A thermal barrier coating and its preparation method and bonding layer preparation process screening method
By screening the surface roughness index of the bonding layer, the suitable preparation process is selected, which improves the interface matching between the bonding layer of the thermal barrier coating and the ceramic thermal insulation layer, solves the problem of short service life of the thermal barrier coating, and realizes the Efficient preparation process screening and extend coating life.
Patent Information
- Application Number
- CN202410172143.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-02-07
AI Technical Summary
In the prior art, the service life of the thermal barrier coating is relatively short, and the screening of the bonding layer preparation process is time-consuming and laborious, and the cost is high.
By detecting the surface roughness index of the bonding layer, the bonding layer preparation process that meets specific conditions is selected, including the bonding layer with Ra in the range of 3 to 8 μm, Rsm is not less than 160 μm, and the smallest Rsk is used. Supersonic flame spraying process prepares MCrAlY-X metal bonding layer to improve the interface matching between the bonding layer and the ceramic heat insulation layer.
It effectively extends the life of the thermal barrier coating, shortens the screening time of the preparation process, saves labor and costs, and improves the efficiency of the thermal barrier coating bonding layer preparation process.
Smart Images

Figure CN118086813B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thermal barrier coatings, and in particular to a thermal barrier coating and a preparation method thereof, and a bonding layer preparation process screening method. Background Art
[0002] Aircraft engines and gas turbines are collectively referred to as gas turbine engines. Turbine blades are one of the components in gas turbine engines that bear the highest temperature and have the harshest service conditions, especially the high-pressure or first-stage turbine guide (stator) blades. Turbine guide blades usually adopt atmospheric plasma spray (APS) process to prepare thermal barrier coating (TBCs) ceramic insulation layer, and the bonding layer in the thermal barrier coating system substrate / bonding layer / ceramic insulation layer is mainly prepared by high-velocity oxygen-fuel (HVOF), atmospheric plasma spraying, vacuum plasma spraying (VPS), vacuum arc plating (ARC-PVD), electron beam physical vapor deposition (EB-PVD), etc. Among them, the low-cost process of MCrAlY-X metal bonding layer mainly adopts HVOF process, which has obvious advantages such as high coating density, low oxygen content, high preparation efficiency and low cost, and is widely used on the surface of aircraft engines and gas turbine guide blades.
[0003] The thermal barrier coating technology of HVOF-MCrAlY-X and APS-8YSZ composite is very mature and has been used as a classic thermal barrier coating on a large scale. Its bonding strength and service life are determined by materials and processes, and are intuitively fed back to the coating as coating microstructure control and interface control between the bonding layer and the ceramic layer. Padture et al. published a paper in an authoritative scientific journal (Nitin.P.Padture,etal.Thermal barrier coatings for gas turbine engine application,science,2002), and believed that the surface oxidation of the bonding layer produces a thermally grown oxide (Thermally GrownOxide, TGO) layer. On the undulating surface of the bonding layer, due to the TGO composition and undulating state, different stress states are generated in the convex and concave areas, resulting in cracking of the TGO or cracking of the ceramic layer near the TGO layer, resulting in failure of the thermal barrier coating. Therefore, in this field, controlling the surface state of the bonding layer has always been a core technical issue in the development and application of thermal barrier coatings.
[0004] In the prior art, when determining the preparation process of the bonding layer, the process parameters are usually adjusted, and different combinations of process parameters are used to prepare the bonding layer, and then the required ceramic thermal insulation layer is prepared. After the prepared thermal barrier coating is subjected to thermal cycle or thermal shock tests, the bonding layer preparation process used in large-scale production in engineering is determined, which is time-consuming, labor-intensive and costly. Summary of the invention
[0005] The first object of the present invention is to provide a method for screening the preparation process of a bonding layer of a thermal barrier coating, so as to solve the technical problems existing in the prior art that the life of the thermal barrier coating is relatively short and the screening of the preparation process of the bonding layer is time-consuming and labor-intensive.
[0006] The method for screening the preparation process of the bonding layer of the thermal barrier coating provided by the present invention comprises the following steps:
[0007] Adopting the preparation process to be screened to prepare the bonding layer, and testing the surface roughness indexes Ra, Rsm and Rsk, or Ra, Rz, Rsm and Rsk of each bonding layer;
[0008] According to the surface roughness index Ra or Ra and Rz of each bonding layer, the bonding layers whose Ra meets the condition or whose Ra and Rz meet the condition are screened out;
[0009] From the bonding layers whose Ra meets the conditions or whose Ra and Rz both meet the conditions, the bonding layers whose Rsm meets the first condition and whose Rsk meets the second condition are screened out, and the corresponding preparation process is used as the preparation process of the bonding layer of the thermal barrier coating.
[0010] Furthermore, the first condition is: Rsm is not less than 160 μm.
[0011] Furthermore, the second condition is: when Ra satisfies the condition or both Ra and Rz satisfy the condition, and Rsm satisfies the first condition, Rsk is minimum.
[0012] Furthermore, the screening method further comprises: if there are multiple bonding layers with the smallest Rsk, screening out the bonding layer with the largest Rsm, and using the corresponding preparation process as the preparation process of the bonding layer of the thermal barrier coating.
[0013] Furthermore, the value range of Ra that satisfies the condition is 3 to 8 μm.
[0014] Furthermore, the bonding layer is a MCrAlY-X metal bonding layer prepared by a supersonic flame spraying process, wherein M represents Ni, Co, CoNi or NiCo; and X represents a refractory or activated element, or does not contain the X element.
[0015] Furthermore, when detecting the surface roughness index of the bonding layer, the sampling length L is 0.8 to 2.5 mm, and the evaluation length is 1L to 5L.
[0016] Furthermore, when testing the surface roughness index of the bonding layer, a contact type roughness meter is used for testing.
[0017] The method for screening the preparation process of the bonding layer of the thermal barrier coating provided by the present invention can produce the following beneficial effects:
[0018] The present invention provides a method for screening the preparation process of the bonding layer of the thermal barrier coating. After the bonding layer of the thermal barrier coating is prepared by the preparation process to be screened, the surface roughness index profile average arithmetic deviation value Ra, profile average width Rsm, profile inclination Rsk, or the average height of unevenness Rz of the bonding layer are detected, and the preparation process of the bonding layer of the thermal barrier coating is determined by screening the above index values of each bonding layer. The screening method provided by the present invention evaluates the bonding layer by several surface roughness indicators such as Ra, Rsm and Rsk, so the screening preparation process can effectively improve the interface matching of the bonding layer of the thermal barrier coating and the ceramic thermal insulation layer, so that the thermal insulation ceramic layer is not easy to fall off from the bonding layer, thereby effectively extending the life of the thermal barrier coating, and the thermal cycle test also verifies this.
[0019] In addition, compared with the conventional method of preparing the bonding layer and ceramic insulation layer of the thermal barrier coating and then conducting a large number of thermal cycle tests to screen the preparation process, the screening method provided by the present invention significantly shortens the time consumption, and can greatly save manpower and costs, and improve the screening efficiency of the preparation process of the thermal barrier coating bonding layer.
[0020] The second object of the present invention is to provide a method for preparing a thermal barrier coating to solve the technical problem of the relatively short service life of the thermal barrier coating in the prior art.
[0021] The method for preparing a thermal barrier coating provided by the present invention comprises the following steps:
[0022] Pre-treating the high temperature alloy substrate;
[0023] Using the preparation process selected by the above-mentioned screening method for preparing a bonding layer of a thermal barrier coating, a bonding layer is prepared on the surface of the alloy substrate;
[0024] A ceramic heat-insulating layer is prepared on the surface of the bonding layer.
[0025] The method for preparing a thermal barrier coating provided by the present invention adopts the thermal barrier coating bonding layer preparation process screened out by the above-mentioned screening method to prepare the bonding layer. Therefore, the interface matching between the bonding layer and the thermal insulation ceramic layer is relatively good, the ceramic thermal insulation layer is not easy to fall off from the bonding layer, and the service life of the thermal barrier coating is relatively long.
[0026] The third object of the present invention is to provide a thermal barrier coating to solve the technical problem of the relatively short life of the thermal barrier coating in the prior art.
[0027] The thermal barrier coating provided by the present invention is prepared by adopting the above-mentioned thermal barrier coating preparation method.
[0028] The thermal barrier coating provided by the present invention is prepared by the above-mentioned thermal barrier coating preparation method, so the interface matching between the bonding layer and the thermal insulation ceramic layer is relatively good, the ceramic thermal insulation layer is not easy to fall off from the bonding layer, and the service life is relatively long. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0030] Figure 1 A flow chart of a method for screening a process for preparing a bonding layer of a thermal barrier coating provided in an embodiment of the present invention;
[0031] Figure 2 A flowchart of a method for preparing a thermal barrier coating provided by an embodiment of the present invention;
[0032] Figure 3 A diagram briefly showing a method for screening a process for preparing a bonding layer of a thermal barrier coating provided in an embodiment of the present invention;
[0033] Figure 4 This is the cross-sectional SEM morphology of the NiCoCrAlYHfSi bonding layer selected in Example 1 of the present invention;
[0034] Figure 5 This is the cross-sectional SEM morphology of the NiCoCrAlYHfSi / YSZ thermal barrier coating selected in Example 1 of the present invention;
[0035] Figure 6 This is the appearance of the NiCoCrAlYHfSi / YSZ thermal barrier coating selected in Example 1 of the present invention after 100 thermal shock tests;
[0036] Figure 7 This is the appearance of the CoCrAlSiY / YSZ+CMAS protective layer thermal barrier coating selected in Example 2 of the present invention after 60 thermal shock tests;
[0037] Figure 8 This is the cross-sectional SEM morphology of the CoNiCrAlY bonding layer selected in Example 3 of the present invention;
[0038] Fig. 9 This is the appearance of the CoNiCrAlY / YSZ thermal barrier coating selected in Example 3 of the present invention after a 1950h thermal cycle test. DETAILED DESCRIPTION
[0039] In order to make the above-mentioned objects, features and advantages of the present invention more clearly understood, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0040] This embodiment provides a method for screening the preparation process of a bonding layer of a thermal barrier coating. Figure 1 As shown, the screening method comprises the following steps:
[0041] S110, prepare a bonding layer using the preparation process to be screened, and detect the surface roughness indicators Ra, Rsm and Rsk, or Ra, Rz, Rsm and Rsk of each bonding layer. Wherein, the bonding layer is an MCrAlY-X metal bonding layer prepared by supersonic flame spraying process, M represents Ni, Co, CoNi or NiCo; X represents a refractory or activated element, or does not contain X element. All the preparation processes to be screened are supersonic flame spraying processes, and the difference lies in different process parameters.
[0042] When testing the surface roughness index of the bonding layer, a contact type roughness meter is used for testing. The sampling length L is 0.8 to 2.5 mm, and the evaluation length is 1L to 5L.
[0043] S120, based on the surface roughness index Ra or Ra and Rz of each bonding layer, screen out bonding layers whose Ra meets the condition or whose Ra and Rz both meet the condition, wherein the value range of Ra meeting the condition is 3-8 μm.
[0044] S130, from the bonding layers where Ra meets the conditions or Ra and Rz both meet the conditions, screen out the bonding layers where Rsm meets the first condition and Rsk meets the second condition, and use the corresponding preparation process as the preparation process of the bonding layer of the thermal barrier coating. Among them, the first condition is: Rsm is not less than 160μm, that is, Rsm≥160μm; the second condition is: under the premise that Ra meets the conditions or Ra and Rz both meet the conditions, and Rsm meets the first condition, Rsk is the smallest, that is, under the premise that Ra is within the value range of 3 to 8μm or Rz also meets the conditions, first screen out the bonding layers where Rsm≥160μm and screen out the bonding layer with the smallest Rsk.
[0045] Preferably, Rsm should be as large as possible, at least greater than or equal to 160 μm, and Rsk should be as small as possible. Therefore, if there are multiple bonding layers with the smallest Rsk, the bonding layer with the largest Rsm is selected and its corresponding preparation process is used as the preparation process of the bonding layer of the thermal barrier coating.
[0046] The present embodiment provides a method for screening the preparation process of the bonding layer of the thermal barrier coating. After the bonding layer of the thermal barrier coating is prepared by the preparation process to be screened, the surface roughness index profile average arithmetic deviation value Ra, profile average width Rsm, profile inclination Rsk, or together with the average height of unevenness Rz of the bonding layer are detected, and the preparation process of the bonding layer of the thermal barrier coating is determined by screening the above index values of each bonding layer. The screening method provided in this embodiment evaluates the bonding layer by several surface roughness indicators such as Ra, Rsm and Rsk, so the screening preparation process can effectively improve the interface matching of the bonding layer of the thermal barrier coating and the ceramic thermal insulation layer, so that the thermal insulation ceramic layer is not easy to fall off from the bonding layer, thereby effectively extending the life of the thermal barrier coating, which is also verified by the thermal cycle test.
[0047] In addition, compared with the conventional method of preparing the bonding layer and ceramic insulation layer of the thermal barrier coating and then conducting a large number of thermal cycle tests to screen the preparation process, the screening method provided in this embodiment is significantly shorter in time, and can greatly save manpower and material resources and improve the screening efficiency of the preparation process of the thermal barrier coating bonding layer.
[0048] In short, on the basis of controlling the surface roughness index Ra or Ra&Rz, the present application further couples the roughness indexes Rsk and Rsm, and adopts a low-cost stylus method to measure and control the surface state of different MCrAlY-X metal bonding layers. The sharp area on the bonding layer surface is reduced by controlling the inclination, and the undulation of the bonding layer is reduced by controlling the average width of the profile. This is beneficial to ensure the roughness of the bonding layer / ceramic layer interface while improving the thermal shock resistance and thermal cycle life of the coating, thereby improving the service performance of the coating.
[0049] This embodiment also provides a method for preparing a thermal barrier coating. Figure 2 As shown, the preparation method comprises the following steps:
[0050] S210, pretreating the high temperature alloy substrate;
[0051] S220, preparing a bonding layer on the surface of the alloy substrate using a preparation process selected by the above-mentioned screening method for preparing a bonding layer of a thermal barrier coating;
[0052] S230, preparing a ceramic heat insulation layer on the surface of the bonding layer.
[0053] The method for preparing the thermal barrier coating provided in this embodiment adopts the thermal barrier coating bonding layer preparation process selected by the above-mentioned screening method to prepare the bonding layer. Therefore, the interface matching between the bonding layer and the thermal insulation ceramic layer is relatively good, the ceramic thermal insulation layer is not easy to fall off from the bonding layer, and the service life of the thermal barrier coating is relatively long.
[0054] This embodiment also provides a thermal barrier coating, which is prepared by the above-mentioned thermal barrier coating preparation method. Therefore, the interface matching between the bonding layer and the thermal insulation ceramic layer of the thermal barrier coating is relatively good, the ceramic insulation layer is not easy to fall off from the bonding layer, and the service life is relatively long.
[0055] The following are three specific embodiments, in which different HVOF spraying process parameters are used to deposit an MCrAlY bonding layer of a thermal barrier coating on the surface of a high-temperature alloy substrate, and a contact roughness meter is used to test the surface roughness of the bonding layer prepared under different process conditions. On this basis, the thermal barrier coating ceramic layer is prepared by APS technology, and finally the effectiveness of the thermal barrier coating bonding layer preparation process screening method provided in this application is verified by a thermal shock test or a thermal impact test: on the basis of ensuring that the roughness index Ra of the bonding layer is within the range of 3 to 8 μm, the bonding layer with a roughness index Rsm ≥ 160 μm and the smallest Rsk has the longest life.
[0056] Embodiment 1
[0057] By adjusting the HVOF spraying process parameters, the NiCoCrAlYHfSi bonding layer of thermal barrier coating with different surface states is deposited on the surface of the high-temperature alloy substrate. The surface roughness of the bonding layer prepared under different process conditions is tested using a contact roughness tester. After the ceramic layer is prepared using the APS technology, the thermal shock resistance of the thermal barrier coating is tested. The specific steps are as follows:
[0058] Step 1: pre-treat the high-temperature alloy substrate. Use acetone solution to clean the surface of the substrate alloy; after the surface of the substrate alloy is dry, perform sandblasting to roughen it. The sandblasting process parameters are: select white corundum Al2O3 with a particle size of 60 mesh, the sandblasting pressure is 0.3-0.4MPa, the sandblasting distance is 60-80mm, and the sandblasting angle is 80-90°; after the sandblasting roughening treatment is completed, use compressed nitrogen to blow away the residual sand on the surface of the substrate alloy.
[0059] Step 2: Using three different combinations of supersonic flame spraying process parameters as shown in Table 1, bonding layers are prepared on the surface of the alloy substrate. The bonding layer material is NiCoCrAlYHfSi, and the powder particle size distribution is -63μm to +15μm. The thickness of the bonding layer prepared by the supersonic flame spraying process is about 130 to 170μm.
[0060] Table 1
[0061]
[0062] Step three, use a contact roughness meter to detect the surface roughness of the bonding layers prepared by the above-mentioned different spraying processes. The measurement parameters of the roughness meter are: sampling length L is 0.8~2.5mm, evaluation length is 1L~5L, and after the test is completed, the Ra, Rsm, Rsk and other indicators of each bonding layer are recorded, as shown in Table 2.
[0063] Table 2
[0064] serial number Ra / μm Rsm / μm R NiCo-1 6.2 163 0.21 NiCo-2 4.3 148 -0.018 NiCo-3 5.5 160 0.151
[0065] Step 4: Prepare a ceramic heat-insulating layer as required. A YSZ ceramic layer with a vertical crack structure is prepared on the above three alloy substrates with a NiCoCrAlYHfSi bonding layer by an atmospheric plasma spraying method, and the thickness of the prepared ceramic layer is 350-400 μm.
[0066] The three NiCoCrAlYHfSi / YSZ thermal barrier coating samples prepared in Example 1 were subjected to a thermal shock test. The specific test conditions were: one cycle was to keep the temperature at 1100°C for 10 minutes and then cool the temperature to room temperature with water. The test results showed that after 100 thermal cycles, the thermal barrier coating with a roughness of Ra=5.5, Rsm=160, and Rsk=0.151 only slightly peeled off at the edge. Figure 4 As shown, combined with Figure 2 and Figure 3 , showing the best thermal shock resistance among the tested samples, verifying the effectiveness of the thermal barrier coating bonding layer preparation process screening method provided in this application.
[0067] Embodiment 2
[0068] By adjusting the HVOF spraying process parameters, the CoCrAlSiY bonding layer of thermal barrier coating with different surface states is deposited on the surface of the high-temperature alloy substrate. The surface roughness of the bonding layer prepared under different process conditions is tested using a contact roughness tester. After the ceramic layer is prepared using the APS technology, the thermal shock resistance of the thermal barrier coating is tested. The specific steps are as follows:
[0069] Step 1: pre-treat the high-temperature alloy substrate. Use acetone solution to clean the surface of the substrate alloy; after the surface of the substrate alloy is dry, perform sandblasting to roughen it. The sandblasting process parameters are: select white corundum Al2O3 with a particle size of 60 mesh, the sandblasting pressure is 0.2-0.4MPa, the sandblasting distance is 60-80mm, and the sandblasting angle is 80-90°; after the sandblasting roughening treatment is completed, use compressed nitrogen to blow away the residual sand on the surface of the substrate alloy.
[0070] Step 2: Adhesive layers are prepared on the surface of the alloy substrate using three different combinations of supersonic flame spraying process parameters as shown in Table 3. The adhesive layer material is CoCrAlSiY, the powder particle size distribution is -45 to +15 μm, and the thickness of the adhesive layer prepared by the supersonic flame spraying process is about 130 to 170 μm.
[0071] Table 3
[0072]
[0073]
[0074] Step three, use a contact roughness meter to detect the surface roughness of the bonding layers prepared by the above-mentioned different spraying processes. The measurement parameters of the roughness meter are: sampling length L is 0.8~2.5mm, evaluation length is 1L~5L, and after the test is completed, the Ra, Rsm, Rsk and other indicators of each bonding layer are recorded, as shown in Table 4.
[0075] Table 4
[0076] serial number Ra / μm Rsm / μm R CoCr-1 6.5 180 0.228 CoCr-2 4.8 170.2 0.228 CoCr-3 7.2 182 0.31
[0077] Step 4: Prepare a ceramic thermal insulation layer as required. A ceramic layer with the same YSZ+CMAS protective layer structure is prepared on the above three alloy substrates with a CoCrAlSiY bonding layer by an atmospheric plasma spraying method, and the thickness of the prepared ceramic layer is 200-300 μm.
[0078] The three CoCrAlSiY / YSZ+CMAS protective layer thermal barrier coating samples prepared in Example 2 were subjected to thermal shock tests. The specific test conditions were: one cycle was to keep the temperature at 1100°C for 10 minutes and then cool it to room temperature with water. The test results showed that after 100 thermal cycles, the thermal barrier coating with a roughness of Ra=6.5, Rsm=180, and Rsk=0.228 only slightly peeled off at the edge. Figure 5 As shown, the best thermal shock resistance was exhibited among the tested samples, verifying the effectiveness of the thermal barrier coating bonding layer preparation process screening method provided in the present application.
[0079] Embodiment 3
[0080] By adjusting the HVOF spraying process parameters, the CoNiCrAlY bonding layer of thermal barrier coating with various roughness is deposited on the surface of the high-temperature alloy substrate. The surface roughness of the bonding layer prepared under different process conditions is tested using a contact roughness tester. After the ceramic layer is prepared using the APS technology, the thermal cycle performance of the thermal barrier coating is tested. The specific steps are as follows:
[0081] Step 1: pre-treat the high-temperature alloy substrate. Use acetone solution to clean the surface of the substrate alloy; after the surface of the substrate alloy is dry, perform sandblasting to roughen it. The sandblasting process parameters are: select white corundum Al2O3 with a particle size of 60 mesh, the sandblasting pressure is 0.2-0.4MPa, the sandblasting distance is 60-80mm, and the sandblasting angle is 80-90°; after the sandblasting roughening treatment is completed, use compressed nitrogen to blow away the residual sand on the surface of the substrate alloy.
[0082] Step 2: Using three different combinations of supersonic flame spraying process parameters as shown in Table 5, bonding layers are prepared on the surface of the alloy substrate. The bonding layer material is CoNiCrAlY, and the powder particle size distribution is -45μm to +15μm. The thickness of the bonding layer prepared by the supersonic flame spraying process is about 150 to 200μm.
[0083] Table 5
[0084]
[0085] Step three, use a contact roughness meter to detect the surface roughness of the bonding layers prepared by the above-mentioned different spraying processes. The measurement parameters of the roughness meter are: sampling length L is 0.8~2.5mm, evaluation length is 1L~5L, and after the test is completed, the Ra, Rsm, Rsk and other indicators of each bonding layer are recorded, as shown in Table 6.
[0086] Table 6
[0087] serial number Ra / μm Rsm / μm R CoNi-1 6.9 249 -0.05 CoNi-2 5.3 277 -0.052 CoNi-3 6.6 235 0.034
[0088] Step 4: Prepare a ceramic heat-insulating layer as required. YSZ ceramic layers of the same thickness are prepared on the above three alloy substrates with CoNiCrAlY bonding layers by atmospheric plasma spraying, and the thickness of the prepared ceramic layers is 250-300 μm.
[0089] The three CoNiCrAlY / YSZ thermal barrier coating samples prepared in Example 3 were subjected to a thermal cycle test. The specific test conditions were: keeping at 1050°C for 50 minutes and then cooling in an air environment (room temperature) for 10 minutes as one cycle. The test results showed that after the thermal barrier coating with roughness Ra=5.3, Rsm=277, and Rsk=-0.052 was subjected to a 1950h thermal cycle test, the thermal barrier coating remained intact without peeling. Figure 7 As shown, combined with Figure 6 , showing the best thermal cycle resistance among the tested samples, verifying the effectiveness of the thermal barrier coating bonding layer preparation process screening method provided in this application.
[0090] Finally, it should be noted that, in this article, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0091] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to the embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for screening a preparation process of a bonding layer of a thermal barrier coating, characterized in that: The steps include: Adopting the preparation process to be screened to prepare the bonding layer, and testing the surface roughness indexes Ra, Rsm and Rsk, or Ra, Rz, Rsm and Rsk of each bonding layer; According to the surface roughness index Ra or Ra and Rz of each bonding layer, the bonding layers whose Ra meets the condition or whose Ra and Rz meet the condition are screened out; From the bonding layers whose Ra meets the condition or whose Ra and Rz both meet the condition, screen out the bonding layers whose Rsm meets the first condition and whose Rsk meets the second condition, and use the corresponding preparation process as the preparation process of the bonding layer of the thermal barrier coating; The first condition is: Rsm is not less than 160 μm; The second condition is: Rsk is minimum when Ra satisfies the condition or both Ra and Rz satisfy the condition and Rsm satisfies the first condition; If there are multiple bonding layers with the smallest Rsk, the bonding layer with the largest Rsm is selected and its corresponding preparation process is used as the preparation process of the bonding layer of the thermal barrier coating; The value range of Ra that meets the conditions is 3 to 8 μm.
2. The method for screening a preparation process of a bonding layer of a thermal barrier coating according to claim 1, characterized in that: The bonding layer is an MCrAlY-X metal bonding layer prepared by supersonic flame spraying process, wherein M represents Ni, Co, CoNi or NiCo; X represents a refractory or activated element, or does not contain the X element.
3. The method for screening a preparation process of a bonding layer of a thermal barrier coating according to claim 1, characterized in that: When testing the surface roughness index of the bonding layer, the sampling length L is 0.8 to 2.5 mm and the evaluation length is 1L to 5L.
4. The method for screening a preparation process of a bonding layer of a thermal barrier coating according to claim 1, characterized in that: When testing the surface roughness index of the bonding layer, a contact type roughness meter is used for testing.
5. A method for preparing a thermal barrier coating, characterized in that: The steps include: Pre-treating the high temperature alloy substrate; Using a preparation process selected by the method for selecting a preparation process for a thermal barrier coating bonding layer according to any one of claims 1 to 4, preparing a bonding layer on the surface of an alloy substrate; A ceramic heat-insulating layer is prepared on the surface of the bonding layer.