A low water absorption cast film and preparation method thereof

By adopting ABC three-layer structure and electron beam surface irradiation technology in the casting film, the problems of high water vapor transmission and poor weather resistance of the EVA film are solved, and casting films with low water absorption and high water vapor barrier properties are achieved. Improve the power generation efficiency and stability of photovoltaic modules.

CN118124225BActive Publication Date: 2024-11-08HEBEI HYDE PLASTIC IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410099675.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-24
Publication Date
2024-11-08
Estimated Expiration
2044-01-24

AI Technical Summary

Technical Problem

The EVA film used in existing photovoltaic modules has high water vapor transmission and poor weather resistance, so it cannot work efficiently in high humidity environments for a long time. The existing improved methods such as reducing the vinyl acetate content or adding water absorbents have limited effects, which cannot effectively improve the casting. Water vapor barrier properties of the membrane.

Method used

Using a low-water absorption casting film with three-layer structure of ABC, ethylene-octene copolymer grafts are added to the A and C layers to improve the bonding performance, and refractive index regulators are added to the B and C layers to enhance light refractive and achieve overall cross-linking through electron beam surface irradiation to form a cast film with low water absorption and high water vapor barrier properties.

Benefits of technology

It improves the bonding performance of the cast film and glass and the water vapor barrier performance, enhances the light capture capability, improves the power generation power and anti-aging performance of photovoltaic modules, and is suitable for long-term use in high humidity environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a low water absorption cast film and a preparation method thereof, belonging to the technical field of cast films. The main points of the technical scheme are that the cast film comprises an ABC three-layer structure; the A layer is composed of the following raw materials by weight: 50-95 parts of ethylene-octene copolymer resin, 0.1-5 parts of silicon dioxide, 5-50 parts of ethylene-octene copolymer grafted material, and 0.1-1.1 parts of composite anti-aging additive; the B layer is composed of the following raw materials: 50-95 parts of ethylene-octene copolymer resin, 0.1-8 parts of silicon dioxide, and a refractive index The C layer is composed of the following raw materials: 50-95 parts of ethylene-octene copolymer resin, 0.1-10 parts of silicon dioxide, 5-50 parts of ethylene-octene copolymer grafted material, 6-10 parts of refractive index regulator, and 0.1-1.1 parts of composite anti-aging additive; the ethylene-octene copolymer grafted material in the A layer and the C layer is an ethylene-octene copolymer grafted coupling agent, which achieves the effect of reducing the water absorption of the cast film while ensuring the light transmittance of the cast film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of cast film, in particular to a cast film with low water absorption and a preparation method thereof Background Art

[0002] Conventional crystalline silicon solar cell modules are usually made of photovoltaic glass, cast film, cell, cast film and backplane arranged in order from top to bottom through vacuum lamination. The role of cast film in photovoltaic modules is to bond photovoltaic glass, cell and backplane together, and at the same time protect the cell and isolate the air. It is one of the key materials of photovoltaic modules. At present, the packaging material of photovoltaic modules mainly adopts EVA film, but the molecular structure of EVA material itself determines that EVA film has shortcomings such as high water vapor permeability and poor weather resistance. Therefore, in the case of high humidity in the working environment, cast film with lower water vapor permeability is needed to ensure the long-term and efficient operation of photovoltaic modules.

[0003] At present, the methods to solve the relatively poor water vapor barrier performance of EVA film are: (1) reducing the content of vinyl acetate (VA) in the matrix resin EVA. As the proportion of polar functional groups decreases, the water vapor barrier property of the EVA film can be increased accordingly, but it will lead to the problem of reduced light transmittance, which is not conducive to the increase of photovoltaic cell power generation; (2) not using polar monomer copolymers as matrix resins. For example, in the existing patents CN106752997A and CN102863916A, metallocene-catalyzed ethylene and α-olefin monomers such as butene, pentene, octene, etc. are used as polymers for encapsulation. Since there are no unsaturated bonds in the molecular chain, the weather resistance is poor. The water barrier properties are significantly better than those of EVA film, but the adhesion between the film and glass obtained by this improvement is too poor. (3) Adding a water absorbent to the cast film to slow down the diffusion of water vapor in the cast film by physical adsorption or chemical reaction. For example, the existing patent CN103756579A adds an ion polymer, and the patent CN104962216A adds dicyclohexylcarbodiimide and 1-ethyl-(3-dimethylaminopropyl)carbodiimide. However, this method loses its water barrier effect when the water absorbent is saturated or completely reacts with water. Therefore, the effect of improving the water barrier performance of the cast film is relatively limited, and it cannot guarantee the long-term use of photovoltaic modules.

[0004] Therefore, it is necessary to develop a cast film with low water absorption to ensure the long-term and efficient operation of photovoltaic modules. Summary of the invention

[0005] In view of the above-mentioned prior art, the present invention provides a low water absorption cast film and a preparation method thereof, which reduces the water absorption of the cast film and improves the water vapor barrier performance of the cast film on the basis of ensuring the light transmittance of the cast film.

[0006] The first aspect of the present invention provides a low water absorption cast film, which adopts the following technical solution:

[0007] A low water absorption cast film, the cast film comprising an ABC three-layer structure;

[0008] The A layer is composed of the following raw materials in parts by weight: 50-95 parts of ethylene-octene copolymer resin, 0.1-5 parts of silicon dioxide, 5-50 parts of ethylene-octene copolymer grafted material, and 0.1-1.1 parts of composite anti-aging additive;

[0009] The B layer is composed of the following raw materials in parts by weight: 50-95 parts of ethylene-octene copolymer resin, 0.1-8 parts of silicon dioxide, 0.5-5 parts of refractive index regulator, and 0.1-1.1 parts of composite anti-aging additive;

[0010] The C layer is composed of the following raw materials in parts by weight: 50-95 parts of ethylene-octene copolymer resin, 0.1-10 parts of silicon dioxide, 5-50 parts of ethylene-octene copolymer grafted material, 6-10 parts of refractive index regulator, and 0.1-1.1 parts of composite anti-aging additive;

[0011] The ethylene-octene copolymer grafted material in the A layer and the C layer is an ethylene-octene copolymer grafted coupling agent.

[0012] And the layer refractive index ratio of the ABC three-layer structure is 1:1.001-1.02:1.021-1.05.

[0013] Preferably, the ethylene-octene copolymer graft material is prepared by the following method: 100 parts of ethylene-octene copolymer, 0.1-0.3 parts of initiator and 0.1-10 parts of oligomer coupling agent are fully mixed and melt-extruded, and the material is cut underwater and vacuum-dried to obtain an ethylene-octene copolymer graft material with a grafting rate of 1-5%; wherein the melt index of the ethylene-octene copolymer is 1-15g / 10min (190°C, 2.16kg).

[0014] Preferably, the oligomer coupling agent is selected from one or more of methacryloxysilane oligomer, 2-methoxyethoxysilane oligomer, methoxysilane oligomer, ethoxysilane oligomer, epoxysilane oligomer, vinylmethoxysilane oligomer, vinylepoxysilane oligomer, vinylalkoxysilane oligomer, and acrylalkoxysilane oligomer; the initiator is one or more of isopropylbenzene hydroperoxide, tert-butyl hydroperoxide, tert-butyl perbenzoate, tert-butyl pervalerate, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, and the like.

[0015] Preferably, the refractive index regulator of the B layer and the C layer is one or more of low-density polyethylene, high-density polyethylene, linear low-density polyethylene, and metallocene polyethylene resin, and the melt index of the low-density polyethylene, high-density polyethylene, linear low-density polyethylene, and metallocene polyethylene resin is 15-50g / 10min (190°C, 2.16kg).

[0016] Preferably, the thickness of the A layer and the C layer is 5-15 μm, and the thickness of the B layer is 200-600 μm.

[0017] Preferably, the composite anti-aging aid comprises an antioxidant, an ultraviolet light absorber and a light stabilizer in a weight ratio of (0.1-0.3):(0.1-0.5):(0.1-0.5).

[0018] Preferably, the antioxidant is one or more of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, n-octadecyl β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, triethylene glycol bis[β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate], tetrakis(2,4-di-tert-butyl-4,4'-biphenyl)bisphosphite, and tris[2.4-di-tert-butylphenyl]phosphite.

[0019] Preferably, the ultraviolet light absorber is one or more of 2-hydroxy-4-n-octyloxybenzophenone, 2-(2'-hydroxy-5'-octylphenyl)-benzotriazole, 2-[2,4-bis(2,4-xylyl)-2-(1,3,5-triazine)5-octyloxyphenol, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate, 2,2,6,6-tetramethyl-4-piperidinyl stearate, salicylic acid, 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone, and 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-hexyloxy-phenol.

[0020] Preferably, the light stabilizer is one or more of 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol, bis(2,2,6,6,-tetramethyl-4-piperidinyl) sebacate, poly(4-hydroxyethyl-2,2,6,6-tetramethyl-1-piperidinethanol) succinate, and poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-[(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediol[(2,2,6,6-tetramethyl-4-piperidinyl)imino]}.

[0021] The second aspect of the present invention provides a method for preparing a low water absorption cast film, comprising the following steps: mixing the three layers of raw materials A, B, and C respectively and extruding them at a temperature of 140-190°C, then casting and cooling to shape, using an energy emission device with a voltage of 200-400kv and an irradiation crosslinking dosage of 10-60KGY to irradiate the surface with an electron beam, wherein the distance between the energy emission device and the cast film is 50-150mm, to form a low water absorption cast film with an overall crosslinking degree of 5-30%.

[0022] In summary, the present invention has the following beneficial effects:

[0023] 1. The cast film obtained by the present invention is composed of three layers of ABC, and ethylene-octene copolymer grafted materials are added to the A layer and the C layer, so that the surface film of the cast film contains a small amount of polar groups, thereby improving the bonding performance between the cast film and the glass, while also ensuring that the overall water absorption rate of the cast film is relatively low, improving the water vapor barrier performance of the cast film, and making the cast film suitable for photovoltaic cells such as HJT and perovskite that have high requirements for water vapor barrier; in addition, the thickness of the A layer and the C layer is 5-15μm, and the thickness of the B layer is 200-600μm, which can effectively ensure the bonding between the cast film and the battery cell, thereby improving the protective effect of the cast film on the battery cell, but when the total thickness of the cast film changes, it will not affect the barrier performance of the cast film and the power generation power of the battery cell.

[0024] 2. The cast film of the present invention is composed of three layers, A, B, and C, and a refractive index regulator is added to the B layer and the C layer. By controlling the content of silicon dioxide in each layer and the content of the refractive index regulator in the B layer and the C layer, the refractive index of the three layers A, B, and C increases successively, and the refractive ability of each layer to light gradually increases, so that the incident sunlight can reach the battery cell as much as possible after refraction by the three layers, and be absorbed and utilized by the battery cell, achieving the purpose of trapping light, improving the light capture ability of the cast film, reducing the possibility of light escaping from the component, and improving the utilization rate of the battery cell to the incident sunlight, thereby improving the power generation of the photovoltaic module. In addition, the coordinated use of the raw materials of the three layers A, B, and C can effectively maintain the anti-aging performance of the film.

[0025] 3. After the ethylene-octene copolymer is pre-crosslinked with an oligomer coupling agent to form an ethylene-octene copolymer graft material with a grafting rate of 1-5%, the integrity of the A layer and the C layer during the component lamination process can be controlled to ensure the dimensional stability of the cast film. At the same time, the cast film can be evenly bonded to the photovoltaic glass and battery cell to prevent delamination and improve the creep resistance of the cast film. Implementation

[0026] The present invention is further described in detail below with reference to the embodiments.

[0027] The antioxidants in the A layer, B layer and C layer of the embodiment of the present application can be selected as a combination of one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, triethylene glycol bis[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate], tetrakis(2,4-di-tert-butyl-4,4'-biphenyl)bisphosphite and tris[2.4-di-tert-butylphenyl]phosphite, but the final results are basically the same, so the antioxidants in the A layer, B layer and C layer of the embodiment of the present application are all selected as tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol ester, CAS No. 6683-19-8.

[0028] In the embodiment of the present application, the ultraviolet light absorber in the A layer, the B layer, and the C layer can be selected as a combination of one or more of 2-hydroxy-4-n-octyloxybenzophenone, 2-(2'-hydroxy-5'-octylphenyl)-benzotriazole, 2-[2,4-bis(2,4-xylyl)-2-(1,3,5-triazine)5-octyloxyphenol, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate, 2,2,6,6-tetramethyl-4-piperidinyl stearate, salicylic acid, 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone, 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-hexyloxy-phenol, but the final result is basically the same, so the ultraviolet light absorber in the A layer, the B layer, and the C layer in the embodiment of the present application is selected as 2-hydroxy-4-n-octyloxybenzophenone, CAS No. 1843-05-6.

[0029] The light stabilizers in the A layer, B layer, and C layer of the present invention can be selected from 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol, bis(2,2,6,6,-tetramethyl-4-piperidinyl) sebacate, poly(4-hydroxyethyl-2,2,6,6-tetramethyl-1-piperidinethanol) succinate, poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4- [(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediol [(2,2,6,6-tetramethyl-4-piperidinyl)imino]} or a combination of several thereof, but the final result is basically the same, so the light stabilizers of layer A, layer B, and layer C in the embodiment of the present application are all selected as 2-(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol, CAS No. 23328-53-2.

[0030] In the embodiment of the present application, the refractive index regulator in layer B and layer C can be selected as a combination of one or more of low-density polyethylene, high-density polyethylene, linear low-density polyethylene, and metallocene polyethylene resin, but the final results achieved are basically the same, so in the embodiment of the present application, a low-density polyethylene with a melt index of 15-50g / 10min (190°C, 2.16kg) is selected.

[0031] Preparation Example 1 The preparation method of ethylene-octene copolymer grafted material is as follows: a twin-screw extruder with a length-to-diameter ratio of 65 is selected, 100 kg of ethylene-octene copolymer with a melt index of 1 g / 10 min (190°C, 2.16 kg), 0.1 kg of isopropylbenzene hydroperoxide, and 0.1 kg of methacryloyloxysilane oligomer are added into the extruder and mixed, and then melt-extruded at 100-160°C, and then the material is cut underwater and vacuum-dried after exiting the die to obtain an ethylene-octene copolymer grafted material with a grafting rate of 1%, which is then sealed and stored for later use.

[0032] Preparation Example 2 The preparation method of ethylene-octene copolymer grafted material is as follows: select a twin-screw extruder with a length-to-diameter ratio of 65, add 100kg of ethylene-octene copolymer with a melt index of 15g / 10min (190℃, 2.16kg), 0.3kg of tert-butyl hydroperoxide, and 10kg of methoxysilane oligomer into the extruder, mix, and melt-extrude at 100-160℃, cut underwater and vacuum dry after exiting the die to obtain ethylene-octene copolymer grafted material with a grafting rate of 5%, and then seal and store for later use. Example 1

[0033] A method for preparing a low water absorption cast film comprises the following steps:

[0034] 50 kg of ethylene-octene copolymer resin, 0.1 kg of silicon dioxide, 5 kg of ethylene-octene copolymer grafted material obtained in Preparation Example 1, and 0.1 kg of composite anti-aging aid in layer A are uniformly mixed to obtain mixture A, wherein the composite anti-aging aid comprises tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid] pentaerythritol ester, 2-hydroxy-4-n-octyloxybenzophenone and 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol in a weight ratio of 0.1:0.5:0.1, wherein the amount of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid] pentaerythritol ester is 0.014 kg, the amount of 2-hydroxy-4-n-octyloxybenzophenone is 0.072 kg, and the amount of 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol is 0.014 kg;

[0035] 50 kg of ethylene-octene copolymer resin, 0.1 kg of silicon dioxide, 0.5 kg of low-density polyethylene with a melt index of 15 g / 10 min (190°C, 2.16 kg), and 0.1 kg of a composite anti-aging additive in layer B are uniformly mixed to obtain a mixture B, wherein the composite anti-aging additive includes pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2-hydroxy- 4-n-octyloxybenzophenone and 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol, wherein the amount of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate is 0.014 kg, the amount of 2-hydroxy-4-n-octyloxybenzophenone is 0.072 kg, and the amount of 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol is 0.014 kg;

[0036] 50 kg of ethylene-octene copolymer resin, 0.1 kg of silicon dioxide, 5 kg of ethylene-octene copolymer grafted material obtained in Preparation Example 1, 6 kg of low-density polyethylene with a melt index of 15 g / 10 min (190° C., 2.16 kg), and 0.1 kg of a composite anti-aging additive in layer C are uniformly mixed to obtain a mixture C, wherein the composite anti-aging additive includes tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid] Pentaerythritol ester, 2-hydroxy-4-n-octyloxybenzophenone and 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol, wherein the amount of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate is 0.014kg, the amount of 2-hydroxy-4-n-octyloxybenzophenone is 0.072kg, and the amount of 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol is 0.014kg;

[0037] Then they are poured into three hoppers of the extruder respectively, and after extrusion at a temperature of 140°C, layer A, layer B and layer C are formed in sequence, and layer A, layer B and layer C are each surfaced in the extrudate with distinct interfaces, and the layer refractive index ratio of layers A, B and C is 1:1.001:1.021. Then, the film is cast and cooled to shape, so that the thickness of layer A of the cast film is 5μm, the thickness of layer B is 200μm, and the thickness of layer C is 5μm. An energy emission device with a voltage of 200kv and an irradiation cross-linking dosage of 10kGY is used for electron beam surface irradiation to form a low water absorption cast film with an overall cross-linking degree of 5%, and the distance between the energy emission device and the cast film is 50mm. Example 2

[0038] A method for preparing a low water absorption cast film comprises the following steps:

[0039] 75 kg of ethylene-octene copolymer resin, 1 kg of silicon dioxide, 20 kg of ethylene-octene copolymer grafted material obtained in Preparation Example 1, and 0.5 kg of composite anti-aging aid in layer A are uniformly mixed to obtain mixture A, wherein the composite anti-aging aid comprises tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid] pentaerythritol ester, 2-hydroxy-4-n-octyloxybenzophenone and 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol in a weight ratio of 0.3:0.1:0.5, wherein the amount of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid] pentaerythritol ester is 0.17 kg, the amount of 2-hydroxy-4-n-octyloxybenzophenone is 0.06 kg, and the amount of 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol is 0.27 kg;

[0040] 70 kg of ethylene-octene copolymer resin, 2 kg of silicon dioxide, 1.5 kg of low-density polyethylene with a melt index of 20 g / 10 min (190 ° C, 2.16 kg), and 0.6 kg of composite anti-aging additives in layer B are uniformly mixed to obtain a mixture B, wherein the composite anti-aging additive includes pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2-hydroxy -4-n-octyloxybenzophenone and 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol, wherein the amount of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate is 0.2kg, the amount of 2-hydroxy-4-n-octyloxybenzophenone is 0.07kg, and the amount of 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol is 0.33kg;

[0041] 75 kg of ethylene-octene copolymer resin, 4 kg of silicon dioxide, 20 kg of ethylene-octene copolymer grafted material obtained in Preparation Example 1, 8 kg of low-density polyethylene with a melt index of 20 g / 10 min (190° C., 2.16 kg), and 0.6 kg of composite anti-aging additive in layer C are uniformly mixed to obtain a mixture C, wherein the composite anti-aging additive includes tetra[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid in a weight ratio of 0.3:0.1:0.5 ] pentaerythritol ester, 2-hydroxy-4-n-octyloxybenzophenone and 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol, wherein the amount of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate is 0.2kg, the amount of 2-hydroxy-4-n-octyloxybenzophenone is 0.07kg, and the amount of 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol is 0.33kg;

[0042] Then they are poured into three hoppers of the extruder respectively, and after extrusion at a temperature of 150°C, layer A, layer B and layer C are formed in sequence, and layer A, layer B and layer C are each surfaced in the extrudate with distinct interfaces, and the layer refractive index ratio of layers A, B and C is 1:1.009:1.028. Then, the film is cast and cooled to shape, so that the thickness of layer A of the cast film is 7μm, the thickness of layer B is 435μm, and the thickness of layer C is 8μm. An energy emission device with a voltage of 200kv and an irradiation cross-linking dosage of 10kGY is used for electron beam surface irradiation to form a low water absorption cast film with an overall cross-linking degree of 5%, and the distance between the energy emission device and the cast film is 50mm. Example 3

[0043] A method for preparing a low water absorption cast film comprises the following steps:

[0044] 85 kg of ethylene-octene copolymer resin, 3 kg of silicon dioxide, 35 kg of ethylene-octene copolymer grafted material obtained in Preparation Example 1, and 1.1 kg of composite anti-aging aid in layer A are uniformly mixed to obtain mixture A, wherein the composite anti-aging aid comprises tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid] pentaerythritol ester, 2-hydroxy-4-n-octyloxybenzophenone and 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol in a weight ratio of 0.3:0.1:0.5, wherein the amount of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid] pentaerythritol ester is 0.37 kg, the amount of 2-hydroxy-4-n-octyloxybenzophenone is 0.12 kg, and the amount of 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol is 0.61 kg;

[0045] 85 kg of ethylene-octene copolymer resin, 5 kg of silicon dioxide, 3 kg of low-density polyethylene with a melt index of 30 g / 10 min (190°C, 2.16 kg), and 1.1 kg of composite anti-aging additives in layer B are uniformly mixed to obtain a mixture B, wherein the composite anti-aging additive includes pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2-hydroxy- 4-n-octyloxybenzophenone and 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol, wherein the amount of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate is 0.37 kg, the amount of 2-hydroxy-4-n-octyloxybenzophenone is 0.12 kg, and the amount of 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol is 0.61 kg;

[0046] 85 kg of ethylene-octene copolymer resin, 7 kg of silicon dioxide, 40 kg of ethylene-octene copolymer grafted material obtained in Preparation Example 1, 9 kg of low-density polyethylene with a melt index of 30 g / 10 min (190° C., 2.16 kg), and 1.1 kg of composite anti-aging additive in layer C are uniformly mixed to obtain a mixture C, wherein the composite anti-aging additive includes tetra[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid in a weight ratio of 0.3:0.1:0.5 ] pentaerythritol ester, 2-hydroxy-4-n-octyloxybenzophenone and 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol, wherein the amount of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate is 0.37kg, the amount of 2-hydroxy-4-n-octyloxybenzophenone is 0.12kg, and the amount of 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol is 0.61kg;

[0047] Then they are poured into three hoppers of the extruder respectively, and after extrusion at a temperature of 170°C, layer A, layer B and layer C are formed in sequence, and layer A, layer B and layer C are each surfaced in the extrudate with distinct interfaces, and the layer refractive index ratio of layers A, B and C is 1:1.012:1.034. Then, the film is cast and cooled to form, so that the thickness of layer A of the cast film is 10.5μm, the thickness of layer B is 450μm, and the thickness of layer C is 11μm. An energy emission device with a voltage of 200kv and an irradiation cross-linking dosage of 10kGY is used for electron beam surface irradiation to form a low water absorption cast film with an overall cross-linking degree of 5%, and the distance between the energy emission device and the cast film is 50mm. Example 4

[0048] A method for preparing a low water absorption cast film comprises the following steps:

[0049] 95 kg of ethylene-octene copolymer resin, 5 kg of silicon dioxide, 50 kg of ethylene-octene copolymer grafted material obtained in Preparation Example 1, and 1.1 kg of composite anti-aging aid in layer A are uniformly mixed to obtain mixture A, wherein the composite anti-aging aid comprises tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid] pentaerythritol ester, 2-hydroxy-4-n-octyloxybenzophenone and 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol in a weight ratio of 0.3:0.1:0.5, wherein the amount of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid] pentaerythritol ester is 0.37 kg, the amount of 2-hydroxy-4-n-octyloxybenzophenone is 0.12 kg, and the amount of 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol is 0.61 kg;

[0050] 95 kg of ethylene-octene copolymer resin, 8 kg of silicon dioxide, 5 kg of low-density polyethylene with a melt index of 50 g / 10 min (190°C, 2.16 kg), and 1.1 kg of a composite anti-aging additive in layer B are uniformly mixed to obtain a mixture B, wherein the composite anti-aging additive includes pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2-hydroxy- 4-n-octyloxybenzophenone and 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol, wherein the amount of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate is 0.37 kg, the amount of 2-hydroxy-4-n-octyloxybenzophenone is 0.12 kg, and the amount of 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol is 0.61 kg;

[0051] 95 kg of ethylene-octene copolymer resin, 10 kg of silicon dioxide, 50 kg of ethylene-octene copolymer grafted material obtained in Preparation Example 1, 10 kg of low-density polyethylene with a melt index of 50 g / 10 min (190° C., 2.16 kg), and 1.1 kg of composite anti-aging additive in layer C were uniformly mixed to obtain a mixture C, wherein the composite anti-aging additive included tetra[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propane in a weight ratio of 0.3:0.1:0.5. Tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid] pentaerythritol ester, 2-hydroxy-4-n-octyloxybenzophenone and 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol, wherein the amount of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate is 0.37kg, the amount of 2-hydroxy-4-n-octyloxybenzophenone is 0.12kg, and the amount of 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol is 0.61kg;

[0052] Then they are poured into three hoppers of the extruder respectively, and after extrusion at a temperature of 190°C, layer A, layer B and layer C are formed in sequence, and layer A, layer B and layer C are each surfaced in the extrudate with distinct interfaces, and the layer refractive index ratio of layers A, B and C is 1:1.02:1.05. Then, the film is cast and cooled to shape, so that the thickness of layer A of the cast film is 15μm, the thickness of layer B is 600μm, and the thickness of layer C is 15μm. An energy emission device with a voltage of 200kv and an irradiation cross-linking dosage of 10kGY is used for electron beam surface irradiation to form a low water absorption cast film with an overall cross-linking degree of 5%, and the distance between the energy emission device and the cast film is 50mm. Example 5

[0053] A method for preparing a low water absorption cast film, which is different from Example 1 in that the ethylene-octene copolymer grafted material of layer A and layer C adopts the ethylene-octene copolymer grafted material obtained in Preparation Example 2. Example 6

[0054] A method for preparing a low water absorption cast film, which is different from Example 1 in that an energy emission device with a voltage of 400kv and an irradiation crosslinking dosage of 60KGY is used to perform electron beam surface irradiation to form a low water absorption cast film with an overall crosslinking degree of 30%, wherein the distance between the energy emission device and the cast film is 150mm.

[0055] Comparative Example 1 A commercially available POE transparent cast film was used, purchased from Sveck SE556.

[0056] Comparative Example 2 The cast film obtained by Example 2 of Chinese Patent CN102863916A: A POE spectrum conversion solar cell cast film and preparation method thereof was used.

[0057] Comparative Example 3 is different from Example 2 in that the ethylene-octene copolymer graft material in layer A is replaced with an equal amount of ethylene-octene copolymer resin, and the other contents remain unchanged.

[0058] Comparative Example 4 is different from Example 2 in that the ethylene-octene copolymer graft material in layer C is replaced with an equal amount of ethylene-octene copolymer resin, and the other contents remain unchanged.

[0059] Comparative Example 5 is different from Example 2 in that the ethylene-octene copolymer grafted materials in layer A and layer C are replaced with an equal amount of ethylene-octene copolymer resin, and the other contents remain unchanged.

[0060] Comparative Example 6 is different from Example 2 in that it is not configured as three layers but only one layer, that is, the raw materials used for the original three layers A, B, and C are all mixed and poured into a hopper of an extruder for melt extrusion to form a layer, which is then cast and cooled to shape. The other steps and raw material amounts are the same as in Example 2, forming a film with a thickness of 450 μm.

[0061] Comparative Example 7 is different from Example 2 in that it is not configured as three layers but as two layers. Specifically, the raw materials for layer A are mixed to form mixture A, and the raw materials used for the original layers B and C are mixed together to form mixture B. Mixture A and mixture B are respectively poured into two hoppers of an extruder, and then melt-extruded to form two layers with distinct interfaces, and then cast and cooled to shape. The other steps and raw material amounts are the same as those in Example 2, wherein the thickness of layer A film is 7 μm, and the thickness of mixture B layer is 443 μm.

[0062] Comparative Example 8 is different from Example 2 in that there is no low-density polyethylene resin in layer B, and the other contents are the same as those in Example 2.

[0063] Comparative Example 9 is different from Example 2 in that there is no low-density polyethylene resin in the C layer, and the other parts are the same as those in Example 2.

[0064] Performance Testing

[0065] (1) The cast film obtained in the above-mentioned embodiments and preparation examples is applied to a photovoltaic module for connecting photovoltaic glass and a cell. According to the provisions of IEC 61215 "Crystalline Silicon Photovoltaic Modules for Terrestrial Use - Design Identification and Finalization", the photovoltaic module is subjected to a power generation test and a power generation test after a strict aging test. The strict aging conditions are as follows: firstly, the DH2000h test (temperature is 85°C, relative humidity is 85% for continuous aging for 2000h), and then, the UV irradiation is 300kwh / m 2 ,Finally, the PID test was carried out for 96 hours (temperature was 85℃, relative humidity was 85%, and negative pressure was 1000V DC voltage environment). The test results are shown in Table 1.

[0066] (2) The water absorption rate of the cast films obtained in the above-mentioned embodiments and preparation examples was measured. The test conditions were as follows: the cast films were placed in an aging box at a relative humidity of 80% and 80°C. After 24 hours, the cast films were taken out and the weight changes before and after were measured. The test results are shown in Table 1.

[0067] Table 1 Photovoltaic module performance and film test results

[0068] project Water absorption of film (%) Film strict test yellowing value Initial power generation / W Power generation after strict test / W Example 1 0.050 0.2 275.2 275.1 Example 2 0.051 0.3 278.5 278.5 Example 3 0.052 0.3 281.8 281.6 Example 4 0.055 0.3 283.6 283.5 Example 5 0.050 0.2 275.4 275.2 Example 6 0.051 0.2 276.1 275.9 Comparative Example 1 1.5 1.9 268.6 260.2 Comparative Example 2 1.12 0.2 270.4 262.3 Comparative Example 3 0.051 0.3 — — Comparative Example 4 0.051 0.3 — — Comparative Example 5 0.059 0.3 — — Comparative Example 6 0.261 0.7 270.5 260.3 Comparative Example 7 0.061 0.4 272.1 264.7 Comparative Example 8 0.064 0.3 270.4 262.4 Comparative Example 9 0.061 0.3 271.3 264.6

[0069] From Table 1, we can see that:

[0070] The water absorption performance of the cast film obtained in the embodiment of the present application is much lower than that in comparative examples 1-2 and comparative examples 6-9, indicating that the water absorption rate of the cast film obtained in the present application is low, and after the cast film obtained in the embodiment of the present application is applied to the photovoltaic module, the initial power generation power of the photovoltaic module and the power generation power after the rigorous test are better than the power generation power of the photovoltaic module in comparative examples 1-9, indicating that the cast film obtained in the embodiment of the present application can effectively capture light and perform light conversion after being applied to the photovoltaic module, thereby increasing the light utilization rate of the photovoltaic module.

[0071] In Comparative Examples 3-5, after the ethylene-octene copolymer grafted material was replaced with the ethylene-octene copolymer resin, the non-adhesive property between the cast film and the glass resulted in separation between the cast film and the glass, causing the photovoltaic module to be unable to generate electricity. Therefore, the power generation power test of the photovoltaic module in Comparative Examples 3-5 failed.

[0072] The embodiments of this specific implementation method are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A low water absorption cast film, characterized in that: The cast film comprises an ABC three-layer structure; The A layer is composed of the following raw materials in parts by weight: 50-95 parts of ethylene-octene copolymer resin, 0.1-5 parts of silicon dioxide, 5-50 parts of ethylene-octene copolymer grafted material, and 0.1-1.1 parts of composite anti-aging additive; The B layer is composed of the following raw materials in parts by weight: 50-95 parts of ethylene-octene copolymer resin, 0.1-8 parts of silicon dioxide, 0.5-5 parts of refractive index regulator, and 0.1-1.1 parts of composite anti-aging additive; The C layer is composed of the following raw materials in parts by weight: 50-95 parts of ethylene-octene copolymer resin, 0.1-10 parts of silicon dioxide, 5-50 parts of ethylene-octene copolymer grafted material, 6-10 parts of refractive index regulator, and 0.1-1.1 parts of composite anti-aging additive; The ethylene-octene copolymer graft material in the A layer and the C layer is an ethylene-octene copolymer graft coupling agent, and the ethylene-octene copolymer graft material is prepared by the following method: 100 parts of ethylene-octene copolymer, 0.1-0.3 parts of initiator and 0.1-10 parts of oligomer coupling agent are mixed and melt-extruded, cut underwater and vacuum-dried to obtain the ethylene-octene copolymer graft material, and the oligomer coupling agent is selected from one or more of methacryloxysilane oligomer, 2-methoxyethoxysilane oligomer, methoxysilane oligomer, ethoxysilane oligomer, epoxysilane oligomer, vinylmethoxysilane oligomer, vinylepoxysilane oligomer, vinylalkoxysilane oligomer and acrylalkoxysilane oligomer; The refractive index adjusting agent of the B layer and the C layer is one or more of low-density polyethylene, high-density polyethylene, linear low-density polyethylene, and metallocene polyethylene resin; The composite anti-aging auxiliary agent comprises an antioxidant, an ultraviolet light absorber and a light stabilizer in a weight ratio of (0.1-0.3): (0.1-0.5): (0.1-0.5).

2. A low water absorption cast film according to claim 1, characterized in that: The thickness of the A layer and the C layer is 5-15 μm, and the thickness of the B layer is 200-600 μm.

3. The low water absorption cast film according to claim 1, characterized in that: The antioxidant is one or more of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, n-octadecylβ-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, triethylene glycol bis[β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate], tetrakis(2,4-di-tert-butyl-4,4'-biphenyl)bisphosphite, and tris[2,4-di-tert-butylphenyl]phosphite.

4. The low water absorption cast film according to claim 1, characterized in that: The ultraviolet light absorber is one or more of 2-hydroxy-4-n-octyloxybenzophenone, 2-(2'-hydroxy-5'-octylphenyl)-benzotriazole, 2-[2,4-bis(2,4-xylyl)-2-(1,3,5-triazine)5-octyloxyphenol, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate, 2,2,6,6-tetramethyl-4-piperidinyl stearate, salicylic acid, 2-hydroxy-4-methoxy-5-sulfonic acid benzophenone, and 2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-hexyloxy-phenol.

5. The low water absorption cast film according to claim 1, characterized in that: The light stabilizer is one or more of 2-(2H-benzotriazole-2-yl)-6-dodecyl-4-methylphenol, bis(2,2,6,6,-tetramethyl-4-piperidinyl) sebacate, poly(4-hydroxyethyl-2,2,6,6-tetramethyl-1-piperidinethanol) succinate, and poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-[(2,2,6,6,-tetramethyl-piperidinyl)imino]-1,6-hexanediol[(2,2,6,6-tetramethyl-4-piperidinyl)imino]}.

6. A method for preparing a low water absorption cast film according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: mixing the three layers of raw materials A, B and C respectively and then extruding them at a temperature of 140-190°C, casting and cooling them for final shaping, and using an energy emitting device with a voltage of 200-400kv and an irradiation cross-linking dosage of 10-60KGY to irradiate the surface with an electron beam, wherein the distance between the energy emitting device and the cast film is 50-150mm, so as to form a cast film with a low water absorption rate and an overall cross-linking degree of 5-30%.