A method for manufacturing stainless steel matte enamel

Through the combination of stainless steel matrix surface roughening and silicon oxygen-based precoating, the stability of stainless steel enamel materials in external force impact and flame ablation is solved, and the high stability and long-term effectiveness of the enamel coating are achieved, which is significantly Improves heat resistance and corrosion resistance.

CN118086904BActive Publication Date: 2024-11-08ZHEJIANG RUIDA ELECTRIC APPLIANCE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410254967.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-06
Publication Date
2024-11-08
Estimated Expiration
2044-03-06

AI Technical Summary

Technical Problem

Existing stainless steel enamel materials are susceptible to external impacts during use, and long-term flame ablation will cause damage, mainly due to the unstable bonding problem between the enamel coating and the stainless steel substrate.

Method used

Through the roughening treatment of the stainless steel matrix surface, the silicon oxygen-based precoat is used to form an integrated connection with the silicon oxygen material in the matte enamel coating, thereby improving the stability and long-term effectiveness of the enamel coating. The specific steps include degreasing treatment using sodium bicarbonate and sodium hydroxide solution, spraying dilute acid solution to remove the oxide layer, sandblasting treatment to improve the surface roughness, then spraying trimethoxysilane to form a silane dissolving solution, and finally spraying matte enamel The coating and aqueous ether are cured.

Benefits of technology

It effectively solves the problem of explosive porcelain in stainless steel enamel, improves the adhesion fastness and heat resistance of the enamel coating, extends the service life, and performs well in high and low temperature impact and corrosion resistance tests.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for manufacturing stainless steel matte enamel, wherein a stainless steel substrate is subjected to alkali washing and acid washing to obtain a pre-treated stainless steel substrate; the pre-treated stainless steel substrate is subjected to sandblasting treatment, and then the sandblasted stainless steel substrate is placed in distilled water for treatment, and then soaked in an aqueous ether solution to obtain a pre-treated stainless steel substrate; trimethoxysilane is added to ether to form a silane solution, and then the solution is sprayed onto the surface of the pre-treated stainless steel substrate to obtain a pre-coated stainless steel substrate; a matte enamel coating is sprayed onto the pre-coated stainless steel substrate to obtain a coated stainless steel substrate; and aqueous ether is sprayed onto the surface of the coated stainless steel substrate to obtain stainless steel matte enamel. The invention utilizes a silicon-oxygen pre-coating layer to form an integrated connection with a silicon-oxygen material in a matte enamel coating layer, thereby improving the stability and long-term effectiveness of the enamel coating layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of stainless steel enamel, and in particular relates to a method for manufacturing stainless steel matte enamel. Background Art

[0002] At present, enamel pot brackets are mainly divided into matte enamel pot brackets and bright enamel pot brackets. With the market demand, enamel pots with stainless steel as the metal substrate are becoming more and more popular, but the surface of stainless steel is usually inert and stable under oxidizing conditions. However, matte enamel materials are easily impacted by external forces during use, causing porcelain explosion, or as the use time increases, long-term flame ablation will cause damage to the enamel material. In essence, it is still a bonding problem between the enamel coating and the stainless steel substrate. Summary of the invention

[0003] In view of the problems in the prior art, the present invention provides a method for manufacturing matte enamel of stainless steel, which solves the problem of ceramic cracking of the existing stainless steel enamel, increases the contact surface of the stainless steel substrate by roughening the surface of the stainless steel substrate, and uses a silicon-oxygen pre-coating layer to cooperate with the silicon-oxygen material in the matte enamel coating to form an integrated connection, thereby improving the stability and long-term effectiveness of the enamel coating.

[0004] In order to achieve the above technical objectives, the technical solution of the present invention is:

[0005] A method for manufacturing stainless steel matte enamel, comprising the following steps:

[0006] Step 1, adding sodium bicarbonate and sodium hydroxide to distilled water and stirring evenly to form a dissolving solution, then immersing the stainless steel substrate in the dissolving solution for 30-50 minutes, taking it out and rinsing it and drying it to obtain a stainless steel substrate with a clean surface; the mass ratio of the sodium bicarbonate to the sodium hydroxide is 4:1-1.3, the pH of the dissolving solution is 8, the stirring speed is 100-300r / min, the immersion temperature is 30-50°C; the drying temperature is 100-120°C; this step utilizes sodium bicarbonate and sodium hydroxide to be dissolved in water to form an alkaline solution, and promotes the reaction between sodium hydroxide and surface grease during the immersion process to achieve the effect of degreasing and washing; in order to improve the degreasing effect during the immersion process, the stainless steel substrate is subjected to a constant temperature ultrasonic treatment of 60-80kHz while being immersed in the dissolving solution to ensure that the grease on the surface of the stainless steel substrate is completely removed and the surface of the stainless steel substrate is clean;

[0007] Step 2: spray a dilute acid solution on the clean surface of the stainless steel substrate, and keep it at a constant temperature for 2-3 hours, ultrasonically clean it with distilled water for 20-30 minutes, and dry it to obtain a pretreated stainless steel substrate; the dilute acid solution is a mixture of hydrochloric acid and sulfuric acid with a pH of 6, and the molar ratio of hydrochloric acid to sulfuric acid is 1:3, and the spraying amount is 2-4mL / cm2 , the temperature of the constant temperature static is 3-5°C; the ultrasonic frequency of the ultrasonic cleaning is 70-90kHz, and the temperature is 50-80°C; the drying is carried out in a nitrogen atmosphere, and the temperature is 120-140°C; this step sprays a layer of acid liquid film on the surface of the stainless steel substrate from which grease is removed, which can destroy the oxide layer on the surface of the stainless steel substrate. At the same time, the stainless steel substrate containing the liquid film is placed in distilled water for ultrasonic cleaning, and the acid liquid film is directly dispersed in the distilled water, and the acid liquid film is separated from the stainless steel substrate by the high-frequency vibration of the ultrasound;

[0008] Step 3, the pre-treated stainless steel substrate is sandblasted for 10-20s, and then the sandblasted stainless steel substrate is placed in distilled water for ultrasonic treatment to remove surface impurities, and then dried and placed in an aqueous ether solution for immersion for 10-20min, and then taken out and dried at low temperature to obtain the pre-treated stainless steel substrate, wherein the ultrasonic frequency of the ultrasonic treatment is 60-80kHz, the temperature is 20-30°C, and the drying temperature is 100-120°C; the preparation method of the aqueous ether solution comprises: a1, anhydrous ether and distilled water are placed in a reactor and stirred evenly, and low-temperature ultrasonic treatment is performed for 20-30min, and the layered liquid is obtained by standing, wherein the volume ratio of the anhydrous ether to the distilled water is 10-20:1, the stirring speed is 200-500r / min, the temperature of the low-temperature ultrasonic treatment is 5-10°C, and the ultrasonic frequency is 70-90kHz; the standing temperature is 20-25°C; this step utilizes anhydrous ether Ether and distilled water are stirred and mixed to achieve full contact between the two, and at the same time, the micro-solubility of ether and distilled water is utilized to form a stable dispersion. The low-temperature ultrasonic treatment here utilizes the high-frequency vibration of ultrasound to promote the full contact between ether and distilled water, thereby improving the dissolution of distilled water in the ether liquid. At the same time, after stirring and sufficient ultrasonic mixing, the distilled water in the ether has reached dissolution saturation. Therefore, the stratification after standing is based on the stratification of ether and distilled water in a micro-soluble system; a2, extracting the ether liquid in the stratified liquid to obtain an aqueous ether liquid, and the extraction temperature is 5-10°C; this step is to extract the stratified liquid, the density of ether in the stratified liquid is less than that of water, and a stratification of distilled water and ether will be formed. The ether liquid can be obtained by extracting the upper layer liquid, and ether and water are micro-soluble, and a clear stratification line can be formed. At the same time, a small amount of distilled water is dissolved in the ether layer. Therefore, the ether liquid after extraction contains a very small amount of distilled water, that is, aqueous ether is obtained. The aqueous ether prepared by the method forms saturated solution by natural dissolution and penetration; the temperature of the low-temperature drying is 40-45°C; the surface of the pre-treated stainless steel is roughened by sandblasting to improve the roughness of the specific surface, and the impurities on the rough surface are completely stripped and removed during the ultrasonic process of distilled water to ensure the cleanliness of the rough surface; at the same time, during the low-temperature drying process, the volatility and low boiling point characteristics of the ether itself are directly converted into steam, and the distilled water remains, resulting in a liquid film on the rough surface;

[0009] Step 4: adding trimethoxysilane to ether to form a silane solution, and then spraying it onto the surface of the pre-treated stainless steel substrate, standing at low temperature for 2-3 hours, to obtain a pre-coated stainless steel substrate; the concentration of the trimethoxysilane in ether is 10-30 g / L, the spray temperature is 5-10 ° C, and the spray volume is 4-8 mL / cm 2 , the temperature of the low-temperature standing is 20-30°C; this step utilizes the solubility of trimethoxysilane in ether to achieve a good dissolution effect, and then sprays it on the surface of the stainless steel substrate after pretreatment. At this time, the distilled water forms contact with the trimethoxysilane and is converted into a contact hydrolysis reaction, thereby forming a trihydroxysilane structure. In the subsequent treatment process, the ether is directly removed during the long-term low-temperature standing due to its own volatility, thereby forming a viscous pre-coating film, which can be tightly attached to the surface of the stainless steel substrate to form a stable connection. Moreover, the pre-coating film has good surface activity and can form a stable connection with the subsequent enamel coating. At the same time, the pre-coating film itself belongs to the trihydroxysilane material, which is essentially a silicon oxide precursor, has good adhesion and thermal insulation, and effectively solves the heat transfer problem of stainless steel;

[0010] Step 5, spraying the matte enamel coating on the pre-coated stainless steel substrate, depressurizing and standing for 2-3 hours to obtain a coated stainless steel substrate, wherein the spraying amount of the matte enamel coating is 5-10 mL / cm 2, the temperature is 20-30℃; the pressure of the decompression and static state is 70-80% of the atmospheric pressure, and the temperature is 20-30℃; the mass ratio of the matte enamel is: 5-10 parts of aluminum isopropoxide, 3-6 parts of cobalt oxide, 5-8 parts of ethyl silicate, 8-15 parts of dimethoxydimethylsilane, 3-6 parts of kaolin, 1-3 parts of sodium fluorosilicate, 30-60 parts of matte glaze enamel powder, and 60-90 parts of anhydrous ether, and the matte glaze enamel powder comes from Hunan Noli New Materials Co., Ltd.; and the preparation method of the matte enamel coating includes: b1, grinding and mixing cobalt oxide, kaolin, sodium fluorosilicate, and matte glaze enamel powder to obtain a mixed fine powder; b2, adding aluminum isopropoxide, ethyl silicate, and dimethyldimethoxysilane to anhydrous ether and stirring evenly to form a dissolving solution; b3, adding the mixed fine powder to the dissolving solution Ultrasonic treatment is performed for 20-30 minutes to obtain a matte enamel coating. The temperature of the ultrasonic treatment is 5-10°C and the ultrasonic frequency is 60-80kHz. The process uses grinding to refine solid particles and form a homogeneous dispersion in a solvent with a certain viscosity, thereby obtaining a stable dispersion system. At the same time, the high-frequency vibration of the ultrasound homogenizes and disperses the particles, thereby obtaining a uniformly dispersed slurry. In the treatment step, the dimethoxydimethylsilane and ethyl silicate in the matte enamel coating are homogeneous materials with the pre-coated stainless steel substrate surface. After hydrolysis, similar silanol structures are formed, which have good adhesion, thereby improving the adhesion of the matte enamel coating on the stainless steel substrate surface. The temperature during the depressurization and static process and the self-volatility of ether can completely remove the ether in the liquid film, thereby forming a surface film structure.

[0011] Step 6, spraying aqueous ether onto the surface of the coated stainless steel substrate, and standing for 2-4 hours, and curing to obtain stainless steel matte enamel; the preparation method of the aqueous ether liquid includes: a1, putting anhydrous ether and distilled water into a reactor and stirring evenly, and performing low-temperature ultrasonic treatment for 20-30 minutes, standing to obtain a layered liquid, the volume ratio of the anhydrous ether to distilled water is 10-20:1, the stirring speed is 200-500r / min, the temperature of the low-temperature ultrasonic treatment is 5-10°C, the ultrasonic frequency is 70-90kHz; the standing temperature is 20-25°C; a2, extracting the ether liquid in the layered liquid to obtain an aqueous ether liquid, the extraction temperature is 5-10°C; the spraying amount of the spray is 5-10mL / cm 2, the temperature is 5-10 ℃; the standing temperature is 40-50 ℃; the curing time is 5-10 ℃, and the temperature is 700-800 ℃; this step utilizes aqueous ether spraying on the surface of the coated stainless steel substrate, and utilizes the ether itself to dissolve the solute to ensure that the water molecules are in contact with ethyl silicate, aluminum isopropoxide and dimethoxydimethyl, and form good connectivity during the standing process, thereby realizing an integrated structure; in the matte enamel coating, dimethoxydimethylsilane and ethyl silicate are in liquid state, and can show excellent permeability, thereby forming a dense silicon oxide encapsulation structure, and the transparency of the silicon oxide material does not affect the matte characteristics of the overall structure, and aluminum isopropoxide is converted into aluminum oxide after hydrolysis and high-temperature curing, and the aluminum oxide can achieve local temperature diffusion, effectively controlling the problem of temperature bumps.

[0012] It can be seen from the above description that the present invention has the following advantages:

[0013] 1. The present invention solves the problem of cracking of existing stainless steel enamel, increases the contact surface of the stainless steel substrate by roughening the surface of the stainless steel substrate, and uses the silicon-oxygen pre-coating layer to form an integrated connection with the silicon-oxygen material in the matte enamel coating, thereby improving the stability and long-term effectiveness of the enamel coating.

[0014] 2. The present invention utilizes a silicon-oxygen pre-coating as a connection between the matte ceramic coating and the stainless steel substrate, thereby improving the adhesion strength of the coating. At the same time, the silicon-oxygen pre-coating has good thermal insulation properties, thereby effectively reducing the thermal conductivity and heat transfer characteristics of the stainless steel substrate. DETAILED DESCRIPTION

[0015] The present invention is described in detail with reference to the embodiments, but no limitation is imposed on the claims of the present invention.

[0016] Example 1

[0017] A method for manufacturing stainless steel matte enamel, comprising the following steps:

[0018] Step 1, adding sodium bicarbonate and sodium hydroxide to distilled water and stirring evenly to form a dissolving solution, then immersing the stainless steel substrate in the dissolving solution for 30 minutes, taking it out and rinsing it and drying it to obtain a stainless steel substrate with a clean surface; the mass ratio of the sodium bicarbonate to the sodium hydroxide is 4:1, the pH of the dissolving solution is 8, the stirring speed is 100 r / min, the immersion temperature is 30° C.; the drying temperature is 100° C.;

[0019] Step 2: spray a dilute acid solution on the cleaned stainless steel substrate surface, and keep it at a constant temperature for 2 hours, ultrasonically clean it with distilled water for 20 minutes, and dry it to obtain a pretreated stainless steel substrate; the dilute acid solution is a mixture of hydrochloric acid and sulfuric acid with a pH of 6, and the molar ratio of hydrochloric acid to sulfuric acid is 1:3, and the spray volume is 2mL / cm2 The constant temperature is 3°C; the ultrasonic cleaning is performed at an ultrasonic frequency of 70kHz and a temperature of 60°C; the drying is performed in a nitrogen atmosphere at a temperature of 120°C;

[0020] Step 3, sandblasting the pretreated stainless steel substrate for 10 seconds, then placing the sandblasted stainless steel substrate in distilled water for ultrasonic treatment to remove surface impurities, drying and then soaking it in aqueous ether solution for 10 minutes, taking it out and drying it at low temperature to obtain the pretreated stainless steel substrate, the ultrasonic frequency of the ultrasonic treatment is 60kHz, the temperature is 20°C, and the drying temperature is 100°C; the preparation method of the aqueous ether solution includes: a1, putting anhydrous ether and distilled water into a reactor and stirring them evenly, and performing low-temperature ultrasonic treatment for 20 minutes, standing to obtain a layered liquid, the volume ratio of anhydrous ether to distilled water is 10:1, the stirring speed is 200r / min, the temperature of the low-temperature ultrasonic treatment is 5°C, and the ultrasonic frequency is 70kHz; the standing temperature is 20°C; a2, extracting the ether liquid in the layered liquid to obtain an aqueous ether liquid, the extraction temperature is 5°C; the temperature of the low-temperature drying is 40°C;

[0021] Step 4: adding trimethoxysilane to ether to form a silane solution, and then spraying it onto the surface of the pre-treated stainless steel substrate, standing at low temperature for 2 hours, to obtain a pre-coated stainless steel substrate; the concentration of the trimethoxysilane in ether is 10 g / L, the spray temperature is 5 ° C, and the spray volume is 4 mL / cm 2 , the low temperature standing temperature is 20°C;

[0022] Step 5: Spray the matte enamel coating on the pre-coated stainless steel substrate, depressurize and let stand for 2 hours to obtain a coated stainless steel substrate. The spray volume of the matte enamel coating is 5 mL / cm 2 , the temperature is 20°C; the pressure of the decompression and static state is 70% of the atmospheric pressure, and the temperature is 20°C; the mass ratio of the matte enamel is: 5 parts of aluminum isopropoxide, 3 parts of cobalt oxide, 5 parts of ethyl silicate, 8 parts of dimethoxydimethylsilane, 3 parts of kaolin, 1 part of sodium fluorosilicate, 30 parts of matte glaze enamel powder, and 60 parts of anhydrous ether, and the matte glaze enamel powder comes from Hunan Noli New Materials Co., Ltd.; and the preparation method of the matte enamel coating comprises: b1, grinding and mixing cobalt oxide, kaolin, sodium fluorosilicate, and matte glaze enamel powder to obtain a mixed fine powder; b2, adding aluminum isopropoxide, ethyl silicate, and dimethyldimethoxysilane to anhydrous ether and stirring evenly to form a dissolving solution; b3, adding the mixed fine powder to the dissolving solution and ultrasonically treating it for 20 minutes to obtain a matte enamel coating, the temperature of the ultrasonic treatment is 5°C, and the ultrasonic frequency is 60kHz;

[0023] Step 6, spraying aqueous ether onto the surface of the coated stainless steel substrate, and standing for 2 hours, and curing to obtain stainless steel matte enamel; the preparation method of the aqueous ether liquid includes: a1, putting anhydrous ether and distilled water into a reactor and stirring evenly, and performing low-temperature ultrasonic treatment for 20 minutes, standing to obtain a layered liquid, the volume ratio of the anhydrous ether and distilled water is 10:1, the stirring speed is 200r / min, the temperature of the low-temperature ultrasonic treatment is 5°C, the ultrasonic frequency is 70kHz; the standing temperature is 20°C; a2, extracting the ether liquid in the layered liquid to obtain an aqueous ether liquid, the extraction temperature is 5°C; the spraying amount of the spray is 5mL / cm 2 , the temperature is 5°C; the static temperature is 40°C; the curing time is 5°C and the temperature is 700°C.

[0024] The stainless steel matte enamel of the present embodiment showed no porcelain bursting after 20 impacts at 400°C in the high and low temperature impact test; no porcelain bursting occurred when impacted by a 1-meter steel ball; no fish scale explosion occurred after long-term placement and use; in the corrosion resistance test, the neutral salt spray test for 72 hours and the acid salt spray test for 24 hours both performed well without corrosion.

[0025] Example 2

[0026] A method for manufacturing stainless steel matte enamel, comprising the following steps:

[0027] Step 1, adding sodium bicarbonate and sodium hydroxide to distilled water and stirring evenly to form a dissolving solution, then immersing the stainless steel substrate in the dissolving solution for 50 minutes, taking it out and rinsing it and drying it to obtain a stainless steel substrate with a clean surface; the mass ratio of the sodium bicarbonate to the sodium hydroxide is 4:1.3, the pH of the dissolving solution is 8, the stirring speed is 300r / min, the immersion temperature is 50°C; the drying temperature is 120°C;

[0028] Step 2: spray a dilute acid solution on the cleaned stainless steel substrate surface, and keep it at a constant temperature for 3 hours, ultrasonically clean it with distilled water for 30 minutes, and dry it to obtain a pretreated stainless steel substrate; the dilute acid solution is a mixture of hydrochloric acid and sulfuric acid with a pH of 6, and the molar ratio of hydrochloric acid to sulfuric acid is 1:3, and the spray volume is 4 mL / cm 2 The constant temperature is 5°C; the ultrasonic cleaning is performed at an ultrasonic frequency of 90kHz and a temperature of 80°C; the drying is performed in a nitrogen atmosphere at a temperature of 140°C;

[0029] Step 3, sandblasting the pretreated stainless steel substrate for 20 seconds, then placing the sandblasted stainless steel substrate in distilled water for ultrasonic treatment to remove surface impurities, drying and then soaking it in aqueous ether solution for 20 minutes, taking it out and drying it at low temperature to obtain the pretreated stainless steel substrate, the ultrasonic frequency of the ultrasonic treatment is 80kHz, the temperature is 30°C, and the drying temperature is 120°C; the preparation method of the aqueous ether solution comprises: a1, placing anhydrous ether and distilled water into a reactor and stirring evenly, and performing low-temperature ultrasonic treatment for 30 minutes, standing to obtain a layered liquid, the volume ratio of anhydrous ether to distilled water is 20:1, the stirring speed is 500r / min, the temperature of the low-temperature ultrasonic treatment is 10°C, and the ultrasonic frequency is 90kHz; the standing temperature is 25°C; a2, extracting the ether liquid in the layered liquid to obtain an aqueous ether liquid, the extraction temperature is 10°C; the temperature of the low-temperature drying is 45°C;

[0030] Step 4: adding trimethoxysilane to ether to form a silane solution, and then spraying it onto the surface of the pre-treated stainless steel substrate, standing at low temperature for 3 hours, to obtain a pre-coated stainless steel substrate; the concentration of the trimethoxysilane in ether is 30 g / L, the spray temperature is 10°C, and the spray volume is 8 mL / cm 2 , the low temperature standing temperature is 30°C;

[0031] Step 5: Spray the matte enamel coating onto the pre-coated stainless steel substrate, depressurize and let stand for 3 hours to obtain a coated stainless steel substrate. The spray volume of the matte enamel coating is 10 mL / cm 2 , the temperature is 30°C; the pressure of the decompression and static state is 80% of the atmospheric pressure, and the temperature is 30°C; the mass ratio of the matte enamel is: 10 parts of aluminum isopropoxide, 6 parts of cobalt oxide, 8 parts of ethyl silicate, 15 parts of dimethoxydimethylsilane, 6 parts of kaolin, 3 parts of sodium fluorosilicate, 60 parts of matte glaze enamel powder, and 90 parts of anhydrous ether, and the matte glaze enamel powder comes from Hunan Noli New Materials Co., Ltd.; and the preparation method of the matte enamel coating comprises: b1, grinding and mixing cobalt oxide, kaolin, sodium fluorosilicate, and matte glaze enamel powder to obtain a mixed fine powder; b2, adding aluminum isopropoxide, ethyl silicate, and dimethyldimethoxysilane to anhydrous ether and stirring evenly to form a dissolving solution; b3, adding the mixed fine powder to the dissolving solution and ultrasonically treating it for 30 minutes to obtain a matte enamel coating, the temperature of the ultrasonic treatment is 10°C, and the ultrasonic frequency is 80kHz;

[0032] Step 6, spraying aqueous ether onto the surface of the coated stainless steel substrate, and standing for 4 hours, and curing to obtain stainless steel matte enamel; the preparation method of the aqueous ether liquid includes: a1, putting anhydrous ether and distilled water into a reactor and stirring evenly, and performing low-temperature ultrasonic treatment for 30 minutes, standing to obtain a layered liquid, the volume ratio of the anhydrous ether to distilled water is 20:1, the stirring speed is 500r / min, the temperature of the low-temperature ultrasonic treatment is 10°C, the ultrasonic frequency is 90kHz; the standing temperature is 25°C; a2, extracting the ether liquid in the layered liquid to obtain an aqueous ether liquid, the extraction temperature is 10°C; the spraying amount of the spray is 10mL / cm 2 , the temperature is 10°C; the static temperature is 50°C; the curing time is 10°C and the temperature is 800°C.

[0033] The stainless steel matte enamel of the present embodiment showed no porcelain bursting after 20 impacts at 400°C in the high and low temperature impact test; no porcelain bursting occurred when impacted by a 1-meter steel ball; no fish scale explosion occurred after long-term placement and use; in the corrosion resistance test, the neutral salt spray test for 72 hours and the acid salt spray test for 24 hours both performed well without corrosion.

[0034] Example 3

[0035] A method for manufacturing stainless steel matte enamel, comprising the following steps:

[0036] Step 1, adding sodium bicarbonate and sodium hydroxide to distilled water and stirring evenly to form a dissolving solution, then immersing the stainless steel substrate in the dissolving solution for 40 minutes, taking it out and rinsing it and drying it to obtain a stainless steel substrate with a clean surface; the mass ratio of the sodium bicarbonate to the sodium hydroxide is 4:1.2, the pH of the dissolving solution is 8, the stirring speed is 200r / min, the immersion temperature is 40°C; the drying temperature is 110°C;

[0037] Step 2: spray a dilute acid solution on the clean surface of the stainless steel substrate, and keep it at a constant temperature for 3 hours, ultrasonically clean it with distilled water for 25 minutes, and dry it to obtain a pretreated stainless steel substrate; the dilute acid solution is a mixture of hydrochloric acid and sulfuric acid with a pH of 6, and the molar ratio of hydrochloric acid to sulfuric acid is 1:3, and the spray volume is 3mL / cm 2 The constant temperature is 4°C; the ultrasonic cleaning is performed at an ultrasonic frequency of 80kHz and a temperature of 70°C; the drying is performed in a nitrogen atmosphere at a temperature of 130°C;

[0038] Step 3, sandblasting the pretreated stainless steel substrate for 15 seconds, then placing the sandblasted stainless steel substrate in distilled water for ultrasonic treatment to remove surface impurities, drying and then soaking it in aqueous ether solution for 15 minutes, taking it out and drying it at low temperature to obtain the pretreated stainless steel substrate, the ultrasonic frequency of the ultrasonic treatment is 70kHz, the temperature is 25°C, and the drying temperature is 110°C; the preparation method of the aqueous ether solution comprises: a1, placing anhydrous ether and distilled water into a reactor and stirring evenly, and performing low-temperature ultrasonic treatment for 25 minutes, standing to obtain a layered liquid, the volume ratio of anhydrous ether to distilled water is 15:1, the stirring speed is 400r / min, the temperature of the low-temperature ultrasonic treatment is 8°C, the ultrasonic frequency is 80kHz; the standing temperature is 22°C; a2, extracting the ether liquid in the layered liquid to obtain an aqueous ether liquid, the extraction temperature is 8°C; the temperature of the low-temperature drying is 43°C;

[0039] Step 4: adding trimethoxysilane to ether to form a silane solution, and then spraying it onto the surface of the pre-treated stainless steel substrate, standing at low temperature for 3 hours, to obtain a pre-coated stainless steel substrate; the concentration of the trimethoxysilane in ether is 20 g / L, the spray temperature is 8 ° C, and the spray volume is 6 mL / cm 2 , the low temperature standing temperature is 25°C;

[0040] Step 5: Spray the matte enamel coating onto the pre-coated stainless steel substrate, depressurize and let stand for 3 hours to obtain a coated stainless steel substrate. The spray volume of the matte enamel coating is 8 mL / cm 2 , the temperature is 25°C; the pressure of the decompression and static state is 75% of the atmospheric pressure, and the temperature is 26°C; the mass ratio of the matte enamel is: 8 parts of aluminum isopropoxide, 5 parts of cobalt oxide, 7 parts of ethyl silicate, 12 parts of dimethoxydimethylsilane, 5 parts of kaolin, 2 parts of sodium fluorosilicate, 40 parts of matte glaze enamel powder, and 80 parts of anhydrous ether, and the matte glaze enamel powder comes from Hunan Noli New Materials Co., Ltd.; and the preparation method of the matte enamel coating comprises: b1, grinding and mixing cobalt oxide, kaolin, sodium fluorosilicate, and matte glaze enamel powder to obtain a mixed fine powder; b2, adding aluminum isopropoxide, ethyl silicate, and dimethyldimethoxysilane to anhydrous ether and stirring evenly to form a dissolving solution; b3, adding the mixed fine powder to the dissolving solution and ultrasonically treating it for 25 minutes to obtain a matte enamel coating, the temperature of the ultrasonic treatment is 8°C, and the ultrasonic frequency is 70kHz;

[0041] Step 6, spraying aqueous ether onto the surface of the coated stainless steel substrate, and standing for 3 hours, and curing to obtain stainless steel matte enamel; the preparation method of the aqueous ether liquid includes: a1, putting anhydrous ether and distilled water into a reactor and stirring evenly, and low-temperature ultrasonic treatment for 25 minutes, standing to obtain a layered liquid, the volume ratio of anhydrous ether and distilled water is 15:1, the stirring speed is 400r / min, the temperature of the low-temperature ultrasonic treatment is 8°C, the ultrasonic frequency is 80kHz; the standing temperature is 22°C; a2, extracting the ether liquid in the layered liquid to obtain an aqueous ether liquid, the extraction temperature is 8°C; the temperature of the low-temperature drying is 43°C; the spray volume of the spray is 8mL / cm 2 , temperature is 8°C; the standing temperature is 45°C; the curing time is 8°C and the temperature is 750°C.

[0042] The stainless steel matte enamel of the present embodiment showed no porcelain bursting after 20 impacts at 400°C in the high and low temperature impact test; no porcelain bursting occurred when impacted by a 1-meter steel ball; no fish scale explosion occurred after long-term placement and use; in the corrosion resistance test, the neutral salt spray test for 72 hours and the acid salt spray test for 24 hours both performed well without corrosion.

[0043] It is understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.

Claims

1. A method for manufacturing stainless steel matte enamel, characterized in that: The steps include: Step 1, adding sodium bicarbonate and sodium hydroxide into distilled water and stirring evenly to form a dissolving solution, then immersing the stainless steel substrate in the dissolving solution for 30-50 minutes, taking it out, rinsing it and drying it to obtain a stainless steel substrate with a clean surface; Step 2, spraying a dilute acid solution on the clean surface of the stainless steel substrate, and standing it at a constant temperature for 2-3 hours, ultrasonically cleaning it with distilled water for 20-30 minutes, and drying it to obtain a pretreated stainless steel substrate; Step 3, sandblasting the pretreated stainless steel substrate for 10-20s, then placing the sandblasted stainless steel substrate in distilled water for ultrasonic treatment to remove surface impurities, drying and soaking in aqueous ether solution for 10-20min, taking out and drying at low temperature to obtain the pretreated stainless steel substrate, wherein the ultrasonic frequency of the ultrasonic treatment is 60-80kHz, the temperature is 20-30°C, the drying temperature is 100-120°C; the temperature of the low-temperature drying is 40-45°C; Step 4, adding trimethoxysilane to ether to form a silane solution, which is then sprayed onto the surface of the pre-treated stainless steel substrate, and allowed to stand at low temperature for 2-3 hours to obtain a pre-coated stainless steel substrate; Step 5, spraying the matte enamel coating on the pre-coated stainless steel substrate, reducing the pressure and standing for 2-3 hours to obtain a coated stainless steel substrate; the mass ratio of the matte enamel is: 5-10 parts of aluminum isopropoxide, 3-6 parts of cobalt oxide, 5-8 parts of ethyl silicate, 8-15 parts of dimethoxydimethylsilane, 3-6 parts of kaolin, 1-3 parts of sodium fluorosilicate, 30-60 parts of matte glaze enamel powder, and 60-90 parts of anhydrous ether, and the matte glaze enamel powder comes from Hunan Noli New Materials Co., Ltd.; Step 6, spraying aqueous ether onto the surface of the coated stainless steel substrate, and standing for 2-4 hours to obtain stainless steel matte enamel after curing; The preparation method of the aqueous ether liquid comprises: a1, putting anhydrous ether and distilled water into a reaction kettle and stirring them evenly, performing low-temperature ultrasonic treatment for 20-30 minutes, and standing to obtain a layered liquid, wherein the volume ratio of the anhydrous ether and distilled water is 10-20:1, the stirring speed is 200-500r / min, the temperature of the low-temperature ultrasonic treatment is 5-10°C, the ultrasonic frequency is 70-90kHz; the standing temperature is 20-25°C; a2, extracting the ether liquid in the layered liquid to obtain an aqueous ether liquid, and the extraction temperature is 5-10°C.

2. The method for manufacturing stainless steel matte enamel according to claim 1, characterized in that: The mass ratio of sodium bicarbonate to sodium hydroxide in step 1 is 4:1-1.3, the pH of the dissolving solution is 8, the stirring speed is 100-300r / min, the immersion temperature is 30-50°C; and the drying temperature is 100-120°C.

3. The method for manufacturing stainless steel matte enamel according to claim 1, characterized in that: The dilute acid solution in step 2 is a mixture of hydrochloric acid and sulfuric acid with a pH of 6, and the molar ratio of hydrochloric acid to sulfuric acid is 1:3, and the spray volume is 2-4 mL / cm 2 The constant temperature standing temperature is 3-5°C.

4. The method for manufacturing stainless steel matte enamel according to claim 1, characterized in that: The ultrasonic cleaning in step 2 is performed at an ultrasonic frequency of 70-90 kHz and a temperature of 50-80° C.; the drying is performed under a nitrogen atmosphere at a temperature of 120-140° C.

5. The method for manufacturing stainless steel matte enamel according to claim 1, characterized in that: The concentration of trimethoxysilane in diethyl ether in step 4 is 10-30 g / L, the spray temperature is 5-10° C., and the spray volume is 4-8 mL / cm 2 The low temperature standing temperature is 20-30°C.

6. The method for manufacturing stainless steel matte enamel according to claim 1, characterized in that: The spray volume of the matte enamel paint in step 5 is 5-10 mL / cm 2 , the temperature is 20-30℃; the pressure of the decompression and static state is 70-80% of the atmospheric pressure, and the temperature is 20-30℃.

7. The method for manufacturing stainless steel matte enamel according to claim 1, characterized in that: The spray volume in step 6 is 5-10 mL / cm 2 , the temperature is 5-10°C; the standing temperature is 40-50°C; the curing time is 5-10°C, and the temperature is 700-800°C.