A photovoltaic cell assembly welding, production method and product
By arranging cells and solder strips on a back panel with a flexible film and negative pressure, followed by laser welding and hot pressing, the method addresses hidden cracks and cold solder joints, achieving improved welding consistency and electrical performance in photovoltaic cell modules.
Patent Information
- Application Number
- CN202211474276.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-11-23
AI Technical Summary
The existing methods for producing photovoltaic cell modules result in hidden cracks and cold solder joints due to secondary handling and positioning of cell strings, and the use of rigid layers during laser welding leads to deformation and uneven pressure, causing further issues.
A method involving the arrangement of cells and solder strips on a back panel, covered by a flexible film with negative pressure, allowing laser welding through the film without a rigid layer above, and subsequent hot pressing with a sealing plate to form a solar cell module.
This approach reduces the risk of hidden cracks and cold solder joints, ensuring better welding consistency and electrical performance by eliminating rigid layer deformation and maintaining consistent tension, while allowing for efficient production with zero false welds.
Smart Images

Figure CN118106614B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor devices, and in particular to a welding method and a production method of a photovoltaic cell assembly, and a solar cell assembly. Background Art
[0002] At present, the production method of photovoltaic cell modules is usually to use infrared heating tubes to heat multiple cells through welding strips to form a cell string, and then move the cell string to the backplane, weld the multiple cell strings on the backplane, and then set a cover plate on the cell string to encapsulate the cell string. In this way of forming a cell module, moving the cell string to the backplane involves secondary movement of the cell string and positioning and moving it on the backplane. This kind of movement and handling can easily cause hidden cracks in the cells at the beginning and end of the cell string.
[0003] In order to solve the above problems, the battery cells and welding strips can be arranged on the back plate, and then the cover plate can be put on to weld them to avoid secondary handling and positioning of the battery string. After welding, they can be directly laminated to form a solar cell module. Usually, the cover plate includes a flexible layer and a rigid layer arranged on the battery cells and welding strips in sequence. The rigid layer provides downward pressure and presses the battery cells and welding strips through the flexible layer. Among them, the rigid layer and the flexible layer are transparent to the laser, so that the laser can pass through the two to weld the welding strips and battery cells. However, this welding method will inevitably cause some cold welding of some solder joints and hidden cracks in the battery. Summary of the invention
[0004] In view of this, the purpose of the present application is to provide a welding method, a production method and a photovoltaic cell assembly for a photovoltaic cell assembly, aiming to solve the problems of cold solder joints and hidden cracks in the prior art.
[0005] In one aspect, the present invention provides a method for welding a photovoltaic cell assembly, the method comprising:
[0006] Arrange the cells and solder strips on the back panel;
[0007] A flexible film is covered on the back panel where the battery cells and solder strips are arranged, and negative pressure is formed between the back panel and the flexible film.
[0008] Using laser to irradiate the connection portion between the battery cell and the welding strip through the flexible film or the back plate to weld the welding strip and the battery cell;
[0009] The flexible film or back plate is transparent to the laser, and the welding strip is used to realize the connection between different battery cells or battery strings.
[0010] Furthermore, in a method for welding a photovoltaic cell assembly of the present invention, a flexible film is covered on a back plate on which the cells and the welding strips are arranged, and a negative pressure is formed between the back plate and the flexible film.
[0011] The back plate on which the battery cells and the welding strips are arranged is arranged on a supporting device, and the size of the flexible film is larger than that of the back plate, so that the flexible film completely covers the back plate, and its edge covers the supporting device, so that a closed space is formed between the flexible film and the supporting device;
[0012] At least one first air suction channel is arranged on the supporting device, and the first air suction channel is arranged under the back plate, or a part of the first air suction channel is located under the back plate, and another part is located under the part of the flexible membrane beyond the back plate, and vacuum is drawn through the first air suction channel.
[0013] Furthermore, in a method for welding a photovoltaic cell assembly of the present invention, a flexible film is covered on a back plate on which the cells and the welding strips are arranged, and a negative pressure is formed between the back plate and the flexible film.
[0014] The back plate on which the battery cells and the welding strips are arranged is arranged on a supporting device, and the size of the flexible film is larger than that of the back plate, so that the flexible film completely covers the back plate, and its edge is fixed on the supporting device;
[0015] The vacuum is drawn through a third suction channel arranged on the flexible membrane.
[0016] Furthermore, in a welding method for a photovoltaic cell assembly of the present invention, the first exhaust channel is an exhaust hole, and vacuum is drawn through the exhaust hole.
[0017] Furthermore, in a welding method for a photovoltaic cell assembly of the present invention, the first exhaust channel includes a groove and an exhaust hole arranged in the groove, and vacuum is drawn through the exhaust hole.
[0018] Furthermore, in a welding method for a photovoltaic cell assembly of the present invention, one end of the groove is arranged below the back plate, and the other end is arranged outside the coverage of the back plate and within the coverage of the flexible film.
[0019] Furthermore, in a welding method of a photovoltaic cell assembly of the present invention, a portion of the flexible film that extends beyond the back plate is pressed down by a frame that is larger than the size of the back plate, wherein the frame is arranged outside the first exhaust channel.
[0020] Furthermore, in a welding method for a photovoltaic cell assembly of the present invention, a second exhaust channel is also provided on the supporting device, and the second exhaust channel is provided outside the coverage of the back panel, and the flexible membrane is pressed down by exhausting air through the second exhaust channel, and the second exhaust channel is provided outside the first exhaust channel.
[0021] Furthermore, in a welding method for a photovoltaic cell assembly of the present invention, the second exhaust channel is a groove arranged on the outer circumference of the back plate, and the exhaust hole is arranged in the groove.
[0022] Furthermore, a welding method for a photovoltaic cell assembly of the present invention also includes a step of flattening the flexible film during or after covering the flexible film on the backplane where the cells and welding strips are arranged, and before forming a negative pressure between the backplane and the flexible film.
[0023] Furthermore, in a welding method for a photovoltaic cell assembly of the present invention, the negative pressure range is -10 to -100 KPa.
[0024] Furthermore, in a method for welding a photovoltaic cell assembly of the present invention, the thickness of the flexible film is in the range of 0.2 to 3 mm.
[0025] Furthermore, in a welding method for a photovoltaic cell assembly of the present invention, the Shore hardness of the flexible film is 20-70.
[0026] Furthermore, in a welding method for a photovoltaic cell assembly of the present invention, the flexible film is at least one of the following materials: EVA, POE, polybutylene terephthalate, poly(hexamethylene terephthalamide)-co-hexamethylene sebacamide copolymer, COPA, silicone, polyvinylidene chloride-polyolefin blend, polyamide, thermoplastic polyolefin elastomer, modified high-density polyethylene PE, epoxy resin with a curing agent, and a composite resin, wherein the composite resin includes polyvinylidene chloride.
[0027] Furthermore, in a welding method for a photovoltaic cell assembly of the present invention, the flexible film is a multilayer film.
[0028] Furthermore, in a welding method for a photovoltaic cell assembly of the present invention, the backplane includes a first rigid layer and a first flexible layer arranged in sequence from bottom to top, the first rigid layer is photovoltaic glass, and the first flexible layer is a heat-sealing film.
[0029] Furthermore, in a welding method for a photovoltaic cell assembly of the present invention, the material of the first flexible layer is POE or EVA.
[0030] Furthermore, in a welding method for a photovoltaic cell assembly of the present invention, the flexible film is a heat-sealing film.
[0031] Furthermore, in a welding method for a photovoltaic cell assembly of the present invention, the flexible film is POE or EVA.
[0032] Furthermore, in a method for welding a photovoltaic cell assembly of the present invention, the cell sheet is coated with insulating glue, and the insulating glue is arranged outside the welding point area.
[0033] Furthermore, in a method for welding a photovoltaic cell assembly of the present invention, the laser is an infrared continuous laser.
[0034] Furthermore, in a method for welding a photovoltaic cell assembly of the present invention, the connection portion between the cell and the welding strip is located above the cell, and the welding strip includes an interconnection bar and a bus bar.
[0035] In another aspect, the present invention provides a method for producing a photovoltaic cell assembly, which further comprises removing the flexible film after the aforementioned method for welding the photovoltaic cell assembly;
[0036] sequentially arranging a second flexible layer and a sealing plate on the battery cell and the welding ribbon;
[0037] The step of thermocompression packaging the solar cell module;
[0038] Wherein, the melting temperature of the flexible film is not less than 150°C.
[0039] Furthermore, in a method for producing a photovoltaic cell assembly of the present invention, the sealing plate is photovoltaic glass, and the material of the second flexible layer is POE or EVA.
[0040] On the other hand, the present invention provides a method for producing a photovoltaic cell assembly, which, after the aforementioned method for welding the photovoltaic cell assembly, further comprises the steps of providing a sealing plate on the flexible film and performing hot pressing packaging on the solar cell assembly;
[0041] Wherein, the flexible film is a heat-sealing film, and the sealing plate is photovoltaic glass.
[0042] Furthermore, in a method for producing a photovoltaic cell assembly of the present invention, the flexible film is EVA or POE.
[0043] On the other hand, the present invention provides a photovoltaic cell assembly prepared by using the welding method or production method of the photovoltaic cell assembly.
[0044] There is a certain degree of vacuum between the flexible film and the back plate of the present invention, and no rigid layer is arranged above the flexible film. On the one hand, the flexible film can form a better contact with the back plate to achieve compression, and has a better welding effect. On the other hand, there is no rigid layer above the flexible film, which avoids the deformation of the rigid layer or the unevenness caused by the processing accuracy of the rigid layer during vacuuming, resulting in cold welding, and also avoids the deformation or unevenness of the rigid layer causing local pressure changes and hidden cracks in the battery cell. At the same time, the welding consistency of the welding point is better, the tension deviation of the welding belt is small, and the electrical performance of the photovoltaic cell module is better. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0046] Figure 1 A flow chart of a photovoltaic cell assembly welding method provided in an embodiment of the present application;
[0047] Figure 2 and Figure 3 A schematic diagram of the structure of a photovoltaic cell assembly in a photovoltaic cell assembly welding method provided in an embodiment of the present application;
[0048] Figures 4 to 10 A schematic diagram of the mechanism of laser processing a support table, a back plate and a flexible film in step S102 of a photovoltaic solar cell assembly welding method provided in an embodiment of the present application. DETAILED DESCRIPTION
[0049] In order to make the above-mentioned objects, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below with reference to the accompanying drawings.
[0050] In the following description, many specific details are set forth to facilitate a full understanding of the present application, but the present application may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present application. Therefore, the present application is not limited to the specific embodiments disclosed below.
[0051] Secondly, the present application is described in detail with reference to the schematic diagram. When describing the embodiments of the present application in detail, for the sake of convenience, the cross-sectional diagrams showing the device structure will not be partially enlarged according to the general scale, and the schematic diagrams are only examples, which should not limit the scope of protection of the present application. In addition, in actual production, the three-dimensional dimensions of length, width and depth should be included.
[0052] At present, a new welding method for solar cell modules is used to arrange cells and welding strips on the back panel. The welding strips are used to achieve the connection between different cells. Flexible layers and rigid layers are laid on the cells and welding strips in sequence.
[0053] There is a certain degree of vacuum between the flexible film and the back plate of the present invention, and no rigid layer is arranged above the flexible film. On the one hand, the flexible film can form a better contact with the back plate to achieve compression, and has a better welding effect. On the other hand, there is no rigid layer above the flexible film, which avoids the deformation of the rigid layer or the unevenness caused by the processing accuracy of the rigid layer during vacuuming, resulting in a change in the laser refractive index to produce a cold weld, and also avoids the deformation or unevenness of the rigid layer causing local pressure changes to cause cracks in the battery cell. The laser is used to irradiate the connecting part of the battery cell and the welding strip through the rigid layer and the flexible layer in turn to weld the welding strip and the battery cell. However, this welding method will inevitably cause some cold welds at some welding points and the problem of battery cracks.
[0054] Based on this, the present invention provides a welding method for a photovoltaic cell assembly, wherein cell sheets and welding strips are arranged on a back panel, and the welding strips are used to achieve connection between different cell sheets; a flexible film is provided on the cell sheets and the welding strips; a laser is used to irradiate the connecting portion of the cell sheets and the welding strips through the flexible film to weld the welding strips and the cell sheets; and the flexible film is transparent to the laser.
[0055] In the present invention, no rigid member for applying pressure to the back plate is arranged on the back plate.
[0056] Specifically, the negative pressure ranges from -10 to -100 KPa, more preferably from -30 to -70 KPa, or any range therebetween.
[0057] In order to better understand the technical solution and technical effects of the present application, specific embodiments will be described in detail below with reference to the accompanying drawings.
[0058] A method for welding a photovoltaic cell assembly is provided in the embodiment of the present application, see the attached Figure 1 The process diagram is as follows:
[0059] S101 arranges the cells and solder strips on the backplane 2, refer to Figure 2 and Figure 3 As a non-limiting embodiment, the back plate 2 includes a first rigid layer 22 and a first flexible layer 21 arranged in sequence, Figure 2 As shown, for the sake of convenience, a certain distance is made between the first rigid layer 22 and the first flexible layer 21 in the figure to form an exploded view of the battery assembly, but in fact the two are arranged in a close relationship. The first rigid layer 22 provides support and can also be used as a component backplane in the later packaging process. The first flexible layer 21 provides a buffer for the battery cell 31 and the welding strip to reduce the risk of hidden cracks, and can also be used as a hot pressing layer in the later packaging process.
[0060] In the embodiment of the present application, the first rigid layer 22 is configured to have strong mechanical strength to provide support for the first flexible layer 21 thereon. The material of the first rigid layer 22 can be glass, such as photovoltaic glass. The first flexible layer 21 is laid on the first rigid layer 22 to cover its surface. The first rigid layer 22 and the first flexible layer 21 can be placed on a laser processing support table, thereby facilitating subsequent laser welding of the battery assembly and reducing the number of movements.
[0061] The first flexible layer 21 is a heat-sealing film, and its melting temperature can be 50-150°C. The prior art generally uses EVA or POE. When welding the battery cell 31 and the welding strip, POE has a higher melting temperature than EVA, and is not easy to melt and adhere to the battery cell 31 when the welding temperature is high. Among them, photovoltaic POE has low water vapor permeability, excellent anti-PID performance, high insulation, fast cross-linking speed, high adhesion to materials such as glass, metal, and polymer backplane, and can maintain long-term adhesion, excellent UV resistance and high temperature and humidity resistance. The light transmittance is good, and the light transmittance at 1100nm-380nm is greater than 90%, which has little effect on laser welding and is very suitable for photovoltaic modules. The first flexible layer 21 has good hot pressing characteristics and can be used as a hot pressing layer in the subsequent packaging process.
[0062] The battery cells 31 and the solder strips are arranged on the first flexible layer 21. Figure 3 As shown, the welding strip is used to realize the connection between different battery cells 31. The battery cell 31 can be a solar cell unit or a half cell, so that the battery assembly is a solar cell assembly. The welding strip is used to realize the connection between adjacent battery cells 31. The position of the welding strip is aligned with the position to be welded of the battery cell 31. It can be located above the position to be welded of the battery cell 31, or it can be located below the position to be welded of the battery cell 31. The connection part between the battery cell 31 and the welding strip serves as the welding area.
[0063] The battery cell 31 can be a back contact battery, such as an IBC battery. The battery cell 31 can be arranged on the back plate 2 with the front side facing down. The electrodes (including the positive electrode and the negative electrode) of the battery cell 31 can be arranged on the back side of the battery 31, that is, arranged above the battery cell 31, and the connection part is located above the battery cell 31. Arranging the battery cell 31 and the welding strip on the first flexible layer 21 can be specifically as follows: first arranging the solar cell 31, and then placing one or more welding strips longitudinally or transversely on the main grid of the adjacent battery cell 31. The positive and negative electrodes of the adjacent battery cells 31 can be connected by the welding strip, so as to realize the series connection between the battery cells 31, and the positions of the positive and negative electrodes of the battery cell 31 can be used as the positions to be welded. The present invention is not limited to this. The battery cell 31 can also be other batteries. When arranging, a welding strip can be placed, then a battery cell 31, then another welding strip, and then another battery cell 31, until it is full. Adjacent battery cells 31 are connected by Z-shaped welding strips.
[0064] The welding strip described in this application includes an interconnection strip 32 and a bus bar 33. The bus bar 33 is a conductive connection component with a multi-layer laminated structure. The interconnection strip 32 is used to connect the battery cells 31 into a battery string. The bus bar 33 is used to achieve the connection between different battery strings. The number of welding strips is related to the number of battery cells 31 and the positional relationship between the welding strip and the battery cell 31. The number of welding strips meets the positive and negative pole connection requirements of the component battery. The welding strip is usually a flat strip. The shape of the welding strip perpendicular to its surface can be determined according to actual conditions, such as a circle, a polygon, etc. The polygon can be, for example, a rectangle, a triangle, etc.
[0065] The battery cell 31 and the welding strip can be transported by a manipulator, and the positions of the battery cell 31 and the welding strip on the first rigid layer 22 and the first flexible layer 21 can be predetermined. The battery cell 31 and the welding strip are placed at the specified position by controlling the displacement of the manipulator, so that the battery cell 31 and the welding strip are arranged sequentially on the first rigid layer 22 and the first flexible layer 21, and the battery cell 31 and the welding strip are laid. Compared with the secondary transport of first obtaining a battery string by welding and then placing the battery string on the backplane, the present invention reduces the number of transports and reduces the risk of hidden cracks in the battery cell 31. During the transport of the battery cell 31 and the welding strip, the position of the battery cell 31 and the welding strip on the backplane 2 can be positioned by CCD vision, which has high accuracy, reduces the number of movements of the battery cell 31 and the welding strip, and reduces the risk of hidden cracks generated during the grabbing and moving process of the battery cell 31.
[0066] S102, covering the back plate 2 with the battery cells 31 and the solder strips with the flexible film 1, and forming a negative pressure between the back plate and the flexible film, refer to Figures 4 to 10 shown.
[0067] A flexible film is covered on the back plate where the battery cells and the welding strips are arranged, and negative pressure is formed between the back plate 2 and the flexible film 1 so that the flexible film 1 is closely attached to the battery cells 31 and the welding strips.
[0068] Specifically, as mentioned above, the backplane where the battery cells 31 and the welding strips are arranged is set on the laser processing support table 4, and the flexible film 1 can be covered by manually laying it on the backplane where the battery cells and the welding strips are arranged; or the surface of the flexible film can be adsorbed by multiple manipulators with negative pressure adsorption devices set on the laser processing support table, and transferred to the backplane where the battery cells and the welding strips are arranged for covering, and then the manipulators are removed; or a lifting mechanism can be set on the laser processing support table, and a fixing device can be set on the edge of the flexible film, and it can be lowered by the lifting mechanism to cover the backplane where the battery cells and the welding strips are arranged. Preferably, it also includes the step of flattening the film during or after covering the flexible film, and the method of flattening it outwards or squeezing it outwards can be adopted. The present invention is not limited to this. As long as the flexible film 1 can be flatly covered on the backplane where the battery cells and the welding strips are arranged, it can be used.
[0069] Negative pressure is formed between the back plate 2 and the flexible film 1 so that the flexible film 1 is closely attached to the battery cell 31 and the welding strip, which can be achieved by the following method.
[0070] The size of the flexible film 1 is larger than that of the back plate 2, so that the flexible film 1 completely covers the back plate 2, and its edge covers the laser processing support table 4. In this arrangement, a relatively closed space is formed between the flexible film 1 and the laser processing support table 4. Figure 4 and Figure 5 , is a top view of the flexible film 1, the back plate 2 and the laser processing support platform 4. In order to make the relative positional relationship clearer, the battery cell 31 and the welding strip are omitted in the figure. Among them, the back plate 2 and the first exhaust channel 41 of the laser processing support platform 4 are both represented by dotted lines. Figure 4 and Figure 5 The size of the flexible film 1 is larger than that of the back plate 2, wherein the width of the flexible film 1 is larger than the width of the back plate 2, and the length is also larger than the length of the back plate 2. The portion of the flexible film 1 that exceeds the back plate 2 is covered on the laser processing support table 4. A first exhaust channel 41 is provided on the laser processing support table 4. The first exhaust channel 41 is used to draw a vacuum so that the flexible film is closely attached to the battery cell 31 and the welding strip. The first exhaust channel 41 is provided below the back plate 2 (see Figure 4 ), or the first exhaust channel 41 is arranged under the portion of the back plate 2 and the flexible membrane 1 extending beyond the back plate. The first exhaust channel 41 mentioned here is arranged under the portion of the back plate 2 and the flexible membrane 1 extending beyond the back plate, which means that one part of it is located under the back plate 2 and the other part is located under the portion of the flexible membrane 1 extending beyond the back plate.
[0071] It is understandable that the back plate 2 cannot be absolutely flat. The first exhaust channel 41 is arranged under the back plate 2, and vacuum can be achieved through the first exhaust channel 41. Preferably, the surface of the laser processing support table 4 can be arranged to have a larger roughness, or have grooves, so that vacuum can be achieved more quickly; or, the first exhaust channel 41 is arranged under the back plate 2 and the part of the flexible membrane 1 that extends beyond the back plate, and there is a space between the two, so that vacuum can be achieved more quickly.
[0072] Preferably, there are multiple first air extraction channels 41, which are circumferentially spaced apart under the back plate 2, or circumferentially spaced apart under the back plate 2 and the flexible membrane 1, and can be circumferentially arranged on one side, two sides, three sides or all four sides.
[0073] See also Figure 6 As a preferred practicable manner, the first air extraction channel 41 includes a groove 411 and an air extraction hole 412 disposed in the groove 411, and the negative pressure device extracts a vacuum through the air extraction hole 412. As mentioned above, the groove 411 can be entirely disposed under the back plate 2. Preferably, one end of the groove 411 is disposed under the back plate 1, and the other end is disposed outside the coverage of the back plate 1 and within the coverage of the flexible film 1.
[0074] As an implementable approach, see Figure 7 and Figure 8 A downward force is applied to the flexible membrane 1 through a frame 5 that is larger than the size of the back plate, so that the flexible membrane 1 and the laser processing support plate 4 are closed. It can be understood that the frame 5 needs to be arranged outside the first exhaust channel 41, and usually, its size is not larger than the size of the flexible membrane 1.
[0075] As another possible implementation, see Fig. 9 and Fig.10 , a second exhaust channel 6 is arranged on the laser processing support table, and the second exhaust channel 6 is arranged outside the coverage of the back plate and within the coverage of the flexible film. The second exhaust channel 6 is used to exhaust air and exert a downward force on the flexible film 1, so that it presses the laser processing support table 4, so that the flexible film 1 and the laser processing support table 4 are closed. Among them, the second exhaust channel 6 is preferably a rectangular groove, in which exhaust holes are arranged for exhaust. It can be understood that the second exhaust channel needs to be arranged outside the first exhaust channel 41. As another feasible method, the second exhaust channel 6 includes four exhaust holes, which are distributed around the back plate 2. In this embodiment, the closer the distance between the air holes, the shorter the time required for vacuuming, which helps to improve the processing efficiency.
[0076] The vacuuming method is not limited to this, and it can also be performed by vacuuming from above. For example, the back panel 2 on which the battery cells 31 and the welding strips are arranged is set on the laser processing support table 4, and the size of the flexible film 1 is larger than the size of the back panel 2, so that the flexible film 1 completely covers the back panel 2, and its edge covers the laser processing support table 4, and the edge of the flexible film 1 is fixed on the laser processing support table 4, and a relatively closed space is formed between the flexible film 1 and the laser processing support table 4, and vacuuming is performed through the third vacuuming channel set on the flexible film. At this time, the third vacuuming channel does not exceed the edge fixing position of the flexible film. The edge of the flexible film 1 can be fixed on the processing support table 4 by adopting a similar method. Figure 7 or Figure 8 The frame 5 is pressed down, or similar Fig. 9 or Fig.10 The third channel 6 is adsorbed.
[0077] No matter which of the above methods is used, closed vacuum can be achieved, so that the flexible film is tightly attached to the back plate where the battery cells and the welding strips are arranged. The back plate has a certain thickness, the flexible film has elasticity, the outer side of the flexible film is pressed tightly, and when the back plate is vacuumed, the flexible film is moved closer to the back plate, and the elasticity of the flexible film makes the flexible film fit well on the back plate.
[0078] Even if the back plate has a certain deformation during vacuuming, the elasticity of the flexible film can also be adaptively changed to achieve tight adhesion. Compared with the prior art with a cover plate, good welding can be achieved in a larger vacuum range and the risk of hidden cracks can be avoided. Compared with the prior art with a cover plate with a vacuum degree of -10 to -50 KPa, the method of the present invention can achieve good welding effects in the range of -10 to -100 KPa.
[0079] In the embodiment of the present application, the flexible film is transparent to the laser and does not affect the laser welding. The flexible film is elastic and has a suitable thickness, so that it can better fit the back plate when vacuuming.
[0080] In the embodiment of the present application, the thickness of the flexible film ranges from 0.2 to 3 mm, and the Shore hardness of the flexible film is 20-70, preferably 30-70, or an intermediate value thereof. When the thickness is too small, for example, less than 0.2 mm, the flexible film is more likely to deform and produce wrinkles, or pull the battery cell and the welding strip to cause positional displacement, resulting in poor welding effect. When the thickness is too large, for example, greater than 3 mm, it affects the transmittance of the laser, is not conducive to welding, and is not conducive to good side bonding to the backplane. The elasticity and thickness of the flexible film 1 also ensure that it has good deformation adaptability when vacuuming, and can better fit the backplane and the battery cell and welding strip thereon.
[0081] As a specific embodiment, the flexible film 1 may have a melting temperature higher than the welding temperature, for example, it is usually greater than 150°C, preferably greater than 200°C, greater than 220°C, more preferably greater than 250°C, greater than 350°C. Specifically, its melting temperature is higher than the welding temperature, so it will not melt during welding and adhere to the soldering tape. The welding temperature here is the laser welding temperature. Usually, this temperature is higher than the melting temperature of the soldering tape. When the material of the soldering tape is different from the material of the grid line of the battery cell 31, this temperature is higher than the low eutectic temperature. This temperature is selected by technicians in this technical field according to welding requirements. With such a setting, it is possible to avoid the flexible film 1 from adhering to the battery cell or the soldering tape during welding. When there are problems such as cold soldering, the flexible film 1 can be removed for repair.
[0082] As another specific implementation, the flexible film 1 can also be a heat-sealing film, for example, a material similar to the first flexible layer 21, whose melting temperature can be 50-150°C, and usually EVA or POE is used. Due to the method of the present invention, zero false solder joints and zero hidden cracks can be basically guaranteed, and the flexible film can be directly used as the material for subsequent hot pressing packaging, and hot pressing packaging can be directly added with a sealing plate, which is convenient and fast, and improves the production efficiency of the component.
[0083] Specifically, the material of the flexible film can be at least one of the following materials: POE, EVA, polybutylene terephthalate (PBT), poly(hexamethylene terephthalamide)-co-hexamethylene sebacamide copolymer (PA), COPA (PA6-66), silicone, polyvinylidene chloride (PVDC)-polyolefin blend, polyamide, thermoplastic polyolefin elastomer, modified high-density polyethylene (PE), epoxy resin with curing agent, composite resin, the composite resin includes polyvinylidene chloride (PVDC), and the composite resin also includes other high-temperature melting resin materials. Among them, polyamide has high polymerization crystallinity, modified high-density polyethylene can be a metal ion polymer, etc., and the curing agent of the epoxy resin can be any one of p-phenylenediamine, m-phenylenediamine, 4,4'-biphenylenediamine, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 2,2-bis(4-aminophenyl)propane and 2,2-bis(3-amino-4-hydroxyphenyl)propane.
[0084] The cycloaliphatic diamine, which is one of the precursors of polyamide with high polymerization crystallinity, is usually selected from bis(4-aminocyclohexyl)methane (PACM), 2,2-bis(4-aminocyclohexyl)propane, bis(4-amino-3-methylcyclohexyl)methane (MACM), 2,2-bis(4-amino-3-methylcyclohexyl)propane, bis(4-amino-3-ethylcyclohexyl)methane (EACM), bis(4-amino-3,5-dimethylcyclohexyl)methane (TMACM), isophoronediamine (5-amino-1,3,3-trimethylcyclohexanemethylamine), 1,3-diaminocyclohexane, 1,3-diaminomethylcyclohexane, 2,5- or 2,6-bis(aminomethyl)norbornane (DN), and 2,5- or 2,6-diaminonorbornane. Preference is given to using cycloaliphatic diamines PACM and alkyl-substituted bis(4-aminocyclohexyl)methane derivatives MACM, EACM and / or TMACM, which account for more than 80 mol % of all precursors.
[0085] Furthermore, the flexible film of the present invention is a single-layer structure, and the flexible film 1 may have a uniform melting temperature or an uneven melting temperature. When the flexible film 1 has a uniform melting temperature, it is understood that the melting temperature of the entire layer is higher than the welding temperature.
[0086] Alternatively, the flexible film may be a multi-layer structure. A second film layer is provided on a side of the flexible film 1 away from the battery cell 31 and the welding strip to improve the laser welding effect.
[0087] S103 , using laser to penetrate the flexible film 1 or the back plate 2 to irradiate the connection portion between the battery cell 31 and the welding ribbon, so as to weld the battery cell 31 and the welding ribbon.
[0088] In the embodiment of the present application, as a preferred implementation, laser is used to irradiate the connection part between the battery cell 31 and the welding strip through the flexible film 1. During the laser welding process, the laser welding process can be controlled by setting the laser parameters, and precise heating of the welding area can be achieved through laser welding. Compared with infrared heating tubes, laser welding will not affect areas outside the welding area, thereby reducing the impact on the performance of the battery assembly.
[0089] The laser can be an infrared continuous laser. The laser emitted by the laser is an infrared continuous laser. The laser parameters include spot size, laser defocus, laser power, light emission time, etc.
[0090] When the electrode of the battery cell 31 is located above the battery cell 31 , the temperature below the battery cell 31 is lower during welding, so the first flexible layer 21 is less likely to adhere to the battery cell 31 than the flexible film 1 during welding.
[0091] Of course, the laser can also be irradiated through the back plate 2 to achieve welding between the battery cell 31 and the welding strip.
[0092] It is understandable that the laser processing module can be arranged above the photovoltaic cell assembly to perform welding through the flexible film 1; the laser processing module can also be arranged below the photovoltaic cell assembly to perform welding through the back plate from below. The laser processing support platform 4 is designed to avoid certain positions to allow the laser to pass through.
[0093] Furthermore, a welding method for a photovoltaic cell assembly of the present invention further includes the step of applying insulating glue to the non-welding point portion of the cell before arranging the cell and the welding strip on the back panel in S101. Usually, the insulating glue is usually applied to the non-welding point portion of the cell. It can be seen that the portion to be welded is actually recessed relative to its surroundings. The welding method for a photovoltaic cell assembly of the present invention eliminates the rigid cover plate, and the elasticity of the flexible film enables it to adapt to this recess when vacuuming, thereby achieving a better fit for the portion to be welded. The welding method of the present invention has a better advantage for this type of welding.
[0094] It should be noted that, during the process S103, the aforementioned negative pressure is maintained.
[0095] When the laser is irradiated through the flexible film for laser welding, the aforementioned flexible film presses the battery cell and the welding strip to bring about a welding effect, and reduces the influence of laser refraction. Compared with the welding method in which a cover plate is set on the flexible film for welding, it has a great improvement, and it can basically achieve zero false welding and zero hidden cracks. In addition, it also maintains better welding consistency, which is specifically manifested in better consistency of welding strip tension, thereby ensuring better electrical performance of solar cell modules. The technical solution of the present invention of covering the flexible film on the back plate and maintaining negative pressure, because the flexible film presses the battery cell and the welding strip tightly, also helps to make the laser irradiate through the back plate for laser welding with better effect. The better the flatness and rigidity of the first rigid layer, the more it can reduce the influence of factors such as refraction, and the better the welding effect.
[0096] As a production method of a photovoltaic cell assembly, the method further includes the following steps: S104, removing the flexible film 1, and heat-pressing and packaging the solar cell assembly.
[0097] Specifically, after welding the welding ribbon and the battery cell 31, the flexible film 1 is removed. The melting temperature of the flexible film is not less than 150°C.
[0098] Then, a second flexible layer and a sealing plate are sequentially arranged on the welded cell 31 and the welding strip, and the solar cell assembly is hot-pressed and packaged. The sealing plate, the second flexible layer, the cell 31, the first flexible layer 21 and the first rigid layer 22 are hot-pressed to form a solar cell assembly.
[0099] It should be noted that before removing the flexible film 1 or during the process of removing the flexible film 1, a step of releasing the negative pressure is also included, such as backblowing or rolling up one side to break the vacuum. The present invention is not limited thereto, and other methods that can create a vacuum are also acceptable.
[0100] As mentioned above, the melting temperature of the first flexible layer and the second flexible layer is 50-150°C. Preferably, the first flexible layer and the second flexible layer are POE or EVA, which can be hot pressed. The first rigid layer 22 and the sealing plate are glass, preferably photovoltaic glass.
[0101] Furthermore, before encapsulating the solar cell assembly, a detection step of the cell 31 is also included. Specifically, the detection method can be at least one of visual detection, electroluminescence (EL) detection or photoluminescence (PL) detection. Among them, the visual detection can be detected by a CCD camera and / or a hidden crack detection device. After the detection, if there are problems such as cold solder joints and hidden cracks, it is necessary to repair.
[0102] Furthermore, it also includes a repair step for the detected defective products before packaging. The flexible film 1 on the upper layer of the battery cell 31 can be removed for repair work. Since the battery cell 31 and the soldering tape are not adhered to the flexible film 1, they are easy to be removed for repair. Specifically, the repair can use an electric soldering iron to heat the soldering tape in the welding area. After the soldering tape is melted by the heat, it is separated from the battery cell 31. Then the soldering tape and the battery cell 31 are removed, and a new soldering tape and battery cell 31 are added to complete the repair.
[0103] As another method for producing a photovoltaic cell assembly, the method further includes the following steps: S104, arranging a sealing plate on the flexible film, and hot-pressing and packaging the solar cell assembly.
[0104] After welding is completed, a sealing plate is arranged on the flexible film, and the solar cell assembly is packaged by hot pressing. The sealing plate, the flexible film, the battery sheet 31, the first flexible layer 21 and the first rigid layer 22 are hot pressed to form a solar cell assembly.
[0105] It should be noted that before the hot pressing packaging, a step of releasing the negative pressure is also included, such as back-blowing, or rolling up one side to break the vacuum. The present invention is not limited to this, and other methods that can create a vacuum are also acceptable.
[0106] As mentioned above, the melting temperature of the first flexible layer and the flexible film is 50-150°C. Preferably, the first flexible layer and the flexible film are POE or EVA, which can be hot pressed. The first rigid layer 22 and the sealing plate are glass, preferably photovoltaic glass.
[0107] On the other hand, the present invention further provides a photovoltaic cell assembly, which is prepared by using the above-mentioned photovoltaic cell assembly welding method or photovoltaic cell assembly production method.
[0108] As mentioned above, due to the use of the method of the present invention, zero cold solder joints and zero hidden cracks can be basically guaranteed, and the flexible film can be directly used as a material for hot pressing packaging, and hot pressing packaging can be directly added with a sealing plate, which is convenient and fast, and improves the production efficiency of the components.
[0109] The above is only a preferred implementation of the present application. Although the present application has been disclosed as a preferred embodiment, it is not intended to limit the present application. Any technician familiar with the art can use the above disclosed methods and technical contents to make many possible changes and modifications to the technical solution of the present application without departing from the scope of the technical solution of the present application, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present application without departing from the content of the technical solution of the present application still falls within the scope of protection of the technical solution of the present application.
Claims
1. A method for welding a photovoltaic cell assembly, characterized in that: The method comprises, Arrange the cells and solder strips on the back panel; The back plate on which the battery cells and the welding strips are arranged is arranged on a supporting device, and a flexible film is covered on the back plate on which the battery cells and the welding strips are arranged. The size of the flexible film is larger than the size of the back plate, so that the flexible film completely covers the back plate, and its edge covers the supporting device, and a negative pressure is formed between the back plate and the flexible film. Using laser to irradiate the connection portion between the battery cell and the welding strip through the flexible film or the back plate to weld the welding strip and the battery cell; Wherein, the flexible film or back plate is transparent to the laser, and the welding strip is used to realize the connection between different battery cells or battery strings; Wherein, no rigid layer is arranged above the flexible membrane.
2. A method for welding a photovoltaic cell assembly according to claim 1, characterized in that: At least one first air suction channel is arranged on the supporting device, and the first air suction channel is arranged under the back plate, or a part of the first air suction channel is located under the back plate, and another part is located under the part of the flexible membrane beyond the back plate, and vacuum is drawn through the first air suction channel.
3. The method for welding a photovoltaic cell assembly according to claim 1, characterized in that: The vacuum is drawn through a third suction channel arranged on the flexible membrane.
4. A method for welding a photovoltaic cell assembly according to claim 2, characterized in that: The first air extraction channel is an air extraction hole, and vacuum is extracted through the air extraction hole.
5. A method for welding a photovoltaic cell assembly according to claim 2, characterized in that: The first air extraction channel includes a groove and an air extraction hole arranged in the groove, and vacuum is extracted through the air extraction hole.
6. A method for welding a photovoltaic cell assembly according to claim 5, characterized in that: One end of the groove is arranged below the back plate, and the other end is arranged outside the coverage range of the back plate and within the coverage range of the flexible film.
7. A method for welding a photovoltaic cell assembly according to claim 2, characterized in that: The part of the flexible film that exceeds the back plate is pressed down by a frame that is larger than the size of the back plate, wherein the frame is arranged outside the first air suction channel.
8. A method for welding a photovoltaic cell assembly according to claim 2, characterized in that: A second air suction channel is also provided on the supporting device. The second air suction channel is provided outside the coverage of the back plate. Air is sucked through the second air suction channel to press the flexible membrane downward. The second air suction channel is provided outside the first air suction channel.
9. A method for welding a photovoltaic cell assembly according to claim 8, characterized in that: The second air extraction channel is a groove arranged on the outer circumference of the back plate, and an air extraction hole is arranged in the groove.
10. A method for welding a photovoltaic cell assembly according to claim 1, characterized in that: During or after the process of covering the flexible film on the back plate on which the battery cells and the welding strips are arranged, the step of flattening the flexible film is also included before negative pressure is formed between the back plate and the flexible film.
11. A method for welding a photovoltaic cell assembly according to any one of claims 1 to 10, characterized in that: The negative pressure range is -10~-100KPa.
12. A method for welding a photovoltaic cell assembly according to any one of claims 1 to 10, characterized in that: The thickness of the flexible film ranges from 0.2 to 3 mm.
13. A method for welding a photovoltaic cell assembly according to any one of claims 1 to 10, characterized in that: The flexible film has a Shore hardness of 20-70.
14. A method for welding a photovoltaic cell assembly according to any one of claims 1 to 10, characterized in that: The flexible film is at least one of the following materials: EVA, POE, polybutylene terephthalate, poly(hexamethylene terephthalamide-co-hexamethylene sebacamide) copolymer, COPA, silicone, polyvinylidene chloride-polyolefin blend, polyamide, thermoplastic polyolefin elastomer, modified high-density polyethylene PE, epoxy resin with curing agent, composite resin, and the composite resin includes polyvinylidene chloride.
15. A method for welding a photovoltaic cell assembly according to any one of claims 1 to 10, characterized in that: The flexible film is a multi-layer film.
16. A method for welding a photovoltaic cell assembly according to any one of claims 1 to 10, characterized in that: The back plate comprises a first rigid layer and a first flexible layer which are arranged in sequence from bottom to top, wherein the first rigid layer is photovoltaic glass, and the first flexible layer is a heat-sealing film.
17. A method for welding a photovoltaic cell assembly according to claim 16, characterized in that: The material of the first flexible layer is POE or EVA.
18. A method for welding a photovoltaic cell assembly according to claim 16, characterized in that: The flexible film is a heat-sealing film.
19. A method for welding a photovoltaic cell assembly according to claim 17, characterized in that: The flexible film is POE or EVA.
20. A photovoltaic cell assembly welding method according to any one of claims 1 to 10, characterized in that: The battery sheet is coated with insulating glue, and the insulating glue is arranged outside the welding point area.
21. A method for welding a photovoltaic cell assembly according to any one of claims 1 to 10, characterized in that: The laser is an infrared continuous laser.
22. A method for welding a photovoltaic cell assembly according to any one of claims 1 to 10, characterized in that: The connection portion between the battery cell and the welding strip is located above the battery cell, and the welding strip includes an interconnection bar and a bus bar.
23. A method for producing a photovoltaic cell assembly, characterized in that: After the welding method of the photovoltaic cell assembly according to any one of claims 1 to 22, the method further comprises removing the flexible film; sequentially arranging a second flexible layer and a sealing plate on the battery cell and the welding ribbon; The step of thermocompression packaging the solar cell module; Wherein, the melting temperature of the flexible film is not less than 150°C.
24. A method for producing a photovoltaic cell assembly according to claim 23, characterized in that: The sealing plate is photovoltaic glass, and the material of the second flexible layer is POE or EVA.
25. A method for producing a photovoltaic cell assembly, characterized in that: After the photovoltaic cell assembly welding method as claimed in any one of claims 1 to 22, it also includes the step of arranging a sealing plate on the flexible film and performing hot pressing packaging on the solar cell assembly; Wherein, the flexible film is a heat-sealing film, and the sealing plate is photovoltaic glass.
26. A method for producing a photovoltaic cell assembly according to claim 25, characterized in that: The flexible film is EVA or POE.
27. A photovoltaic cell assembly, prepared by the photovoltaic cell assembly welding method described in any one of claims 1 to 22, or the photovoltaic cell assembly production method described in any one of claims 23 to 26.
Citation Information
Patent Citations
Attaching structure for laser welding of solar cell module and welding equipment
CN217859343U