A light release force composite release film and preparation method thereof
By electrostatically spraying silica and PMMA layers on the PET surface, combined with the composite structure of the antistatic layer and the micro-nano particle layer, the problem of increased peeling force of the existing release film when the surface tension is increased is solved, achieving a lightweight Stripping effects and reducing costs.
Patent Information
- Application Number
- CN202410120467.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-29
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-01-29
AI Technical Summary
When the surface tension of the existing release film is increased, the peeling force increases, making it difficult to meet the low peeling force requirements as a release material. Moreover, the silicone coating has problems of agglomeration and high cost.
Electrostatically sprayed silica is used to form a porous structure on the PET surface, and a PMMA layer is coated on it. Through the composite structure of the antistatic layer and the micro-nano particle layer, the release force is reduced and the light peeling effect is achieved.
A release film with low peeling force is realized, which avoids the agglomeration phenomenon of silicone coating, improves the separability of the film and the irregular concave and convex effect on the surface, and reduces the production cost.
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer materials, and in particular to a light release force composite release film and a preparation method thereof. Background Art
[0002] Release film material refers to a film that is non-sticky or slightly sticky after contacting certain special materials under certain conditions. Polyethylene terephthalate (PET) release film is based on the original PET film as the supporting substrate. The substrate is surface treated to have ultra-low surface energy, strong tensile resistance, stability, and easy peeling. It is the most common release film product and is widely used in electronics, die-cutting and punching processing, printed circuit boards, packaging materials, adhesive products, waterproof materials and other industries.
[0003] The release force of the release film produced is different for the same substrate and different release agents. Based on the release force, it can be divided into light release film, medium release film and heavy release film. The current release force is 5g at the minimum and 2000g at the maximum. At present, most release films are formed by silicone coating, but silicone is modified to increase the surface tension of the release film. However, since increasing the surface tension will also increase the peeling force, the release material must have a relatively low peeling force. Summary of the invention
[0004] Technical problem to be solved: The purpose of the present invention is to provide a composite release film with light release force and a preparation method thereof. In the present invention, silicon dioxide is directly sprayed on the surface of PET by electrostatic spraying, and then PMMA is coated to obtain a release film with light peeling force.
[0005] Technical solution: A light release force composite release film, the release film includes a PET substrate layer, an antistatic layer, a micro-nano particle layer and a PMMA layer, the PET substrate layer and the PMMA layer are located on both sides of the composite layer formed by the antistatic layer and the micro-nano particle layer, and the antistatic layer is connected to the PET substrate layer and the micro-nano particle layer.
[0006] The method for preparing the above-mentioned composite release film with light release force comprises the following steps:
[0007] S1. Preparation of antistatic layer: adding graphene to N, N-dimethylformamide solution, uniformly dispersing by ultrasonication, and then adding the graphene solution to polylactic acid solution to obtain polylactic acid / graphene spinning solution, and electrospinning using the polylactic acid / graphene spinning solution to obtain an electrospinning membrane;
[0008] S2. Composite of substrate layer and antistatic layer: The PET substrate layer and the antistatic layer are composited by hot melt lamination;
[0009] S3. Preparation of micro-nano particle layer: adding hollow porous micro-nano SiO2 particles to a mixed solution of N, N-dimethylformamide / dichloromethane in proportion, adding polylactic acid to the solution after stirring, stirring to obtain an electrostatic spray solution, using one side of the antistatic layer as a receiving plate, electrospraying to obtain a micro-nano particle layer with a concave-convex structure;
[0010] S4. Preparation of PMMA film: dissolve polymethyl methacrylate in toluene, heat and stir until completely dissolved, apply the polymethyl methacrylate solution on one side of the micro-nano particle layer to form a film, and after the solvent evaporates, a release film is obtained.
[0011] Preferably, the mass ratio of graphene to polylactic acid is 2-4:100, the concentration of polylactic acid in the polylactic acid / graphene spinning solution is 6-9wt%, the thickness of the electrospinning membrane is 0.2-0.3mm, wherein the electrospinning membrane is divided into a first membrane layer and a second membrane layer, the porosity of the first membrane layer is 75-85%, and the porosity of the second membrane layer is 88-95%.
[0012] Preferably, the PET substrate layer and the first film layer are heat-melt pressed.
[0013] Preferably, the content of nano-SiO2 particles in the hollow porous micro-nano particles is 70-80%, and the content of micron particles is 20-30%.
[0014] Preferably, in step S2, the mass ratio of the hollow porous micro-nano SiO2 particles to the polylactic acid is 1-1.5:1.
[0015] Preferably, in step S3, the concentration of polylactic acid in the electrostatic spray solution is 1-1.5 wt %, the voltage of the electrostatic spray is 18-22 kV, and the receiving distance is 15-22 cm.
[0016] Preferably, the concentration of the polymethyl methacrylate solution in step S4 is 12.5-18 wt %, and the coating angle is 45°.
[0017] Preferably, the preparation method of the micro-nano porous silica is:
[0018] S11. The hexadecyltrimethylammonium bromide was dissolved in an aqueous solution of urea and mixed and stirred to obtain a mixed solution 1, wherein the mass ratio of hexadecyltrimethylammonium bromide and urea was 2-3:1, and the concentration of urea in the mixed solution was 1.5-3wt%;
[0019] S12. The tetraethyl orthosilicate was added to cyclohexane and ethanol, mixed and stirred to obtain a mixed solution 2, the concentration of tetraethyl orthosilicate was 5-7wt%;
[0020] S13. Add solution 2 prepared in step S12 dropwise to solution 1 prepared in step S11 at a volume ratio of 1:1-1.5. After stirring evenly, stir the reaction for 40-150 min. Heat the reaction at 110-125°C for 8-12 h. Filter under reduced pressure to obtain a precipitate. Wash and dry the precipitate and calcine it at 580°C for 4-5 h to obtain micro-nano porous silica.
[0021] Beneficial effects: The light release force composite release film of the present invention has the following advantages:
[0022] 1. The release film of the present invention is prepared by a multi-layer composite method. First, an antistatic layer is prepared. The antistatic layer is prepared by electrostatic spinning. In the present invention, the electrostatic spinning layer is divided into two layers. The layer close to PET is the first film layer. The first film layer has a low porosity, which is convenient for hot-melt pressing with the PET substrate layer. The first film layer has a high porosity, which is convenient for later loading of electrostatic spray-loaded silica particles. The thickness of the electrostatic spinning film is limited to 0.2-0.3 mm. Under a certain pressure, the electrostatic spinning film has a certain elasticity, which is conducive to the peeling of the release film.
[0023] 2. The present invention does not use organic silicon coating, but uses electrostatic spraying of silicon dioxide. The composite microspheres of electrostatic spraying are porous structures, and the dispersion between microspheres is good, which effectively improves the serious agglomeration of silicon dioxide. At the same time, silicon dioxide is mixed with two different particle sizes to increase the irregular concave-convex effect on the membrane surface;
[0024] 3. In the present invention, after electrostatically spraying silicon dioxide, PMMA is scraped on the silicon dioxide surface to form a film. After scraping, the surface of the PMMA film has an irregular concave-convex effect, which reduces the release force and achieves a light release force effect, so that it can be separated quickly. DETAILED DESCRIPTION
[0025] The present invention will be further described below in conjunction with embodiments, which are explanations of the present invention and are not limited to the following embodiments:
[0026] Example 1
[0027] The preparation method of micro-nano porous silica is:
[0028] S11. The hexadecyltrimethylammonium bromide was dissolved in an aqueous solution of urea and mixed and stirred to obtain a mixed solution 1, wherein the mass ratio of hexadecyltrimethylammonium bromide to urea was 2:1, and the concentration of urea in the mixed solution was 1.5wt%;
[0029] S12. The tetraethyl orthosilicate was added to cyclohexane and ethanol, mixed and stirred to obtain a mixed solution 2, the concentration of tetraethyl orthosilicate was 5wt%;
[0030] S13. Add solution 2 prepared in step S12 dropwise to solution 1 prepared in step S11 at a volume ratio of 1:1.5. After stirring evenly, stir the reaction for 100 min. Heat the reaction at 110°C for 8 h. Filter under reduced pressure to obtain a precipitate. Wash and dry the precipitate and calcine it at 580°C for 4 h to obtain micro-nano porous silica.
[0031] Example 2
[0032] The preparation method of micro-nano porous silica is:
[0033] S11. The hexadecyltrimethylammonium bromide was dissolved in an aqueous solution of urea and mixed and stirred to obtain a mixed solution 1, wherein the mass ratio of hexadecyltrimethylammonium bromide to urea was 2.5:1, and the concentration of urea in the mixed solution was 2.2wt%;
[0034] S12. The tetraethyl orthosilicate was added to cyclohexane and ethanol, mixed and stirred to obtain a mixed solution 2, the concentration of tetraethyl orthosilicate was 6wt%;
[0035] S13. Add solution 2 prepared in step S12 dropwise into solution 1 prepared in step S11 at a volume ratio of 1:1. After stirring evenly, stir the mixture for 40 minutes. Heat the mixture to 125°C for 10 hours. Filter under reduced pressure to obtain a precipitate. Wash and dry the precipitate and calcine it at 580°C for 4 hours to obtain micro-nano porous silica.
[0036] Example 3
[0037] The preparation method of micro-nano porous silica is:
[0038] S11. The hexadecyltrimethylammonium bromide was dissolved in an aqueous solution of urea and mixed and stirred to obtain a mixed solution 1, wherein the mass ratio of hexadecyltrimethylammonium bromide to urea was 3:1, and the concentration of urea in the mixed solution was 3wt%;
[0039] S12. The tetraethyl orthosilicate was added to cyclohexane and ethanol, mixed and stirred to obtain a mixed solution 2, the concentration of tetraethyl orthosilicate was 7wt%;
[0040] S13. Add solution 2 prepared in step S12 to solution 1 prepared in step S11 at a volume ratio of 1:1.2, stir evenly, stir for 150 minutes, heat to react at 120°C for 12 hours, filter under reduced pressure to obtain a precipitate, wash and dry the precipitate, and calcine at 580°C for 5 hours to obtain micro-nano porous silica. The porous silica prepared in Example 1, Example 3 and Example 3 is sieved to be divided into micron-sized and nano-sized silica for subsequent use, and the mass ratios of micron-sized silica and nano-sized silica are 2:8, 2.5:7.5 and 3:7.
[0041] Example 4
[0042] A light release composite release film, the release film comprising a PET substrate layer, an antistatic layer, a micro-nano particle layer and a PMMA layer, the PET substrate layer and the PMMA layer are located on both sides of a composite layer formed by the antistatic layer and the micro-nano particle layer, and the antistatic layer is connected to the PET substrate layer and the micro-nano particle layer;
[0043] The method for preparing the above-mentioned composite release film with light release force comprises the following steps:
[0044] S1. Preparation of antistatic layer: adding graphene to N, N-dimethylformamide solution, ultrasonically dispersing it uniformly, and then adding the graphene solution to polylactic acid solution to obtain polylactic acid / graphene spinning solution, wherein the mass ratio of graphene to polylactic acid is 2:100, and the concentration of polylactic acid in the polylactic acid / graphene spinning solution is 9wt%, and electrospinning is performed using the polylactic acid / graphene spinning solution to obtain an electrospinning membrane, wherein the thickness of the electrospinning membrane is 0.3mm, wherein the electrospinning membrane is divided into a first membrane layer and a second membrane layer, wherein the first membrane layer has a thickness of 0.15mm and a porosity of 90.5%, and the second membrane layer has a thickness of 0.15mm and a porosity of 94.5%;
[0045] S2. Composite substrate layer and antistatic layer: hot melt lamination of the PET substrate layer and the first film layer of the antistatic layer;
[0046] S3. Preparation of micro-nano particle layer: Add hollow porous micro-nano SiO2 particles to a mixed solution of N, N-dimethylformamide / dichloromethane in proportion, the mass ratio of micron-sized silica and nano-sized silica is 2:8, stir evenly, add polylactic acid to the solution, the mass ratio of hollow porous micro-nano SiO2 particles and polylactic acid is 1:1, stir evenly to obtain an electrostatic spray solution, the concentration of polylactic acid in the electrostatic spray solution is 1wt%, and the side of the antistatic layer is used as a receiving plate for electrospraying, the voltage of the electrostatic spray is 18kV, the receiving distance is 15cm, the time is 3h, and the flow rate is 2.5mL / h, to obtain a micro-nano particle layer with a concave-convex structure;
[0047] S4. Preparation of PMMA film: dissolve polymethyl methacrylate in toluene, heat and stir until completely dissolved, and apply a 18wt% polymethyl methacrylate solution on one side of the micro-nano particle layer to form a film at a coating angle of 45°. After the solvent evaporates, a release film is obtained.
[0048] Example 5
[0049] A light release composite release film, the release film comprising a PET substrate layer, an antistatic layer, a micro-nano particle layer and a PMMA layer, the PET substrate layer and the PMMA layer are located on both sides of a composite layer formed by the antistatic layer and the micro-nano particle layer, and the antistatic layer is connected to the PET substrate layer and the micro-nano particle layer;
[0050] The method for preparing the above-mentioned composite release film with light release force comprises the following steps:
[0051] S1. Preparation of antistatic layer: adding graphene to N, N-dimethylformamide solution, ultrasonically dispersing it uniformly, and then adding the graphene solution to polylactic acid solution to obtain polylactic acid / graphene spinning solution, wherein the mass ratio of graphene to polylactic acid is 4:100, and the concentration of polylactic acid in the polylactic acid / graphene spinning solution is 6wt%, and electrospinning is performed using the polylactic acid / graphene spinning solution to obtain an electrospinning membrane, wherein the thickness of the electrospinning membrane is 0.2 mm, wherein the electrospinning membrane is divided into a first membrane layer and a second membrane layer, wherein the first membrane layer has a thickness of 0.1 mm and a porosity of 76.5%, and the second membrane layer has a thickness of 0.1 mm and a porosity of 93.8%;
[0052] S2. Composite substrate layer and antistatic layer: hot melt lamination of the PET substrate layer and the first film layer of the antistatic layer;
[0053] S3. Preparation of micro-nano particle layer: Add hollow porous micro-nano SiO2 particles to a mixed solution of N, N-dimethylformamide / dichloromethane in proportion, the mass ratio of micron-sized silica and nano-sized silica is 2:8, stir evenly, add polylactic acid to the solution, the mass ratio of hollow porous micro-nano SiO2 particles and polylactic acid is 1.5:1, stir evenly to obtain an electrostatic spray solution, the concentration of polylactic acid in the electrostatic spray solution is 1.5wt%, and the side of the antistatic layer is used as a receiving plate for electrospraying, the voltage of the electrostatic spray is 22kV, the receiving distance is 22cm, the time is 3h, and the flow rate is 2.5mL / h, to obtain a micro-nano particle layer with a concave-convex structure;
[0054] S4. Preparation of PMMA film: dissolve polymethyl methacrylate in toluene, heat and stir until completely dissolved, and apply a 12.5wt% polymethyl methacrylate solution on one side of the micro-nano particle layer to form a film at a coating angle of 45°. After the solvent evaporates, a release film is obtained.
[0055] Example 6
[0056] A light release composite release film, the release film comprising a PET substrate layer, an antistatic layer, a micro-nano particle layer and a PMMA layer, the PET substrate layer and the PMMA layer are located on both sides of a composite layer formed by the antistatic layer and the micro-nano particle layer, and the antistatic layer is connected to the PET substrate layer and the micro-nano particle layer;
[0057] The method for preparing the above-mentioned composite release film with light release force comprises the following steps:
[0058] S1. Preparation of antistatic layer: adding graphene to N, N-dimethylformamide solution, ultrasonically dispersing it uniformly, and then adding the graphene solution to polylactic acid solution to obtain polylactic acid / graphene spinning solution, wherein the mass ratio of graphene to polylactic acid is 3.6:100, and the concentration of polylactic acid in the polylactic acid / graphene spinning solution is 8wt%, and electrospinning is performed using the polylactic acid / graphene spinning solution to obtain an electrospinning membrane, wherein the thickness of the electrospinning membrane is 0.3mm, wherein the electrospinning membrane is divided into a first membrane layer and a second membrane layer, wherein the first membrane layer has a thickness of 0.15mm and a porosity of 75.6%, and the second membrane layer has a thickness of 0.15mm and a porosity of 92.6%;
[0059] S2. Composite substrate layer and antistatic layer: hot melt lamination of the PET substrate layer and the first film layer of the antistatic layer;
[0060] S3. Preparation of micro-nano particle layer: Add hollow porous micro-nano SiO2 particles to a mixed solution of N, N-dimethylformamide / dichloromethane in proportion, the mass ratio of micron-sized silica and nano-sized silica is 3:7, stir evenly, add polylactic acid to the solution, the mass ratio of hollow porous micro-nano SiO2 particles and polylactic acid is 1.2:1, stir evenly to obtain an electrostatic spray solution, the concentration of polylactic acid in the electrostatic spray solution is 1.2wt%, and the side of the antistatic layer is used as a receiving plate for electrospraying, the voltage of the electrostatic spray is 18kV, the receiving distance is 20cm, the time is 3h, and the flow rate is 2.5mL / h, to obtain a micro-nano particle layer with a concave-convex structure;
[0061] S4. Preparation of PMMA film: dissolve polymethyl methacrylate in toluene, heat and stir until completely dissolved, and apply a 14wt% polymethyl methacrylate solution on one side of the micro-nano particle layer to form a film at a coating angle of 45°. After the solvent evaporates, a release film is obtained.
[0062] Example 7
[0063] A light release composite release film, the release film comprising a PET substrate layer, an antistatic layer, a micro-nano particle layer and a PMMA layer, the PET substrate layer and the PMMA layer are located on both sides of a composite layer formed by the antistatic layer and the micro-nano particle layer, and the antistatic layer is connected to the PET substrate layer and the micro-nano particle layer;
[0064] The method for preparing the above-mentioned composite release film with light release force comprises the following steps:
[0065] S1. Preparation of antistatic layer: adding graphene to N, N-dimethylformamide solution, ultrasonically dispersing it uniformly, and then adding the graphene solution to polylactic acid solution to obtain polylactic acid / graphene spinning solution, wherein the mass ratio of graphene to polylactic acid is 2.5:100, and the concentration of polylactic acid in the polylactic acid / graphene spinning solution is 7wt%, and electrospinning is performed using the polylactic acid / graphene spinning solution to obtain an electrospinning membrane, wherein the thickness of the electrospinning membrane is 0.25 mm, wherein the electrospinning membrane is divided into a first membrane layer and a second membrane layer, wherein the first membrane layer has a thickness of 0.15 mm and a porosity of 78.5%, and the second membrane layer has a thickness of 0.1 mm and a porosity of 94.9%;
[0066] S2. Composite substrate layer and antistatic layer: hot melt lamination of the PET substrate layer and the first film layer of the antistatic layer;
[0067] S3. Preparation of micro-nano particle layer: Add hollow porous micro-nano SiO2 particles to a mixed solution of N, N-dimethylformamide / dichloromethane in proportion, the mass ratio of micron-sized silica and nano-sized silica is 3:7, stir evenly, add polylactic acid to the solution, the mass ratio of hollow porous micro-nano SiO2 particles and polylactic acid is 1.4:1, stir evenly to obtain an electrostatic spray solution, the concentration of polylactic acid in the electrostatic spray solution is 1.4wt%, and the side of the antistatic layer is used as a receiving plate for electrospraying, the voltage of the electrostatic spray is 22kV, the receiving distance is 18cm, the time is 3h, and the flow rate is 2.5mL / h, to obtain a micro-nano particle layer with a concave-convex structure;
[0068] S4. Preparation of PMMA film: dissolve polymethyl methacrylate in toluene, heat and stir until completely dissolved, and apply a 16wt% polymethyl methacrylate solution on one side of the micro-nano particle layer to form a film at a coating angle of 45°. After the solvent evaporates, a release film is obtained.
[0069] Example 8
[0070] A light release composite release film, the release film comprising a PET substrate layer, an antistatic layer, a micro-nano particle layer and a PMMA layer, the PET substrate layer and the PMMA layer are located on both sides of a composite layer formed by the antistatic layer and the micro-nano particle layer, and the antistatic layer is connected to the PET substrate layer and the micro-nano particle layer;
[0071] The method for preparing the above-mentioned composite release film with light release force comprises the following steps:
[0072] S1. Preparation of antistatic layer: adding graphene to N, N-dimethylformamide solution, ultrasonically dispersing it uniformly, and then adding the graphene solution to polylactic acid solution to obtain polylactic acid / graphene spinning solution, wherein the mass ratio of graphene to polylactic acid is 2.9:100, and the concentration of polylactic acid in the polylactic acid / graphene spinning solution is 7.8wt%, and electrospinning is performed using the polylactic acid / graphene spinning solution to obtain an electrospinning membrane, wherein the thickness of the electrospinning membrane is 0.3mm, wherein the electrospinning membrane is divided into a first membrane layer and a second membrane layer, wherein the first membrane layer has a thickness of 0.15mm and a porosity of 76.9%, and the second membrane layer has a thickness of 0.15mm and a porosity of 93.3%;
[0073] S2. Composite substrate layer and antistatic layer: hot melt lamination of the PET substrate layer and the first film layer of the antistatic layer;
[0074] S3. Preparation of micro-nano particle layer: Add hollow porous micro-nano SiO2 particles to a mixed solution of N, N-dimethylformamide / dichloromethane in proportion, the mass ratio of micron-sized silica and nano-sized silica is 3:7, stir evenly, add polylactic acid to the solution, the mass ratio of hollow porous micro-nano SiO2 particles and polylactic acid is 1.4:1, stir evenly to obtain an electrostatic spray solution, the concentration of polylactic acid in the electrostatic spray solution is 15wt%, and the side of the antistatic layer is used as a receiving plate for electrospraying, the voltage of the electrostatic spray is 20kV, the receiving distance is 18cm, the time is 3h, and the flow rate is 2.5mL / h, to obtain a micro-nano particle layer with a concave-convex structure;
[0075] S4. Preparation of PMMA film: dissolve polymethyl methacrylate in toluene, heat and stir until completely dissolved, and apply a 15wt% polymethyl methacrylate solution on one side of the micro-nano particle layer to form a film at a coating angle of 45°. After the solvent evaporates, a release film is obtained.
[0076] Comparative Example 1
[0077] A composite release film with light release force, the release film comprising a PET substrate layer, a micro-nano particle layer and a PMMA layer, wherein the PET substrate layer and the PMMA layer are located on both sides of the composite layer formed by the micro-nano particle layer;
[0078] The method for preparing the above-mentioned composite release film with light release force comprises the following steps:
[0079] S1. Preparation of micro-nano particle layer: Add hollow porous micro-nano SiO2 particles to a mixed solution of N, N-dimethylformamide / dichloromethane in proportion, the mass ratio of micron-sized silicon dioxide to nano-sized silicon dioxide is 3:7, stir evenly, add polylactic acid to the solution, the mass ratio of hollow porous micro-nano SiO2 particles to polylactic acid is 1.2:1, stir evenly to obtain an electrostatic spray solution, the concentration of polylactic acid in the electrostatic spray solution is 1.2wt%, and one side of the PET substrate layer is used as a receiving plate for electrospraying, the voltage of the electrostatic spray is 18kV, the receiving distance is 20cm, the time is 3h, and the flow rate is 2.5mL / h, to obtain a micro-nano particle layer with a concave-convex structure;
[0080] S4. Preparation of PMMA film: dissolve polymethyl methacrylate in toluene, heat and stir until completely dissolved, and apply a 14wt% polymethyl methacrylate solution on one side of the micro-nano particle layer to form a film at a coating angle of 45°. After the solvent evaporates, a release film is obtained.
[0081] Comparative Example 2
[0082] A light release composite release film, the release film comprising a PET substrate layer, an antistatic layer, a micro-nano particle layer and a PMMA layer, the PET substrate layer and the PMMA layer are located on both sides of a composite layer formed by the antistatic layer and the micro-nano particle layer, and the antistatic layer is connected to the PET substrate layer and the micro-nano particle layer;
[0083] The method for preparing the above-mentioned composite release film with light release force comprises the following steps:
[0084] S1. Preparation of antistatic layer: adding graphene to N, N-dimethylformamide solution, ultrasonically dispersing it uniformly, and then adding the graphene solution to polylactic acid solution to obtain polylactic acid / graphene spinning solution, wherein the mass ratio of graphene to polylactic acid is 2.8:100, and the concentration of polylactic acid in the polylactic acid / graphene spinning solution is 7.5wt%. The polylactic acid / graphene spinning solution is used for electrospinning to obtain an electrospinning membrane, wherein the thickness of the electrospinning membrane is 0.25mm and the porosity is 75.2%;
[0085] S2. Composite substrate layer and antistatic layer: hot melt lamination of the PET substrate layer and the first film layer of the antistatic layer;
[0086] S3. Preparation of micro-nano particle layer: Add hollow porous micro-nano SiO2 particles to a mixed solution of N, N-dimethylformamide / dichloromethane in proportion, the mass ratio of micron-sized silica and nano-sized silica is 3:7, stir evenly, add polylactic acid to the solution, the mass ratio of hollow porous micro-nano SiO2 particles and polylactic acid is 1.5:1, stir evenly to obtain an electrostatic spray solution, the concentration of polylactic acid in the electrostatic spray solution is 1.4wt%, and the side of the antistatic layer is used as a receiving plate for electrospraying, the voltage of the electrostatic spray is 22kV, the receiving distance is 18cm, the time is 3h, and the flow rate is 3mL / h, to obtain a micro-nano particle layer with a concave-convex structure;
[0087] S4. Preparation of PMMA film: dissolve polymethyl methacrylate in toluene, heat and stir until completely dissolved, and apply a 16wt% polymethyl methacrylate solution on one side of the micro-nano particle layer to form a film at a coating angle of 45°. After the solvent evaporates, a release film is obtained.
[0088] Comparative Example 3
[0089] A light release force composite release film, the release film comprising a PET substrate layer, an antistatic layer, a micron particle layer and a PMMA layer, the PET substrate layer and the PMMA layer are located on both sides of a composite layer formed by the antistatic layer and the micron particle layer, and the antistatic layer is connected to the PET substrate layer and the micron particle layer;
[0090] The method for preparing the above-mentioned composite release film with light release force comprises the following steps:
[0091] S1. Preparation of antistatic layer: adding graphene to N, N-dimethylformamide solution, ultrasonically dispersing it uniformly, and then adding the graphene solution to polylactic acid solution to obtain polylactic acid / graphene spinning solution, wherein the mass ratio of graphene to polylactic acid is 3.6:100, and the concentration of polylactic acid in the polylactic acid / graphene spinning solution is 8wt%, and electrospinning is performed using the polylactic acid / graphene spinning solution to obtain an electrospinning membrane, wherein the thickness of the electrospinning membrane is 0.3mm, wherein the electrospinning membrane is divided into a first membrane layer and a second membrane layer, wherein the first membrane layer has a thickness of 0.15mm and a porosity of 75.6%, and the second membrane layer has a thickness of 0.15mm and a porosity of 92.6%;
[0092] S2. Composite substrate layer and antistatic layer: hot melt lamination of the PET substrate layer and the first film layer of the antistatic layer;
[0093] S3. Preparation of micron particle layer: Add micron SiO2 particles to a mixed solution of N, N-dimethylformamide / dichloromethane, stir evenly, then add polylactic acid to the solution, the mass ratio of micron SiO2 particles to polylactic acid is 1.5:1, stir evenly to obtain an electrostatic spray solution, the concentration of polylactic acid in the electrostatic spray solution is 1.2wt%, and the antistatic layer side is used as a receiving plate for electrospraying. The voltage of the electrostatic spray is 18kV, the receiving distance is 20cm, the time is 3h, and the flow rate is 2.5mL / h to obtain a micron particle layer with a concave-convex structure;
[0094] S4. Preparation of PMMA film: dissolve polymethyl methacrylate in toluene, heat and stir until completely dissolved, and apply a 14wt% polymethyl methacrylate solution on one side of the micron particle layer to form a film at a coating angle of 45°. After the solvent evaporates, a release film is obtained.
[0095] Performance Test:
[0096] The release films of the above-mentioned embodiments and comparative examples were peeled off at 180°, and tested by the method for release films of optical functional films in GB / T25256-2010, with a peeling rate of 300 mm / min.
[0097] <![CDATA[Peeling force / cN·(25 mm) -1 > Example 4 2.1 Example 5 1.9 Example 6 2.2 Example 7 1.7 Example 8 2.0 Comparative Example 1 7.5 Comparative Example 2 4.2 Comparative Example 3 3.6
[0098] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A composite release film with light release force, characterized in that: The release film comprises a PET substrate layer, an antistatic layer, a micro-nano particle layer and a PMMA layer, wherein the PET substrate layer and the PMMA layer are located on both sides of a composite layer formed by the antistatic layer and the micro-nano particle layer, and the antistatic layer is connected to the PET substrate layer and the micro-nano particle layer; The method for preparing the composite release film with light release force comprises the following steps: S1. Preparation of antistatic layer: adding graphene to N, N-dimethylformamide solution, uniformly dispersing by ultrasonication, and then adding the graphene solution to polylactic acid solution to obtain polylactic acid / graphene spinning solution, and electrospinning using the polylactic acid / graphene spinning solution to obtain an electrospinning membrane; S2. Composite of the substrate layer and the antistatic layer: The PET substrate layer and the antistatic layer are composited by hot melt lamination; S3. Preparation of micro-nano particle layer: adding hollow porous micro-nano SiO2 particles to a mixed solution of N, N-dimethylformamide / dichloromethane in proportion, adding polylactic acid to the solution after stirring, stirring to obtain an electrostatic spray solution, using one side of the antistatic layer as a receiving plate, electrospraying to obtain a micro-nano particle layer with a concave-convex structure; S4. Preparation of PMMA film: dissolve polymethyl methacrylate in toluene, heat and stir until completely dissolved, apply the polymethyl methacrylate solution on one side of the micro-nano particle layer to form a film, and after the solvent evaporates, a release film is obtained.
2. The light release force composite release film according to claim 1, characterized in that: The mass ratio of graphene to polylactic acid is 2-4:100, the concentration of polylactic acid in the polylactic acid / graphene spinning solution is 6-9wt%, the thickness of the electrospinning membrane is 0.2-0.3mm, and the electrospinning membrane is divided into a first membrane layer and a second membrane layer, the porosity of the first membrane layer is 75-85%, and the porosity of the second membrane layer is 88-95%.
3. The light release force composite release film according to claim 2, characterized in that: The PET substrate layer and the first film layer are heat-melted and pressed.
4. The light release force composite release film according to claim 1, characterized in that: The content of nano-SiO2 particles in the hollow porous micro-nano SiO2 particles is 70-80%, and the content of micron particles is 20-30%.
5. The light release force composite release film according to claim 1, characterized in that: In the step S2, the mass ratio of the hollow porous micro-nano SiO2 particles to the polylactic acid is 1-1.5:
1.
6. The light release force composite release film according to claim 1, characterized in that: In step S3, the concentration of polylactic acid in the electrostatic spray solution is 1-1.5wt%, the voltage of the electrostatic spray is 18-22kV, and the receiving distance is 15-22cm.
7. The light release force composite release film according to claim 1, characterized in that: The concentration of the polymethyl methacrylate solution in step S4 is 12.5-18 wt %, and the coating angle is 45°.
8. The light release force composite release film according to claim 1, characterized in that: The preparation method of the hollow porous micro-nano SiO2 particles is as follows: S11. The hexadecyltrimethylammonium bromide was dissolved in an aqueous solution of urea and mixed and stirred to obtain a mixed solution 1, wherein the mass ratio of hexadecyltrimethylammonium bromide and urea was 2-3:1, and the concentration of urea in the mixed solution was 1.5-3wt%; S12. The tetraethyl orthosilicate was added to cyclohexane and ethanol, and the mixture was stirred to obtain a mixed solution 2, wherein the concentration of the tetraethyl orthosilicate was 5-7wt%; S13. Add solution 2 prepared in step S12 dropwise to solution 1 prepared in step S11 at a volume ratio of 1:1-1.
5. After stirring evenly, stir the reaction for 40-150 min. Heat the reaction at 110-125°C for 8-12 h. Filter under reduced pressure to obtain a precipitate. Wash and dry the precipitate and calcine it at 580°C for 4-5 h to obtain hollow porous micro-nano SiO2 particles.