A casting release agent and its preparation method
By using a casting release agent prepared with components such as dichloromethane, the problems of unstable aluminum powder filler and high cost were solved, achieving a chemically stable, low-cost, and strongly adhesive release effect, thus improving the surface quality and drying efficiency of sand molds.
Patent Information
- Application Number
- CN202410306778.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-18
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-03-18
AI Technical Summary
Existing casting release agents use aluminum powder as a filler, which has problems such as unstable chemical properties, pollution of the construction environment, and high cost.
The casting release agent is made of components such as dichloromethane, solvent oil, silicate mineral powder, quartz powder, silicone oil, fumed silica, polystyrene, and polyvinyl butyral. After being evenly mixed by a disperser, solid powder is added to prevent the powder from clumping. After standing and venting, the material is discharged, forming a chemically stable and highly adhesive release agent.
It achieves cost reduction, improves the stability and adhesion of the release agent, ensures the surface quality of the sand mold, shortens the drying time, and provides excellent coating performance.
Smart Images

Figure CN118106440B_ABST
Abstract
Description
Technical Field
[0001] This invention specifically relates to a casting release agent and its preparation method. Background Technology
[0002] The information disclosed in this background section is intended only to enhance some understanding of the overall background of the invention and is not necessarily to be construed as an admission or in any way implying that the information constitutes prior art known to those skilled in the art.
[0003] Casting is the process of molten metal being poured into a mold of a specific shape, and after solidification, obtaining a casting with specific dimensions and properties. Molds are commonly used to create the cavities for pouring molten metal. Molten sand mixed with a binder is applied to the surface of a model with the shape of the casting. After the binder in the sand mold solidifies, the sand mold is detached from the model surface, resulting in a sand mold cavity with a shape opposite to the model. The mold can be reused multiple times. To reduce friction during demolding, minimize wear on the model, and achieve a high surface quality, a release agent is coated onto the mold surface.
[0004] Existing casting release agents use aluminum powder (aluminum silver paste) as filler, which has drawbacks such as easy reaction, unstable chemical properties, pollution of the construction environment, and high cost. Summary of the Invention
[0005] To address the above shortcomings, this invention provides a casting release agent that is chemically stable, dries quickly, has high strength, good coatability, and is low in cost.
[0006] Specifically, the present invention adopts the following technical solution: In a first aspect of the invention, a casting release agent is provided, which, by weight, is composed of the following components: 50-80 parts dichloromethane, 10-80 parts solvent oil, 17-40 parts silicate mineral powder and / or quartz powder, 1-2 parts magnesium aluminum silicate, 1-5 parts silicone oil, 0.5-2 parts silica, 1-2 parts polystyrene, 0.5-2 parts polyvinyl butyral, and 1-5 parts liquid paraffin.
[0007] In this invention, the solvent oil refers to a light oil that plays a role in dissolving, diluting, washing, and extracting certain substances in chemical production.
[0008] In one or more embodiments of the present invention, the solvent oil is 120# solvent oil, which is used to adjust the drying speed. Adding too much reduces the drying speed.
[0009] In this invention, the silicate mineral powder includes, but is not limited to, talc powder, pyrophyllite powder, mullite powder, mica powder, feldspar powder (including orthoclase powder, plagioclase powder, and parafeldspar powder), pyroxene powder, amphibole powder, wollastonite powder, kaolinite powder, chlorite powder, serpentine powder, and montmorillonite powder.
[0010] In one or more embodiments of the present invention, the silicate mineral powder is one or more of the following: talc powder, pyrophyllite powder, mullite powder, mica powder, feldspar powder, pyroxene powder, amphibole powder, wollastonite powder, kaolinite powder, chlorite powder, serpentine powder, and montmorillonite powder.
[0011] In one or more embodiments of the present invention, the silicone oil is methyl silicone oil, which is used to increase the lubrication effect of the release agent. Adding too much of it will slow down the drying speed.
[0012] In one or more embodiments of the present invention, the density of the polystyrene is 15~25 kg / m³. 3 It is used to provide bonding strength. Too high a proportion results in high filler adhesion strength but reduced release lubrication, while too low a proportion results in low filler adhesion and fewer uses of the release layer.
[0013] In one or more embodiments of the present invention, the viscosity of the polyvinyl butyral is 10-20 seconds, which is used to improve the suspension of the release agent, but if the content is too high, the drying speed will be slowed down.
[0014] In this invention, the liquid paraffin is used to enhance the lubrication effect of the release agent.
[0015] In one or more embodiments of the present invention, the casting release agent is made of the following components in parts by weight: 65 parts dichloromethane, 10 parts solvent oil, 15 parts silicate mineral powder, 3.5 parts quartz powder, 1 part magnesium aluminum silicate, 1 part silicone oil, 1 part silica, 1 part polystyrene, 0.5 parts polyvinyl butyral, and 1 part liquid paraffin.
[0016] In one or more embodiments of the present invention, the silicate mineral powder is one or more of talc powder, pyrophyllite powder, mullite powder, and mica powder. Talc powder is preferred.
[0017] In a second aspect of the invention, a method for preparing the casting release agent is provided, the method comprising the following steps: Step 1: Add dichloromethane, solvent oil, silicone oil, liquid paraffin, polystyrene, and polyvinyl butyral to a container and stir evenly using a disperser. Note that the dispersion speed should be controlled at 100-500 rpm and the mixture should be dispersed for 2-10 minutes. Step 2: Add solid powders - silicate mineral powder and / or quartz powder, magnesium aluminum silicate, and fumed silica. Disperse evenly, and add slowly to prevent the powder from clumping. Control the speed of the disperser at 100-500 rpm and disperse for 5-10 minutes. After even dispersion, reduce the speed, let stand to release the air, and then discharge the material.
[0018] Compared with the related technologies known to the inventors, one of the technical solutions of the present invention has the following beneficial effects: 1. Conventional casting release agents use aluminum powder as filler, which is expensive, costing over 200 million yuan per ton. Newly developed release agents use quartz powder and / or silicate mineral powder as fillers, including talc powder, mica powder, pyrophyllite powder, mullite powder, etc., which cost around 1,000 yuan per ton. Compared with aluminum powder, this can significantly reduce costs.
[0019] 2. In aluminum powder casting release agents, the aluminum powder used as a filler is chemically unstable and easily reacts with the solution, causing the release agent to fail. In contrast, the product of this invention is stable and will not undergo chemical reactions or become uneven even after prolonged storage.
[0020] 3. In conventional casting release agents, the fillers have low adhesion to the mold surface. After molding, aluminum powder transfers to the sand mold surface, causing the sand mold to not solidify and reducing its surface quality. In contrast, the product of this invention has high adhesion strength to the mold surface, making the sand mold easy to solidify and resulting in high surface quality.
[0021] 4. The casting release agent of this invention has a short drying time and excellent coating performance. Attached Figure Description
[0022] The accompanying drawings, which form part of this specification, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.
[0023] Figure 1 This is a disperser used in experiments.
[0024] Figure 2 The release agent that has failed due to the chemical reaction changes from silvery-white to golden-yellow.
[0025] Figure 3 The surface of the mold after applying release agent.
[0026] Figure 4 The release agent aluminum powder adheres to the surface of the sand mold, reducing the surface quality of the sand mold.
[0027] Figure 5 Polystyrene precipitates.
[0028] Figure 6 Comparative tests of release agents #1 to #4. Detailed Implementation
[0029] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.
[0030] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the exemplary embodiments of the present invention. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, and / or combinations thereof.
[0031] To enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below with reference to specific embodiments.
[0032] Example 1 Preparation of No. 4 casting release agent, according to parts by weight The composition includes 65 parts dichloromethane, 10 parts solvent oil, 15 parts silicate mineral powder, 3.5 parts quartz powder, 1 part magnesium aluminum silicate, 1 part silicone oil, 1 part silicate, 1 part polystyrene, 0.5 parts polyvinyl butyral, and 1 part liquid paraffin. The solvent oil is 120# solvent oil, the silicate mineral powder is talc, and the density of the polystyrene is 15-25 kg / m³. 3 The viscosity of polyvinyl butyral is 10-20 seconds.
[0033] A process for preparing a release agent includes the following steps: Step 1: Prepare the above-mentioned release agent; Step 2: Add dichloromethane, solvent oil, silicone oil, liquid paraffin, polystyrene, and polyvinyl butyral to a container. Use a disperser to mix thoroughly, ensuring the dispersion speed is controlled at 150 rpm for 5 minutes. Figure 1 .
[0034] Step 3: Add solid powders - talc, quartz powder, magnesium aluminum silicate, and silica. Disperse them evenly. When adding the materials, be careful to do so slowly to prevent the powders from clumping. Control the speed of the disperser at 250 rpm and disperse for 10 minutes. After dispersing evenly, reduce the speed, let it stand to release the air, and then discharge the material. Example 2
[0035] The ingredients are: 50 parts dichloromethane, 20 parts solvent oil, 23 parts silicate mineral powder, 2 parts magnesium aluminum silicate, 1 part silicone oil, 0.5 parts silicate black, 2 parts polystyrene, and 1 part liquid paraffin. The solvent oil is 120# solvent oil, the silicate mineral powder is talc, and the density of the polystyrene is 15-25 kg / m³. 3 The viscosity of polyvinyl butyral is 10-20 seconds.
[0036] The preparation process is the same as in Example 1. Example 3
[0037] The composition comprises 51.5 parts dichloromethane, 18 parts solvent oil, 18 parts talc, 2 parts quartz powder, 1.5 parts magnesium aluminum silicate, 1.5 parts silicone oil, 1 part silicate, 1.5 parts polystyrene, 1 part polyvinyl butyral, and 3 parts liquid paraffin. The solvent oil is 120# solvent oil, the silicate mineral powder is talc, and the density of the polystyrene is 15-25 kg / m³. 3 The viscosity of polyvinyl butyral is 10-20 seconds.
[0038] The preparation process is as described in Example 1. Example 4
[0039] The composition includes 65 parts dichloromethane, 10 parts solvent oil, 15 parts silicate mineral powder, 3.5 parts quartz powder, 1 part magnesium aluminum silicate, 1 part silicone oil, 1 part silicate, 1 part polystyrene, 0.5 parts polyvinyl butyral, and 1 part liquid paraffin. The solvent oil is 120# solvent oil, the silicate mineral powder is mica powder, and the density of the polystyrene is 15-25 kg / m³. 3 The viscosity of polyvinyl butyral is 10-20 seconds.
[0040] The preparation process is as described in Example 1. Example 5
[0041] The composition includes 65 parts dichloromethane, 10 parts solvent oil, 15 parts silicate mineral powder, 3.5 parts quartz powder, 1 part magnesium aluminum silicate, 1 part silicone oil, 1 part silicate, 1 part polystyrene, 0.5 parts polyvinyl butyral, and 1 part liquid paraffin. The solvent oil is 120# solvent oil, the silicate mineral powder is a 1:1 mixture of pyrophyllite powder and mullite powder, and the polystyrene has a density of 15-25 kg / m³. 3 The viscosity of polyvinyl butyral is 10-20 seconds.
[0042] The preparation process is as described in Example 1. Example 6
[0043] The composition includes 65 parts dichloromethane, 10 parts solvent oil, 15 parts silicate mineral powder, 3.5 parts quartz powder, 1 part magnesium aluminum silicate, 1 part silicone oil, 1 part silicate, 1 part polystyrene, 0.5 parts polyvinyl butyral, and 1 part liquid paraffin. The solvent oil is 120# solvent oil, the silicate mineral powder is kaolinite powder, and the density of the polystyrene is 15-25 kg / m³. 3 The viscosity of polyvinyl butyral is 10-20 seconds.
[0044] The preparation process is as described in Example 1.
[0045] Comparative Example 1: Preparation of Release Agent No. 1 An aluminum powder casting release agent is composed of the following raw materials in parts by weight: 80 parts dichloromethane, 8.5 parts 120# solvent oil, 8 parts aluminum powder, 1.5 parts magnesium aluminum silicate, 1.5 parts methyl silicone oil, and 1 part polystyrene.
[0046] The preparation method is as follows: Step 1: Add dichloromethane, 120# solvent oil, methyl silicone oil, and polystyrene to a container and stir evenly using a disperser. Note that the dispersion speed should be controlled at 100-500 rpm and the mixture should be dispersed for 2-10 minutes. Step 2: Add solid powder, aluminum powder and magnesium aluminum silicate are evenly dispersed. When adding materials, pay attention to the speed of slow addition to prevent the powder from clumping. Control the speed of the disperser at 100-500 rpm and disperse for 5-10 minutes. After even dispersion, reduce the speed, let stand to release the air and then discharge the material.
[0047] like Figure 2 As shown, during use, the aluminum powder used as a filler in the aluminum powder casting release agent is chemically unstable and easily reacts with the solution, causing the release agent to fail and change from silvery-white to golden-yellow. For example... Figure 3 Aluminum powder casting release agent is applied to the surface of the casting mold. For example... Figure 4 and Figure 6 In aluminum powder casting release agents, the filler has low adhesion to the mold surface. After molding, the aluminum powder is transferred to the sand mold surface, and the sand mold does not solidify, reducing the surface quality of the sand mold.
[0048] The difference between the preparation of the No. 2 release agent in Comparative Example 2 and Example 1 is that dichloromethane is replaced with a weight ratio of dichloromethane to methanol of 7:3.
[0049] When the weight ratio of dichloromethane to methanol is 7:3, reaching the azeotropic point can accelerate the evaporation rate of the solution. However, the addition of methanol reduces the solubility of polystyrene in the solution, causing polystyrene to aggregate and fail to dissolve into the system, thus acting as a binder. For example... Figure 5 and 6 As shown.
[0050] Comparative Example 3: Preparation of Release Agent #3 The difference from Example 1 is that polyvinyl butyral is not added.
[0051] Comparative Example 4 The difference from Example 1 is that the silica is replaced with ultrafine calcium sulfate.
[0052] Comparative Example 5 The difference from Example 1 is that: 3 parts polystyrene.
[0053] Excessive mixing ratio leads to high filler adhesion strength, reduced lubrication during demolding, and poor demolding effect.
[0054] Performance tests were conducted on the above-described embodiments and comparative products, and the results are shown in Table 1.
[0055] Adhesion strength (number of demolding cycles): Demolding tests were conducted by brushing the same material onto the same mold surface under the same conditions until sand adhered to the mold. The number of cycles was recorded.
[0056] Stability: Whether the product exhibits sedimentation or stratification when left to stand.
[0057] Drying time: the molding time of the casting release agent.
[0058] Table 1 Example Adhesion strength / (number of film peeling cycles) stability Drying time / minute Example 1 18 Stablize 10 Example 2 16 Stablize 15 Example 3 15 Stablize 12 Example 4 17 Stablize 10 Example 5 15 Stablize 10 Example 6 16 Stablize 10 Comparative Example 1 6 Unstable 12 Comparative Example 2 2 Unstable 28 Comparative Example 3 3 Unstable 10 Comparative Example 4 6 Unstable 12 Comparative Example 5 6 Unstable 15
Claims
1. A foundry release agent characterized by, It is made from the following components in parts by weight: 50-80 parts dichloromethane, 10-80 parts solvent oil, 17-40 parts silicate mineral powder and / or quartz powder, 1-2 parts magnesium aluminum silicate, 1-5 parts silicone oil, 0.5-2 parts silica, 1-2 parts polystyrene, 0.5-2 parts polyvinyl butyral, and 1-5 parts liquid paraffin. The solvent oil is 120# solvent oil; the silicate mineral powder is one or more of talc powder, pyrophyllite powder, mullite powder, mica powder; the silicone oil is methyl silicone oil; the density of polystyrene is 15-25 kg / m 3 ; the viscosity of polyvinyl butyral is 10-20 seconds.
2. The foundry release agent of claim 1 wherein, It is made from the following components in parts by weight: 65 parts dichloromethane, 10 parts solvent oil, 15 parts silicate mineral powder, 3.5 parts quartz powder, 1 part magnesium aluminum silicate, 1 part silicone oil, 1 part silica, 1 part polystyrene, 0.5 parts polyvinyl butyral, and 1 part liquid paraffin.
3. The method of producing a casting release agent as claimed in claim 1 or 2, characterized by, The method includes: Step 1: Add dichloromethane, solvent oil, silicone oil, liquid paraffin, polystyrene, and polyvinyl butyral to a container, stir evenly using a disperser, control the dispersion speed at 100-500 rpm, and disperse for 2-10 minutes; Step 2: Add solid powders - silicate mineral powder and / or quartz powder, magnesium aluminum silicate, and fumed silica. Disperse evenly, and add slowly to prevent the powder from clumping. Control the speed of the disperser at 100-500 rpm and disperse for 5-10 minutes. After even dispersion, reduce the speed, let stand to release the air, and then discharge the material.
Citation Information
Patent Citations
Mold releasing coating for centrifugal casting and painting method of mold releasing coating
CN105127364A
Environment-friendly release agent for precise casting and preparing technology for environment-friendly release agent
CN105945212A