A nylon composite material with high thermal conductivity and preparation method thereof

By surface treatment of titanium dioxide and combining it with nylon 66 resin, the problem of insufficient thermal conductivity of polymer-based dielectric composite materials is solved, the thermal conductivity and dielectric properties of the material are improved, and it is suitable for communication equipment in high-frequency electric field environments.

CN118085561BActive Publication Date: 2024-11-22安特普工程塑料(苏州)有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410524012.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-29
Publication Date
2024-11-22
Estimated Expiration
2044-04-29

AI Technical Summary

Technical Problem

The existing polymer-based dielectric composite materials lack thermal conductivity under high-frequency electric fields, resulting in heat accumulation, affecting equipment reliability, and poor compatibility of ceramic fillers lead to degradation of mechanical properties.

Method used

By surface treatment of titanium dioxide, modified titanium dioxide and glass fiber combined with nylon 66 resin, the thermal conductivity and dielectric properties of the material are improved, and a highly thermal conductivity nylon composite material is prepared by injection molding.

Benefits of technology

It realizes a nylon composite material that maintains a high dielectric constant and low dielectric loss at high frequencies, improves the thermal conductivity and mechanical properties of the material, and is suitable for applications in the communication field.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of compositions of polymer compounds, and discloses a nylon composite material with high thermal conductivity and a preparation method thereof. The nylon composite material with high thermal conductivity comprises the following components in parts by weight: 30 to 60 parts of nylon 66, 5 to 15 parts of glass fiber, 30 to 60 parts of modified titanium dioxide, and 0.5 to 2 parts of an auxiliary agent. In the present invention, the nylon composite material with high thermal conductivity prepared by adding modified titanium dioxide to nylon 66 has good thermal conductivity, and can still maintain a high dielectric constant and low dielectric loss at high frequencies, which is very important for the application of the material in the field of communications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer compound compositions, and in particular to a nylon composite material with high thermal conductivity and a preparation method thereof. Background Art

[0002] As a popular material in the field of electrical and electronic, polymer-based dielectric composites are widely used in microelectronic systems, high-temperature electronic devices and energy storage equipment due to their low price, good processing performance and arbitrary shape design and control. With the development of science and technology and manufacturing, polymer-based dielectric composites have more and more application space, but they are also facing more and more challenges, such as in the fields of aerospace, new energy vehicles and integrated circuits. In the study of high-frequency electric fields, high dielectric constant materials are obtained and their thermal conductivity is studied at the same time. Due to the existence of dielectric loss, heat will be generated under the electric field. If the heat cannot be effectively discharged, it will cause heat accumulation and temperature rise during long-term use. Therefore, starting from the material itself, understanding and improving the thermal conductivity of the material will help reduce the problem of heat accumulation. Nylon is non-toxic, light, has excellent mechanical strength, wear resistance and good corrosion resistance, and is suitable for high-temperature electronic devices and energy storage systems. However, due to the high thermal impedance of the polymer itself, it is difficult to discharge the heat accumulated inside the material when working under high temperature conditions for a long time, which will affect the reliability of the equipment. At present, researchers mainly enhance the thermal conductivity of polymers by adding thermally conductive fillers, mainly metal particles and ceramic particles. Due to the requirements of the insulation performance of materials in the field of electronics and electrical appliances, ceramic particles have become the main choice. In chip packaging, solar panel module packaging and flexible wearable devices, materials are required to have a higher dielectric constant, so ceramic fillers are often added to enhance the dielectric properties of polymer-based composites.

[0003] The simplest and most effective strategy is to prepare polymer composites by adding thermally conductive fillers to polymers to improve their thermal conductivity. After adding uniformly distributed fillers to the polymer, when heat is transferred in the polymer composite, phonons are transferred along the polymer-filler-polymer path. When the filler filling amount reaches a certain value, the fillers can contact each other, and the thermal conductivity of the composite material will increase more rapidly, but this often requires a higher filler filling amount and brings problems such as increased processing difficulty and increased viscosity. In addition, the properties of the interface between the polymer and the filler are often quite different. The introduction of too much filler will lead to the generation of additional pores, aggravating the scattering of phonons, resulting in a decrease in thermal conductivity and a decrease in the mechanical properties of the composite material.

[0004] Chinese patent 201210273668.4 discloses a high thermal conductivity and insulating polyamide 66 composition that can be directly laser-formed for LED light source substrates and a preparation method thereof, which has the advantages of high thermal conductivity, direct laser forming, excellent insulation, resistance to chemicals and corrosion, etc. The composition of the invention is prepared from the following raw materials in parts by weight: 40-70 parts of polyamide 66, 5-35 parts of thermal conductor, 5-8 parts of inorganic pigment, 0.15 parts of antioxidant A, 0.15 parts of antioxidant B, 0.5 parts of lubricant, and 0.3 parts of coupling agent. The polyamide 66 composition provided by the invention has the advantages of light weight, easy forming, flexible circuit design, simple process, etc., and has excellent high-temperature electrical insulation.

[0005] Chinese patent 201711021284.2 discloses a low-frequency and low-dielectric-loss AgNb co-doped titanium dioxide-based dielectric ceramic material and a preparation method thereof. The general formula of the ceramic material is (Ag 1 / 4 Nb 3 / 4 ) x Ti1-xO2, where x represents the molar fraction, and the value of x is 0.005~0.01. The preparation method of the ceramic material of the invention is simple, repeatable and has a high yield. By introducing the metal element Ag into the Nb-doped titanium dioxide-based ceramic material, the ceramic material can be made to have a high yield at a frequency of 40~10 6 High dielectric constant (>10 4 ), low dielectric loss (<0.09), especially significantly reducing the low-frequency dielectric loss of ceramic materials, in the range of 40~10 3 The dielectric loss in the Hz frequency range is always kept below 0.06, and it has excellent frequency and temperature stability, maintained between -10% and 10%, which meets the parameter requirements of ceramic capacitors and has great application value.

[0006] In the prior art, ceramic fillers are often filled into polymers by direct blending. However, ceramic fillers have poor compatibility and dispersibility in polymer systems due to their strong hydrophilicity, which not only affects the mechanical properties of the polymer but also the thermal conductivity and dielectric properties. Therefore, new strategies are developed to enable polymer composites to achieve higher thermal conductivity at lower filling amounts and meet various requirements according to actual application needs, such as mechanical properties, electrical insulation properties, dielectric properties, etc. Summary of the invention

[0007] In view of the above-mentioned defects in the prior art, the technical problem to be solved by the present invention is to provide a nylon composite material with high thermal conductivity and a preparation method thereof.

[0008] Conventional measurements of dielectric constants are mainly concentrated in the low-frequency field and rarely pay attention to the thermal conductivity of materials. The existence of dielectric loss leads to heat conversion during use. When dielectric loss cannot be reduced, good thermal conductivity can cause overheating of the product during use, and even affect the normal use and good experience of the entire product, such as the stability of communication signals (temperature will affect the change of dielectric constant). With the development of the communication field and technological advancement, the stability of high-frequency electric fields and signal transmission is crucial. Therefore, it is very necessary to study the thermal conductivity of high dielectric constant materials. Titanium dioxide is often used as a filler added to polymers to improve performance due to its good thermal conductivity and good dielectric properties. However, titanium dioxide itself has poor compatibility in polymers and poor dispersibility, which makes it easy to agglomerate and affects the mechanical properties of the polymer. Glycidyl methacrylate is an ester compound with a molecular formula of C7H 10 O3, also known as 2,3-epoxypropyl methacrylate, abbreviated as GMA. It is a colorless and transparent liquid. It is insoluble in water and soluble in most common organic solvents. Because its molecules contain two functional groups, active vinyl and epoxy with ionic reaction, it can be polymerized in the form of functional groups and ionic reactions. It can not only modify polymers, but also perform surface treatment on some fillers to enhance the bonding effect with resins, such as calcium carbonate, talcum powder, ceramic powder, etc. The surface treatment of titanium dioxide is to enhance and improve its surface bonding effect with nylon 66 resin; the use of additives helps to disperse the powder and the bonding effect between glass fiber and resin, and improve the strength of the material. The surface treatment of titanium dioxide helps to improve the surface bonding effect, dispersion effect, and material strength.

[0009] The technical solution of the present invention:

[0010] A nylon composite material with high thermal conductivity comprises the following components in parts by weight: 30-60 parts of nylon 66, 5-15 parts of glass fiber, 30-60 parts of modified titanium dioxide, and 0.5-2 parts of an auxiliary agent.

[0011] Furthermore, the auxiliary agent is a mixture of one or more of ethylene bisstearamide and zinc stearate.

[0012] The preparation method of the modified titanium dioxide comprises the following steps:

[0013] Add titanium dioxide to a mixing tank, and then use a sprayer to spray glyceryl methacrylate diluted with acetone into the tank, mix in batches, and stir evenly in a closed environment for 30 to 60 seconds each time until the addition is completed. Transfer the mixture to a tray and let it stand for 1 hour, then dry and cool.

[0014] Furthermore, the amount of the glycerol methacrylate is 0.5-2wt% of the titanium dioxide.

[0015] Furthermore, the volume of the acetone is 100 to 200 times that of glyceryl methacrylate.

[0016] Preferably, the preparation method of the modified titanium dioxide comprises the following steps:

[0017] Add titanium dioxide into a mixing tank, and then use a sprayer to spray glyceryl methacrylate diluted with acetone into the tank. The amount of glyceryl methacrylate is 0.5-2wt% of titanium dioxide, and the volume of acetone is 100-200 times that of glyceryl methacrylate. Mix in batches and stir evenly in a closed environment. Stir for 30-60s each time until the addition is completed. Transfer the mixture to a tray and let it stand for 1h, then dry and cool.

[0018] More preferably, the method for preparing the modified titanium dioxide comprises the following steps:

[0019] X1: Disperse titanium dioxide in dichloromethane, add acetylacetone as a dispersant, then add terephthaloyl chloride and triethylamine, heat to 35-45°C and stir for 20-40 hours. After the reaction is completed, cool to room temperature, filter, wash the residue with dichloromethane and dry under reduced pressure to obtain grafted titanium dioxide;

[0020] X2: Disperse the grafted titanium dioxide in step X1 in dichloromethane, add acetylacetone as a dispersant, then add stearyl alcohol and triethylamine, stir for 4-6 hours after the addition is completed, filter after the reaction is completed, wash the residue with water, acid, alkali and then with dichloromethane, dry the organic phase and concentrate under reduced pressure to obtain modified titanium dioxide.

[0021] A method for preparing a nylon composite material with high thermal conductivity comprises the following steps:

[0022] S1 premixes nylon 66, modified titanium dioxide and additives according to the formula, adds them into the main hopper, then adds glass fiber, and extrude and granulate;

[0023] S2: drying the material obtained in step S1 for 2-6 hours, injecting it into a mold, and performing injection molding. After the injection molding is completed, a nylon composite material is obtained.

[0024] Furthermore, the drying temperature in step S2 is 70-90°C.

[0025] Furthermore, the injection molding pressure in step S2 is 69-124 MPa.

[0026] Furthermore, the injection molding temperature in step S2 is 270-300°C.

[0027] Furthermore, in step S2, the mold temperature is 66-110°C.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The high thermal conductivity nylon composite material prepared by adding modified titanium dioxide to nylon 66 has good thermal conductivity and can still maintain a high dielectric constant and low dielectric loss at high frequencies, which is very important for the application of the material in the communication field. DETAILED DESCRIPTION

[0030] The technical solutions of the present invention are described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.

[0031] The parameters of some raw materials in the embodiments of the present invention are as follows:

[0032] Nylon is a large family. The most commonly used ones are nylon 66, nylon 6, etc.; long-chain nylon: nylon 11, nylon 12, nylon 610, nylon 612, nylon 1010, etc.; high-temperature nylon: nylon 46, nylon 4T, nylon 6T, nylon 9T, nylon 10T, etc. The specific values ​​of the dielectric constants of different nylons are also different, usually ranging from 3 to 5. This patent selects nylon 66, nylon 66 melting point: 262°C, density: 1.13-1.14g / cm 3 , the thermal conductivity of nylon 66 is: 0.25W / mK.

[0033] The glass fibers used for reinforcement are mainly divided into chopped glass fibers and continuous glass fibers in terms of shape; from the perspective of surface treatment, there are special glass fibers based on different resins, such as glass fibers for nylon, glass fibers for polyoxymethylene, glass fibers for polyester, etc. The difference lies in the use of targeted glass fibers, which can obtain better mechanical properties; the diameter range of glass fibers used for plastic reinforcement is usually 10~20μm. Therefore, the choice of glass fiber is nylon-specific glass fiber, chopped glass fibers with a diameter of 10~20μm and a length of 4~5mm. As an engineering plastic, the main purpose of adding glass fiber is to improve the strength of the material. Density of glass fiber: 2.54g / cm 3 .

[0034] Titanium dioxide, density: 4.0g / cm 3 .

[0035] Comparative Example 1

[0036] A method for preparing a nylon composite material with high thermal conductivity comprises the following steps:

[0037] S1: premix 4.9 kg of nylon 66, 4 kg of titanium dioxide, 50 g of ethylene bisstearamide and 50 g of zinc stearate, add them into the main hopper, then add 1 kg of glass fiber and extrude them into granules;

[0038] S2: drying the material obtained in step S1 at 80°C for 4h, injecting it into a mold, and performing injection molding at 84MPa, an injection molding temperature of 280°C, and a mold temperature of 80°C. After the injection molding is completed, a nylon composite material is obtained.

[0039] Comparative Example 2

[0040] A method for preparing a nylon composite material with high thermal conductivity comprises the following steps:

[0041] S1: premix 3.9 kg of nylon 66, 5 kg of titanium dioxide, 50 g of ethylene bisstearamide and 50 g of zinc stearate, add the mixture into the main hopper, then add 1 kg of glass fiber and extrude into granules;

[0042] S2: drying the material obtained in step S1 at 80°C for 4h, injecting it into a mold, and performing injection molding at 84MPa, an injection molding temperature of 280°C, and a mold temperature of 80°C. After the injection molding is completed, a nylon composite material is obtained.

[0043] Comparative Example 3

[0044] A method for preparing a nylon composite material with high thermal conductivity comprises the following steps:

[0045] S1: premix 2.9 kg of nylon 66, 6 kg of titanium dioxide, 50 g of ethylene bisstearamide and 50 g of zinc stearate, add them into the main hopper, then add 1 kg of glass fiber and extrude them into granules;

[0046] S2: drying the material obtained in step S1 at 80°C for 4h, injecting it into a mold, and performing injection molding at 84MPa, an injection molding temperature of 280°C, and a mold temperature of 80°C. After the injection molding is completed, a nylon composite material is obtained.

[0047] Example 1

[0048] A method for preparing a nylon composite material with high thermal conductivity comprises the following steps:

[0049] S1: premix 4.9 kg of nylon 66, 4 kg of modified titanium dioxide, 50 g of ethylene bisstearamide and 50 g of zinc stearate, add them into the main hopper, then add 1 kg of glass fiber and extrude them into granules;

[0050] S2: drying the material obtained in step S1 at 80°C for 4h, injecting it into a mold, and performing injection molding at 84MPa, an injection molding temperature of 280°C, and a mold temperature of 80°C. After the injection molding is completed, a nylon composite material is obtained.

[0051] The preparation method of the modified titanium dioxide comprises the following steps:

[0052] Add titanium dioxide into a mixing tank, and then use a sprayer to spray glyceryl methacrylate diluted with acetone into the tank. The amount of glyceryl methacrylate is 1wt% of titanium dioxide, and the volume of acetone is 150 times that of glyceryl methacrylate. Mix in batches and stir evenly in a closed environment for 45 seconds each time until the addition is completed. Transfer the mixture to a tray and let it stand for 1 hour, then dry and cool.

[0053] Example 2

[0054] A method for preparing a nylon composite material with high thermal conductivity comprises the following steps:

[0055] S1: premix 3.9 kg of nylon 66, 5 kg of modified titanium dioxide, 50 g of ethylene bisstearamide and 50 g of zinc stearate, add them into the main hopper, then add 1 kg of glass fiber and extrude them into granules;

[0056] S2: drying the material obtained in step S1 at 80°C for 4h, injecting it into a mold, and performing injection molding at 84MPa, an injection molding temperature of 280°C, and a mold temperature of 80°C. After the injection molding is completed, a nylon composite material is obtained.

[0057] The preparation method of the modified titanium dioxide comprises the following steps:

[0058] Add titanium dioxide into a mixing tank, and then use a sprayer to spray glyceryl methacrylate diluted with acetone into the tank. The amount of glyceryl methacrylate is 1wt% of titanium dioxide, and the volume of acetone is 150 times that of glyceryl methacrylate. Mix in batches and stir evenly in a closed environment for 45 seconds each time until the addition is completed. Transfer the mixture to a tray and let it stand for 1 hour, then dry and cool.

[0059] Example 3

[0060] A method for preparing a nylon composite material with high thermal conductivity comprises the following steps:

[0061] S1: premix 2.9 kg of nylon 66, 6 kg of modified titanium dioxide, 50 g of ethylene bisstearamide and 50 g of zinc stearate, add them into the main hopper, then add 1 kg of glass fiber and extrude them into granules;

[0062] S2: drying the material obtained in step S1 at 80°C for 4h, injecting it into a mold, and performing injection molding at 84MPa, an injection molding temperature of 280°C, and a mold temperature of 80°C. After the injection molding is completed, a nylon composite material is obtained.

[0063] The preparation method of the modified titanium dioxide comprises the following steps:

[0064] Add titanium dioxide into a mixing tank, and then use a sprayer to spray glyceryl methacrylate diluted with acetone into the tank. The amount of glyceryl methacrylate is 1wt% of titanium dioxide, and the volume of acetone is 150 times that of glyceryl methacrylate. Mix in batches and stir evenly in a closed environment for 45 seconds each time until the addition is completed. Transfer the mixture to a tray and let it stand for 1 hour, then dry and cool.

[0065] Example 4

[0066] A method for preparing a nylon composite material with high thermal conductivity comprises the following steps:

[0067] S1: premix 2.9 kg of nylon 66, 6 kg of modified titanium dioxide, 50 g of ethylene bisstearamide and 50 g of zinc stearate, add them into the main hopper, then add 1 kg of glass fiber and extrude them into granules;

[0068] S2: drying the material obtained in step S1 at 80°C for 4h, injecting it into a mold, and performing injection molding at 84MPa, an injection molding temperature of 280°C, and a mold temperature of 80°C. After the injection molding is completed, a nylon composite material is obtained.

[0069] The preparation method of the modified titanium dioxide comprises the following steps:

[0070] X1 weighed 2 kg of titanium dioxide and dispersed it in 50 L of dichloromethane, added 500 mL of acetylacetone as a dispersant, then added 2.4 kg of terephthaloyl chloride and 1 L of triethylamine, heated to 37 ° C and stirred for 28 hours. After the reaction was completed, it was cooled to room temperature and filtered. The residue was washed with dichloromethane and dried under reduced pressure at 35 ° C and -0.9 MPa to obtain grafted titanium dioxide;

[0071] X2 weighs 2.8 kg of the grafted titanium dioxide in step X1 and disperses it in 56 L of dichloromethane, adds 560 mL of acetylacetone as a dispersant, then adds 2.7 kg of stearyl alcohol and 1 L of triethylamine, and stirs for 6 hours after the addition is completed. After the reaction is completed, filter, wash the residue with water, acid, alkali, and then wash with dichloromethane. After the organic phase is dried, concentrate under reduced pressure at 35°C and -0.9 MPa to obtain modified titanium dioxide.

[0072] Test Example 1

[0073] The dielectric properties, thermal conductivity and mechanical properties of the nylon composite materials prepared in the control example and the embodiment were tested. The test method of dielectric properties refers to ASTM D150-2022 "Standard Test Method for AC Loss Characteristics and Dielectric Constant (Dielectric Constant) of Solid Electrical Insulation", the test method of thermal conductivity refers to ASTM E1461-13 (2022) "Standard Test Method for Determination of Thermal Diffusivity by Flash Method", the test method of tensile strength refers to ASTM D638-2022 "Standard Test Method for Tensile Properties of Plastics", the test method of flexural strength and flexural modulus refers to ASTM D790-2017 "Standard Test Method for Flexural Properties of Unreinforced and Reinforced Plastics and Electrical Insulating Materials", the test method of notched impact strength refers to ASTM D256-2010 (R2018) Standard Test Method for Determining the Pendulum Impact Performance of Plastics, and the test method of unnotched impact strength refers to ASTMD4812-19e1 "Standard Test Method for Impact Resistance of Unnotched Izod Beams of Plastics", and the specific test results are shown in Table 1.

[0074] Table 1 Test results of dielectric properties, thermal conductivity and mechanical properties of nylon composite materials

[0075] Test items Comparative Example 1 Comparative Example 2 Comparative Example 3 Example 1 Example 2 Example 3 Example 4 Tensile strength(MPa) 78 58 61 68 60 54 63 Bending strength(MPa) 131 102 100 124 110 95 106 Flexural modulus (MPa) 5857 5374 6101 5719 6408 7992 8024 Izod notched impact strength (j / m) 34 31 47 30 35 37 36 Izod unnotched impact strength (j / m) 249 190 240 304 314 234 303 <![CDATA[Dielectric constant D k (2.0 GHz)]]> 4.554 6.149 7.689 5.123 6.228 7.943 7.945 <![CDATA[Dielectric constant D k (10.1 GHz)]]> 4.522 6.101 7.650 5.082 6.209 7.976 7.969 <![CDATA[Dielectric constant D k (18.3 GHz)]]> 4.524 6.108 7.635 5.081 6.214 7.999 7.981 <![CDATA[Dielectric loss D k (2.0 GHz)]]> <![CDATA[1.45×10- 2 ]]> <![CDATA[1.66×10- 2 ]]> <![CDATA[1.93×10- 2 ]]> <![CDATA[1.41×10- 2 ]]> <![CDATA[1.23×10- 2 ]]> <![CDATA[1.05×10- 2 ]]> <![CDATA[1.03×10- 2 ]]> <![CDATA[Dielectric loss D k (10.1 GHz)]]> <![CDATA[1.23×10- 2 ]]> <![CDATA[1.36×10- 2 ]]> <![CDATA[1.72×10- 2 ]]> <![CDATA[1.22×10- 2 ]]> <![CDATA[1.12×10- 2 ]]> <![CDATA[1.35×10- 2 ]]> <![CDATA[1.36×10- 2 ]]> <![CDATA[Dielectric loss D k (18.3 GHz)]]> <![CDATA[1.46×10- 2 ]]> <![CDATA[2.14×10- 2 ]]> <![CDATA[2.25×10- 2 ]]> <![CDATA[1.51×10- 2 ]]> <![CDATA[1.77×10- 2 ]]> <![CDATA[1.13×10- 2 ]]> <![CDATA[1.11×10- 2 ]]> Thermal conductivity (flow) (W / mK) 0.574 0.675 0.828 0.637 0.757 0.959 0.951 Thermal conductivity (vertical) (W / mK) 0.596 0.707 0.848 0.613 0.723 0.903 0.901

[0076] Different dielectric constants and dielectric loss values ​​are obtained by adjusting the proportion of titanium dioxide. Taking 2.0GHz, 10.1GHz, and 18.3GHz as examples, in Reference Examples 1 to 3, at the same frequency, as the proportion of titanium dioxide increases, the dielectric constant value is also increasing, while in Examples 1 to 3, at the same frequency, as the proportion of modified titanium dioxide increases, the dielectric constant value is also increasing. The law of thermal conductivity is that it increases with the increase of the proportion of titanium dioxide. From the contribution to the dielectric constant value and thermal conductivity, the test data show that modified titanium dioxide is better than titanium dioxide.

[0077] In summary, the comparison shows that the dielectric constant, dielectric loss and thermal conductivity of titanium dioxide after surface treatment have all been improved. According to the test data, the dielectric constant increases, the dielectric loss decreases, and the thermal conductivity is also improved. The material has a certain thermal conductivity, which is conducive to the diffusion of heat generated by dielectric loss; at the same time, the dielectric constant value also increases with the addition of titanium dioxide, which has the function of improving thermal conductivity and dielectric constant, providing data support for product design.

[0078] It can be seen from the mechanical properties test that different titanium dioxide has a very obvious effect on the mechanical properties of nylon composite materials. When conventional titanium dioxide is used, the mechanical properties of nylon composite materials are significantly poor, so its tensile and bending resistance are not ideal. This is due to the poor dispersibility and poor compatibility of titanium dioxide itself in the polymer. When titanium dioxide is gathered in large quantities in the polymer, the flexibility of the material itself decreases. After titanium dioxide is modified, as in Examples 1 to 3, the improvement in its mechanical properties is not obvious, but Example 4 is better than Example 1 to 3. This may be because the modification of titanium dioxide in Example 4 is not only the grafting of long fatty chains, but also the introduction of rigid groups, so that the mechanical properties are further improved after it is blended with the polymer. It can be seen from the dielectric property test that when the amount of modified titanium dioxide increases, the dielectric constant and thermal conductivity are improved. The better the thermal conductivity, the better the diffusion of heat generated by dielectric loss. In Example 4, titanium dioxide is modified to introduce rigid groups and long fatty chains to improve its dispersibility and compatibility, and the entanglement of long fatty chains is not only not easy to agglomerate but also can improve its mechanical properties in the material. The nylon composite material prepared by adding modified titanium dioxide to nylon 66 not only has improved mechanical properties, but also has good thermal conductivity. It can still maintain a high dielectric constant and low dielectric loss at high frequencies, which is very important for the application of materials in the field of communications.

Claims

1. A nylon composite material with high thermal conductivity, characterized in that: It is composed of the following components in parts by weight: 2.9 parts of nylon 66, 1 part of glass fiber, 6 parts of modified titanium dioxide, and 0.1 part of additives; The preparation method of the modified titanium dioxide comprises the following steps: X1 weighed 2 kg of titanium dioxide and dispersed it in 50 L of dichloromethane, added 500 mL of acetylacetone as a dispersant, then added 2.4 kg of terephthaloyl chloride and 1 L of triethylamine, heated to 37 ° C and stirred for 28 hours. After the reaction was completed, it was cooled to room temperature and filtered. The residue was washed with dichloromethane and dried under reduced pressure at 35 ° C and -0.9 MPa to obtain grafted titanium dioxide; X2 weighed 2.8 kg of the grafted titanium dioxide in step X1 and dispersed it in 56 L of dichloromethane, added 560 mL of acetylacetone as a dispersant, and then added 2.7 kg of stearyl alcohol and 1 L of triethylamine. After the addition was completed, stirred for 6 hours. After the reaction was completed, filtered, the residue was washed with water, acid, alkali, and then washed with dichloromethane. After the organic phase was dried, it was concentrated under reduced pressure at 35°C and -0.9 MPa to obtain modified titanium dioxide; The auxiliary agent is ethylene bis stearamide and zinc stearate mixed in a mass ratio of 1:

1.

2. A method for preparing a nylon composite material with high thermal conductivity as claimed in claim 1, characterized in that: The steps include: S1 premixes nylon 66, modified titanium dioxide and additives according to the formula, adds them into the main hopper, then adds glass fiber, and extrude and granulate; S2: drying the material obtained in step S1 for 2-6 hours, injecting it into a mold, and performing injection molding. After the injection molding is completed, a nylon composite material is obtained.

3. The method for preparing a nylon composite material with high thermal conductivity as claimed in claim 2, characterized in that: The drying temperature in step S2 is 70-90°C.

4. The method for preparing a nylon composite material with high thermal conductivity as claimed in claim 2, characterized in that: The injection molding pressure in step S2 is 69-124 MPa.

5. The method for preparing a nylon composite material with high thermal conductivity as claimed in claim 2, characterized in that: The injection molding temperature in step S2 is 270-300°C.

6. The method for preparing a nylon composite material with high thermal conductivity as claimed in claim 2, characterized in that: In step S2, the mold temperature is 66-110°C.