, and the mixed solution is stirred to obtain a sodium hyaluronate network precursor.
[0022] Preferably, the step P3 is as follows:
[0023] C1: dissolving the aminated silk fibroin solid in purified water to obtain an aminated silk fibroin solution;
[0024] C2: The aminated silk fibroin solution and the unaminated silk fibroin solution are mixed, and MES, NHS and EDC are added to obtain a silk fibroin network prepolymer.
[0025] Preferably, the step P4 is as follows:
[0026] D1: Mix the sodium hyaluronate network precursor and the silk fibroin network prepolymer and react them in an ice bath for 3-5 hours;
[0027] D2: The reactants in step D1 are placed in a low-temperature refrigerator at a temperature of -20 to -80°C and rapidly frozen for 12 to 24 hours, and then thawed at room temperature to obtain a block gel;
[0028] D3: crushing the block gel into granules, and screening to obtain gel particles with a particle size of 100 to 1000 μm;
[0029] D4: The gel particles are placed in a stainless steel mesh basket, placed in pure water or water for injection for oscillation and cleaning for 1-2 days, and then placed in physiological saline for cleaning and balancing for 1-3 days to obtain double-network sodium hyaluronate / silk protein gel particles bridged by amino-modified silk protein.
[0030] More preferably, the step P1 is specifically as follows:
[0031] A1: Prepare an aqueous solution of unaminated silk fibroin with a mass fraction of 0.1-3% at a temperature of +0-6°C; add MES to the aqueous solution of unaminated silk fibroin and stir to make the ES concentration in the solution 3.0-8.0 mmol / L;
[0032] A2: Add spermine to the solution in step A1, stir slowly in an ice bath for 15-30 minutes, then add NHS and EDC, keep in an ice bath, stir slowly for 3-5 hours, and make the mass fractions of spermine, NHS and EDC in the solution 0.5-5.0%, 0.1-4.0%, and 0.2-8.0%, respectively;
[0033] A3: placing the solution of step A2 in a low-temperature refrigerator at a temperature of -20 to -80°C and rapidly freezing it for 24 hours, and then thawing it at +2 to +8°C to obtain a crude amino-modified silk fibroin solution;
[0034] A4: The crude product of the amino-modified silk fibroin solution was dialyzed with 1.0 mmol / L MES solution for 24 hours at +2 to +8°C, and the molecular weight cutoff of the dialysis membrane was 5-10 kDa. It was then dialyzed with purified water for 72 hours. The solution obtained after dialysis was filtered with a filter, and the filtrate was freeze-dried to obtain the amino-modified silk fibroin solid.
[0035] More preferably, the mass fraction of the sodium hyaluronate solution in step B1 is 1.0-5.0%, and the molecular weight of the sodium hyaluronate is 500-3000 kDa; the mass fraction of the aminated silk fibroin solution in step B2 is 1.0-5.0%; the volume ratio of the sodium hyaluronate solution to the aminated silk fibroin solution in step B3 is 70:30-90:10, and the added amounts of MES and NHS powders are both 10%-20% of the sum of the masses of sodium hyaluronate and aminated silk fibroin in the mixed solution.
[0036] More preferably, the mass fractions of the aminated silk fibroin solution and the unaminated silk fibroin solution in step C2 are both 1.0-5.0%, and the volume ratio of the aminated silk fibroin solution to the unaminated silk fibroin solution is 10:90-30:70; the amounts of MES, NHS and EDC added in step C2 are 5-15%, 5-15% and 15-25% of the total amount of aminated and non-aminated silk fibroin, respectively.
[0037] More preferably, the mass ratio of the sodium hyaluronate network precursor to the silk fibroin network prepolymer in step D1 is 10:90-80:20.
[0038] A double-network sodium hyaluronate / silk protein gel bridged by aminated silk protein, wherein the double-network sodium hyaluronate / silk protein gel bridged by aminated silk protein is prepared according to the above-mentioned preparation method of double-network sodium hyaluronate / silk protein gel bridged by aminated silk protein, and the gel is composed of a sodium hyaluronate network bridged by aminated silk protein and a silk protein network bridged by aminated silk protein, and the sodium hyaluronate network and the silk protein network are also bridged by aminated silk protein.
[0039] Preferably, the mass ratio of sodium hyaluronate to the total amount of silk fibroin in the gel is 10:90-85:15.
[0040] In order to enhance the cross-linking stability of the gel itself, the present invention pre-aminates the silk fibroin solution to form active molecules with cross-linking ability, which are respectively prepared with hyaluronic acid and unaminated silk fibroin to form hyaluronic acid network precursor and silk fibroin network prepolymer. The two network prepolymers are copolymerized to form a double-network sodium hyaluronate / silk fibroin gel. The gel prepared by the present invention is stable, not easy to collapse, and has controllable degradation characteristics.
[0041] The principle of the present invention is as follows: 1-Ethyl-3- (3-dimethylaminopropyl) - Carbodiimide hydrochloride (EDC) is used to activate the carboxyl groups of the side chains of silk fibroin, and the carboxyl groups on the side chains of the silk fibroin are reacted with spermine to convert the carboxyl groups on the side chains of the silk fibroin to amino groups, thereby obtaining aminoated silk fibroin; then, the carboxyl groups on the sodium hyaluronate molecules and the carboxyl groups on the side chains of the non-aminoated silk fibroin are respectively activated with EDC, and the aminoated silk fibroin is used as a bridging molecule to respectively generate a sodium hyaluronate network bridged by the aminoated silk fibroin and a silk fibroin network bridged by the aminoated silk fibroin; the sodium hyaluronate network and the silk fibroin network are bridged by the aminoated silk fibroin to obtain a double-network sodium hyaluronate / silk fibroin gel bridged by the aminoated silk fibroin.
[0042] Compared with the prior art, the advantages of the present invention are:
[0043] (1) The gel of the present invention is composed of a sodium hyaluronate network bridged by aminated silk protein and a silk protein network bridged by aminated silk protein, and the sodium hyaluronate network and the silk protein network are also bridged by aminated silk protein, and the network structure is firm, has strong anti-biodegradation ability, and is not easy to collapse or disintegrate. Among them, due to the presence of the silk protein network, the biodegradation speed of the gel is slow, the gel as a whole is not easy to collapse or disintegrate, and the gel has strong cell adhesion ability; because the sodium hyaluronate network is bridged by aminated silk protein inside, and the sodium hyaluronate network and the silk protein network are also bridged by aminated silk protein, the biodegradation of the sodium hyaluronate network can be delayed.
[0044] (2) In the gel preparation process of the present invention, amino-modified silk fibroin is used as a bridging agent, and only low-toxic EDC is used as an activator. EDC does not eventually become a component of the gel and does not change the natural polymer properties of the gel. This can avoid the adverse effects of cross-linking agent residues on the biocompatibility of the gel.
[0045] (4) The present invention mixes a sodium hyaluronate aqueous solution with an aminated silk fibroin aqueous solution to obtain a sodium hyaluronate network precursor with the aminated silk fibroin as a bridging molecule, and mixes an unaminated silk fibroin aqueous solution with an aminated silk fibroin aqueous solution to obtain a silk fibroin network prepolymer with the aminated silk fibroin as a bridging molecule. The sodium hyaluronate network and the silk fibroin network are generated using the same reaction system, which can not only avoid mutual interference between the reaction systems, but also enable the chemically active groups to fully react with each other, thereby improving the reaction efficiency.
[0046] (5) The process of rapid freezing-low temperature re-dissolution (i.e., rapid freezing-low temperature thawing) is used in the preparation process of the gel of the present invention, which not only reduces the probability of the transformation of the silk fibroin from the water-soluble Silk I structure to the insoluble Silk II structure, thereby ensuring that more active groups of the water-soluble silk fibroin are fully exposed, but also maintains the reaction efficiency of the amination, thereby generating a stable amination silk fibroin. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 The process flow chart of the double network sodium hyaluronate / silk fibroin gel bridged by the amino-modified silk fibroin of the present invention.
[0048] Figure 2 It is a schematic diagram of the structure of the double-network sodium hyaluronate / silk fibroin gel bridged by the amino-modified silk fibroin of the present invention. DETAILED DESCRIPTION
[0049] The present invention is further described in detail below with reference to the accompanying drawings.
[0050] like Figure 1As shown, this is a process flow chart of the double-network sodium hyaluronate / silk fibroin gel bridged by amino-modified silk fibroin of the present invention. Example 1
[0051] A method for preparing a double-network sodium hyaluronate / silk fibroin gel bridged by aminated silk fibroin comprises the following steps:
[0052] The silk fibroin in the silk fibroin solution obtained after degumming, dissolving and dialyzing the mulberry silk was named "unaminated silk fibroin", and the mass fraction of the unaminated silk fibroin solution was determined by weight method.
[0053] A1: Dilute the unaminated silk fibroin solution to 0.1% with purified water. Take 1000 mL of 0.1% unaminated silk fibroin solution, pre-cool it in an ice bath for 30 minutes, add MES powder to the solution to make the concentration of MES in the solution 5.0 mmol / L, stir to mix and dissolve MES.
[0054] A2: Add 3 g of spermine to the solution, stir slowly in an ice bath for 15 minutes, then add 10 g and 20 g of NHS and EDC respectively, maintain the ice bath, and stir slowly for 3 hours.
[0055] A3: The solution was quickly frozen in a low-temperature refrigerator at -80°C for 24 hours, and then thawed at +4°C to obtain a crude amino-modified silk fibroin solution.
[0056] A4: The crude product of the amino-modified silk fibroin solution was dialyzed with 1.0 mmol / L MES solution for 24 hours at +4°C, with the molecular weight cutoff of the dialysis membrane being 10 kDa, and then dialyzed with purified water for 72 hours. The solution obtained after dialysis was filtered with a 200-mesh filter, and the filtrate was freeze-dried to obtain an amino-modified silk fibroin solid, which was named S-1.
[0057] B1: Dissolve sodium hyaluronate solid with a molecular weight of 1500 kDa in purified water to obtain a sodium hyaluronate solution with a mass fraction of 1.0%.
[0058] B2: Dissolve the aminated silk fibroin solid in purified water to obtain an aminated silk fibroin solution having the same mass fraction of 1.0%.
[0059] B3: In an ice bath, dissolve 1.0 g of MES and 1.0 g of NHS powder in 200 mL of 1.0% aminated silk fibroin solution, and then mix with 800 mL of 1.0% sodium hyaluronate solution to obtain a sodium hyaluronate / aminated silk fibroin mixed solution. Stir the mixture for 30 minutes to obtain a sodium hyaluronate network precursor.
[0060] C1: Dissolve the aminated silk fibroin solid in purified water to obtain an aminated silk fibroin solution with a mass fraction of 1.0%.
[0061] C2: In an ice bath, an aminated silk fibroin solution with a mass fraction of 1.0% was mixed with an unaminated silk fibroin solution with the same mass fraction in a volume ratio of 30:70. After adding EDC, MES and NHS powders accounting for 20%, 10% and 10% of the total mass of the silk fibroin in the solution, the mixture was slowly stirred for 3 hours to obtain a silk fibroin network prepolymer.
[0062] D1: Mix the sodium hyaluronate network precursor and the silk fibroin network prepolymer in a mass ratio of 60:40 and react in an ice bath for 3 hours.
[0063] D2: The block gel was crushed and granulated, and after screening, gel particles with an average particle size of 548 μm were obtained.
[0064] D3: The gel particles are placed in a stainless steel mesh basket, placed in pure water or water for injection for 1 day for shaking and washing, and then placed in physiological saline for washing and balancing for 1 day to obtain double-network sodium hyaluronate / silk fibroin gel particles bridged by amino-modified silk fibroin, such as Figure 2 As shown in the figure, the mass ratio of sodium hyaluronate to the total amount of silk fibroin in the gel is 48:52. Example 2
[0065] A method for preparing a double-network sodium hyaluronate / silk fibroin gel bridged by aminated silk fibroin comprises the following steps:
[0066] The silk fibroin in the silk fibroin solution obtained after degumming, dissolving and dialyzing the mulberry silk was named "unaminated silk fibroin", and the mass fraction of the unaminated silk fibroin solution was determined by weight method.
[0067] A1: Dilute the unaminated silk fibroin solution to 0.3% by mass with purified water. Take 1000 mL of the 0.3% unaminated silk fibroin solution, pre-cool it in an ice bath for 30 minutes, add MES powder to the solution to make the concentration of MES in the solution 5.0 mmol / L, stir to mix and dissolve MES.
[0068] A2: Add 5 g of spermine to the solution, stir slowly in an ice bath for 15 minutes, then add 30 g of NHS and 60 g of EDC respectively, maintain the ice bath, and stir slowly for 3 hours.
[0069] A3: The solution was quickly frozen in a low-temperature refrigerator at -80°C for 24 hours, and then thawed at +6°C to obtain a crude amino-modified silk fibroin solution.
[0070] A4: The crude product of the amino-modified silk fibroin solution was dialyzed with 1.0 mmol / L MES solution for 24 hours at +6°C, with the molecular weight cutoff of the dialysis membrane being 10 kDa, and then dialyzed with purified water for 72 hours. The solution obtained after dialysis was filtered with a 200-mesh filter, and the filtrate was freeze-dried to obtain an amino-modified silk fibroin solid, which was named S-2.
[0071] B1: Dissolve sodium hyaluronate solid with a molecular weight of 1500 kDa in water for injection to obtain a sodium hyaluronate solution with a mass fraction of 2.5%.
[0072] B2: Dissolve the aminated silk fibroin solid in water for injection to obtain an aminated silk fibroin solution having the same mass fraction of 2.5%.
[0073] B3: In an ice bath, dissolve 2.5 g of MES and 2.5 g of NHS powder in 300 mL of 2.5% aminated silk fibroin solution, and then mix with 700 mL of 2.5% sodium hyaluronate solution to obtain a sodium hyaluronate / aminated silk fibroin mixed solution. Stir the mixture for 30 minutes to obtain a sodium hyaluronate network precursor.
[0074] C1: Dissolve the aminated silk fibroin solid in purified water to obtain an aminated silk fibroin solution with a mass fraction of 2.5%.
[0075] C2: In an ice bath, a 2.5% aminated silk fibroin solution was mixed with an unaminated silk fibroin solution of the same mass fraction at a volume ratio of 10:90. After adding EDC, MES and NHS powders accounting for 20%, 10% and 10% of the total mass of the silk fibroin in the solution, the mixture was slowly stirred for 3 hours to obtain a silk fibroin network prepolymer.
[0076] D1: Mix the sodium hyaluronate network precursor and the silk fibroin network prepolymer in a mass ratio of 20:80 and react in an ice bath for 3 hours.
[0077] D2: The block gel was crushed and granulated, and after screening, gel particles with an average particle size of 563 μm were obtained.
[0078] D3: The gel particles were loaded into a stainless steel mesh basket, placed in pure water or water for injection for oscillation and cleaning for 1 day, and then placed in physiological saline for cleaning and balancing for 1 day to obtain double-network sodium hyaluronate / silk fibroin gel particles bridged by amino-modified silk fibroin. The mass ratio of sodium hyaluronate to the total amount of silk fibroin in the gel was 14:86. Example 3
[0079] A method for preparing a double-network sodium hyaluronate / silk fibroin gel bridged by aminated silk fibroin comprises the following steps:
[0080] The silk fibroin in the silk fibroin solution obtained after degumming, dissolving and dialyzing the mulberry silk was named "unaminated silk fibroin", and the mass fraction of the unaminated silk fibroin solution was determined by weight method.
[0081] A1: Dilute the unaminated silk fibroin solution to 1.0% with purified water. Take 1000 mL of 1.0% unaminated silk fibroin solution, pre-cool it in an ice bath for 30 minutes, add MES powder to the solution to make the concentration of MES in the solution 5.0 mmol / L, stir to mix and dissolve MES.
[0082] A2: Add 30 g of spermine to the solution, slowly stir in an ice bath for 15 minutes, then add 30 g of NHS and 60 g of EDC respectively, maintain the ice bath, and slowly stir for 3 hours.
[0083] A3: The solution was quickly frozen in a low-temperature refrigerator at -80°C for 24 hours, and then thawed at +8°C to obtain a crude amino-modified silk fibroin solution.
[0084] A4: The crude product of the amino-modified silk fibroin solution was dialyzed with 1.0 mmol / L MES solution for 24 hours at +2 to +8°C, with the molecular weight cutoff of the dialysis membrane being 10 kDa, and then dialyzed with purified water for 72 hours. The solution obtained after dialysis was filtered with a 200-mesh filter, and the filtrate was freeze-dried to obtain an amino-modified silk fibroin solid, which was named S-3.
[0085] B1: Sodium hyaluronate solid with a molecular weight of 2580 kDa is dissolved in purified water to obtain a sodium hyaluronate solution with a mass fraction of 3.0%.
[0086] B2: Dissolve the aminated silk fibroin solid in purified water to obtain an aminated silk fibroin solution having the same mass fraction of 3.0%.
[0087] B3: In an ice bath, 3.0 g of MES and 3.0 g of NHS powder were dissolved in 300 mL of an amino-modified silk fibroin solution with a mass fraction of 3.0%, and then mixed with 700 mL of a sodium hyaluronate solution with a mass fraction of 3.0% to obtain a sodium hyaluronate / amino-modified silk fibroin mixed solution. The mixed solution was stirred for 30 minutes to obtain a sodium hyaluronate network precursor.
[0088] C1: Dissolve the aminated silk fibroin solid in purified water to obtain an aminated silk fibroin solution with a mass fraction of 3.0%.
[0089] C2: In an ice bath, a 3.0% aminated silk fibroin solution was mixed with an unaminated silk fibroin solution of the same mass fraction at a volume ratio of 10:90. After adding EDC, MES and NHS powders accounting for 20%, 10% and 10% of the total mass of the silk fibroin in the solution, the mixture was slowly stirred for 3 hours to obtain a silk fibroin network prepolymer.
[0090] D1: Mix the sodium hyaluronate network precursor and the silk fibroin network prepolymer in a mass ratio of 80:20 and react in an ice bath for 3 hours.
[0091] D2: The block gel was crushed and granulated, and after screening, gel particles with an average particle size of 580 μm were obtained.
[0092] D3: The gel particles were placed in a stainless steel mesh basket, placed in pure water or water for injection for oscillation and cleaning for 1 day, and then placed in physiological saline for cleaning and balancing for 1 day to obtain double-network sodium hyaluronate / silk fibroin gel particles bridged by amino-modified silk fibroin. The mass ratio of sodium hyaluronate to the total amount of silk fibroin in the gel was 73:27. Example 4
[0093] A method for preparing a double-network sodium hyaluronate / silk fibroin gel bridged by aminated silk fibroin comprises the following steps:
[0094] The silk fibroin in the silk fibroin solution obtained after degumming, dissolving and dialyzing the mulberry silk was named "unaminated silk fibroin", and the mass fraction of the unaminated silk fibroin solution was determined by weight method.
[0095] A1: Dilute the unaminated silk fibroin solution to 3.0% by mass with purified water. Take 1000 mL of 3.0% unaminated silk fibroin solution, pre-cool it in an ice bath for 30 minutes, add MES powder to the solution to make the concentration of MES in the solution 5.0 mmol / L, stir to mix and dissolve MES.
[0096] A2: Add 50 g of spermine to the solution, slowly stir in an ice bath for 15 minutes, then add 40 g of NHS and 80 g of EDC respectively, maintain the ice bath, and slowly stir for 3 hours.
[0097] A3: The solution was quickly frozen in a low-temperature refrigerator at -80°C for 24 hours, and then thawed at +8°C to obtain a crude amino-modified silk fibroin solution.
[0098] A4: The crude product of the amino-modified silk fibroin solution was dialyzed with 1.0 mmol / L MES solution for 24 hours at +8°C, with the molecular weight cutoff of the dialysis membrane being 10 kDa, and then dialyzed with purified water for 72 hours. The solution obtained after dialysis was filtered with a 200-mesh filter, and the filtrate was freeze-dried to obtain an amino-modified silk fibroin solid, which was named S-4.
[0099] B1: Sodium hyaluronate solid with a molecular weight of 500 kDa is dissolved in purified water to obtain a sodium hyaluronate solution with a mass fraction of 5.0%.
[0100] B2: Dissolve the aminated silk fibroin solid in purified water to obtain an aminated silk fibroin solution having the same mass fraction of 5.0%.
[0101] B3: In an ice bath, 5.0 g of MES and 5.0 g of NHS powder were dissolved in 100 mL of 5.0% aminated silk fibroin solution, and then mixed with 900 mL of 5.0% sodium hyaluronate solution to obtain a sodium hyaluronate / aminated silk fibroin mixed solution. The mixed solution was stirred for 30 minutes to obtain a sodium hyaluronate network precursor.
[0102] C1: Dissolve the aminated silk fibroin solid in purified water to obtain an aminated silk fibroin solution with a mass fraction of 5.0%.
[0103] C2: In an ice bath, an aminated silk fibroin solution with a mass fraction of 5.0% was mixed with an unaminated silk fibroin solution with the same mass fraction in a volume ratio of 30:70. After adding EDC, MES and NHS powders accounting for 20%, 10% and 10% of the total mass of the silk fibroin in the solution, the mixture was slowly stirred for 3 hours to obtain a silk fibroin network prepolymer.
[0104] D1: Mix the sodium hyaluronate network precursor and the silk fibroin network prepolymer in a mass ratio of 90:10 and react in an ice bath for 3 hours.
[0105] D2: The block gel was crushed and granulated, and after screening, gel particles with an average particle size of 598 μm were obtained.
[0106] D3: The gel particles were placed in a stainless steel mesh basket, placed in pure water or water for injection for oscillation and cleaning for 1 day, and then placed in physiological saline for cleaning and balancing for 1 day to obtain double-network sodium hyaluronate / silk fibroin gel particles bridged by amino-modified silk fibroin. The mass ratio of sodium hyaluronate to the total amount of silk fibroin in the gel was 81:19.
[0107] Comparative Example 1
[0108] Preparation of silk fibroin / sodium hyaluronate mixed network gel (control gel): MES was dissolved in a 0.1% by mass unaminated silk fibroin solution to a concentration of 50 mmol / L, and then NHS and EDC solutions were added dropwise to the solution to make the concentrations of NHS and EDC in the solution 1.0% and 2.0%, respectively, to obtain component A.
[0109] Sodium hyaluronate solid with a molecular weight of 1500 kDa was dissolved in 50 mmol / L MES solution, and slowly stirred while dissolving to make the mass fraction of sodium hyaluronate in the solution be 1.0%. NHS and EDC solutions were then added dropwise to the solution to make the concentrations of NHS and EDC in the solution be 0.1% and 0.2%, respectively, to obtain component B.
[0110] 52 mL of component A and 96 mL of component B were mixed and reacted for 24 hours. The resulting block gel was crushed and granulated, and after screening, gel particles with an average particle size of 546 μm were obtained. The gel particles were placed in a stainless steel basket, placed in pure water or water for injection for 1 day for oscillation and washing, and then placed in physiological saline for 1 day for washing and balancing to obtain silk fibroin / sodium hyaluronate mixed network gel particles 1 (control sample gel 1). The mass proportion of silk fibroin in the gel is about 52%, which is the same as the total mass proportion of silk fibroin in the gel of Example 1.
[0111] Comparative Example 2
[0112] The only difference from Example 1 is that the rapid freezing-low temperature reconstitution process is not used, that is, step A3 is omitted.
[0113] The surface Zeta potential of the unaminated silk fibroin and the aminated silk fibroin of Examples 1-4 was determined using a particle size potential analyzer. The free primary amino content in the unaminated silk fibroin and the aminated silk fibroin of Examples 1-4 was determined using the ninhydrin colorimetric method and glycine solution as the standard solution. The results are shown in Table 1.
[0114] Table 1 Physical and chemical properties of amino-modified silk fibroin
[0115]
[0116] As can be seen from Table 1, compared with the unaminated silk fibroin, the surface charge of the aminated silk fibroin is reversed to positive, the Zeta potential is significantly increased, and the content of free primary amino groups is significantly increased; compared with the aminated silk fibroin, the Zeta potential prepared under the conditions of Comparative Example 2 is reduced, indicating stronger particle instability, while the free primary amino groups are reduced, indicating a decrease in amination efficiency.
[0117] The gels of Examples 1-4 and Comparative Examples 1-2 were tested for dissolution rate and biodegradability. The specific testing methods are as follows:
[0118] Gel dissolution test: Take about 1.0 g of freeze-dried double-network sodium hyaluronate / silk fibroin gel particles bridged by amino-silk fibroin and accurately weigh their mass M0 (g). Put the gel particles into a nylon mesh bag, immerse them in 100 mL of physiological saline (PBS), and treat them at 37°C for 24 hours. Filter, freeze-dry the remaining gel, weigh its mass M1 (g), and calculate the gel dissolution rate (%) in PBS according to formula (1). This dissolution rate represents the ability of the gel to resist water dissolution and is used to evaluate the effective cross-linking degree of sodium hyaluronate and silk fibroin in the gel.
[0119]
[0120] Gel biodegradation test: Prepare a PBS mixed solution containing 10.0 U / mL hyaluronidase IS and 2.0 U / mL collagenase IA as a simulated body fluid for in vitro biodegradation of the gel. Take about 1.0 g of freeze-dried double-network sodium hyaluronate / silk fibroin gel particles bridged by amino-silk fibroin and accurately weigh their mass MM0 (g). After the gel particles are placed in a nylon mesh bag, they are immersed in 100 mL of simulated body fluid and treated with constant temperature oscillation at 37°C for 7 days, and replaced with fresh simulated body fluid every 48 hours. After the degradation is completed, the remaining gel is freeze-dried and its residual mass MM1 (g) is weighed. The biodegradation rate (%) of the gel in the simulated body fluid is calculated according to formula (2). The biodegradation rate is used to evaluate the performance of the gel in resisting biodegradation.
[0121]
[0122] Table 2 Test results of gel dissolution rate and biodegradation rate in Examples 1-4 and Comparative Examples 1-2
[0123]
[0124] As can be seen from Table 2, the dissolution loss rates of the double-network sodium hyaluronate / silk fibroin gel bridged by amino-treated silk fibroin in Examples 1-4 are all less than 2%, indicating that the sodium hyaluronate and silk fibroin in the gel have been effectively cross-linked; the dissolution loss rate of Comparative Example 1 is as high as 56.9%, indicating that the gel cross-linking is weak and the internal tissue structure is loose; and compared with Example 1, the cross-linking effect of sodium hyaluronate and silk fibroin in the gel of Comparative Example 2 is reduced.
[0125] The biodegradation rates of the double-network sodium hyaluronate / silk fibroin gel bridged by amino-silk fibroin in Examples 1-4 are all less than 30%. After 7 days of degradation in simulated body fluid, the gel can maintain its original shape and does not collapse; the biodegradation rate in Comparative Example 1 is high, indicating that the gel has been mostly degraded; the biodegradation rate in Comparative Example 2 is 34.5±0.3%, indicating that it has a certain ability to resist simulated body fluids, and the gel can maintain a certain original shape, but compared with Example 1, the biodegradation rate of Comparative Example 2 is improved, indicating that the amino-silk fibroin prepared by the rapid freezing-low-temperature re-dissolution process is beneficial to improving the anti-degradation ability of the gel.
[0126] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a double-network sodium hyaluronate / silk fibroin gel bridged by amino-modified silk fibroin, comprising: degumming, dissolving, and dialyzing mulberry silk to obtain a silk fibroin solution, and diluting the silk fibroin solution with purified water to obtain a silk fibroin aqueous solution, characterized in that : The silk fibroin aqueous solution is an unaminated silk fibroin aqueous solution, and then the following steps are performed: P1: MES, spermine, NHS and EDC were added to the unaminated silk fibroin aqueous solution in sequence, and after stirring, the mixture was subjected to rapid freezing-low temperature thawing, low temperature dialysis-freeze drying in sequence, and the aminated silk fibroin solid was obtained by post-treatment; P2: Mixing sodium hyaluronate aqueous solution, MES, NHS and amino-modified silk fibroin to obtain a sodium hyaluronate network precursor with amino-modified silk fibroin as a bridging molecule; P3: Mix the unaminated silk fibroin aqueous solution, MES, NHS, EDC and the aminated silk fibroin to obtain a silk fibroin network prepolymer with the aminated silk fibroin as a bridging molecule; P4: mixing and reacting the sodium hyaluronate network precursor and the silk fibroin network prepolymer to obtain a block gel, and then granulating, washing, and balancing to obtain double-network sodium hyaluronate / silk fibroin gel particles bridged by amino-modified silk fibroin; The step P1 is specifically as follows: A1: Prepare an aqueous solution of unaminated silk fibroin with a mass fraction of 0.1-3% at a temperature of +0-6 °C; add MES to the aqueous solution of unaminated silk fibroin and stir to make the concentration of MES in the solution 3.0-8.0 mmol / L; A2: Then add spermine to the solution of step A1, slowly stir in an ice bath for 15-30 minutes, then add NHS and EDC, maintain an ice bath, slowly stir for 3-5 hours, and make the mass fractions of spermine, NHS and EDC in the solution be 0.5~5.0%, 0.1~4.0%, 0.2~8.0%, respectively; A3: The solution of step A2 is placed in a low-temperature refrigerator at a temperature of -20 ~ -80 ° C and quickly frozen for 24 hours, and then thawed at +2 ~ +8 ° C to obtain a crude amino-based silk fibroin solution; A4: The crude product of the amino-modified silk fibroin solution is first dialyzed with 1.0 mmol / L MES solution for 24 hours in a +2~+8°C environment, and the molecular weight cutoff of the dialysis membrane is 5-10 kDa, and then dialyzed with purified water for 72 hours. The solution obtained after dialysis is filtered with a filter, and the filtrate is freeze-dried to obtain an amino-modified silk fibroin solid.
2. The method for preparing the aminated silk fibroin bridged double network sodium hyaluronate / silk fibroin gel according to claim 1, characterized in that : The step P2 is as follows: B1: Dissolve sodium hyaluronate solid in purified water or water for injection to obtain a 1.0-5.0% sodium hyaluronate solution; B2: dissolving the amino-modified silk fibroin solid in purified water or water for injection to obtain an amino-modified silk fibroin solution; B3: Under ice bath conditions, MES and NHS are dissolved in the aminated silk fibroin solution, and then mixed with the sodium hyaluronate solution to obtain a sodium hyaluronate / aminated silk fibroin mixed solution, and the mixed solution is stirred to obtain a sodium hyaluronate network precursor.
3. The method for preparing the aminated silk fibroin bridged double network sodium hyaluronate / silk fibroin gel according to claim 1, characterized in that : The step P3 is as follows: C1: Dissolve the aminated silk fibroin solid in purified water to obtain a 1.0~5.0% aminated silk fibroin solution; C2: The aminated silk fibroin solution is mixed with the unaminated silk fibroin solution, and MES, NHS and EDC are added to obtain a silk fibroin network prepolymer.
4. The method for preparing the aminated silk fibroin bridged double network sodium hyaluronate / silk fibroin gel according to claim 1, characterized in that : The step P4 is as follows: D1: Mix the sodium hyaluronate network precursor and the silk fibroin network prepolymer and react in an ice bath for 3-5 hours; D2: The reactants in step D1 are placed in a low-temperature refrigerator at a temperature of -20~-80 ° C and quickly frozen for 12-24 hours, and then thawed at room temperature to obtain a block gel; D3: The block gel is crushed and granulated, and after screening, gel particles with a particle size of 100~1000μm are obtained; D4: The gel particles are placed in a stainless steel mesh basket, placed in pure water or water for injection for oscillation and cleaning for 1-2 days, and then placed in physiological saline for cleaning and balancing for 1-3 days to obtain double-network sodium hyaluronate / silk protein gel particles bridged by amino-modified silk protein.
5. The method for preparing the aminated silk fibroin bridged double network sodium hyaluronate / silk fibroin gel according to claim 2, characterized in that : The mass fraction of the sodium hyaluronate solution in step B1 is 1.0~5.0%, and the molecular weight of the sodium hyaluronate is 500~3000kDa; the mass fraction of the aminated silk fibroin solution in step B2 is 1.0~5.0%; the volume ratio of the sodium hyaluronate solution to the aminated silk fibroin solution in step B3 is 70:30~90:10, and the added amounts of MES and NHS powders are both 10%~20% of the sum of the masses of sodium hyaluronate and aminated silk fibroin in the mixed solution.
6. The method for preparing the aminated silk fibroin bridged double network sodium hyaluronate / silk fibroin gel according to claim 3, characterized in that : In step C2, the mass fractions of the aminated silk fibroin solution and the unaminated silk fibroin solution are both 1.0-5.0%, and the volume ratio of the aminated silk fibroin solution to the unaminated silk fibroin solution is 10:90-30:70; in step C2, the amounts of MES, NHS and EDC added are 5-15%, 5-15% and 15-25% of the total amount of silk fibroin, respectively.
7. The method for preparing the aminated silk fibroin bridged double network sodium hyaluronate / silk fibroin gel according to claim 4, characterized in that :The mass ratio of the sodium hyaluronate network precursor to the silk fibroin network prepolymer in step D1 is 10:90~80:
20.
8. A double network sodium hyaluronate / silk fibroin gel bridged by amino-modified silk fibroin, characterized in that : The aminated silk fibroin bridged double network sodium hyaluronate / silk fibroin gel is prepared according to the preparation method of the aminated silk fibroin bridged double network sodium hyaluronate / silk fibroin gel according to any one of claims 1-7, and the gel is composed of a sodium hyaluronate network bridged by aminated silk fibroin and a silk fibroin network bridged by aminated silk fibroin, and the sodium hyaluronate network and the silk fibroin network are also bridged by aminated silk fibroin.