A porous polymer membrane and a method for preparing the same
By pouring the surface of a solidification bath solution of cellulose ether, organic solvent and water, the viscosity and surface tension of the polymer film are adjusted, and the problems of pore size uniformity and process complexity in the preparation of porous polymer films are solved, achieving high efficiency and environmental protection Film preparation process.
Patent Information
- Application Number
- CN202410230391.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-02-29
AI Technical Summary
In the existing porous polymer membrane preparation process, it is difficult to ensure the uniformity of membrane pore size and the complexity of the preparation process, and there are high energy consumption and environmental protection problems.
By pouring the polymer solution into the surface of the solidification bath solution containing cellulose ether, organic solvent and water, the viscosity of the polymer solution, the surface tension of the solidification bath, the ambient temperature and humidity are adjusted, so that the polymer solution and the solidification bath solution can be adjusted in the When in contact, they match each other to form a uniform porous polymer membrane.
It has achieved extensive control over the pore size of porous polymer membranes, with pore uniformity up to 91% to 99%, no high-temperature or low-temperature heat treatment required, simple operation, low energy consumption, zero wastewater discharge, good environmental protection.
Smart Images

Figure CN118126373B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer membranes, and in particular to a porous polymer membrane and a preparation method thereof. Background Art
[0002] Polymer films are widely used in various fields of industry and daily life, and play an extremely important role in scientific and economic development. Compared with non-porous dense polymer films, porous polymer films usually have lower density, higher specific surface area, and have the characteristics of sound insulation and heat insulation, good permeability, and high separation efficiency. Therefore, they have great application value in many fields such as water treatment, industrial separation / extraction, energy storage (battery separators), electronic components, and medical and health care. In the industrial preparation of porous polymer films, the mainstream pore preparation methods include phase separation method, template method, and melt extrusion / stretching method. The specific characteristics of phase separation method for membrane preparation: through the phase separation process, the polymer solution phase is separated into two coexisting liquid phases in thermodynamic equilibrium, in which the polymer-rich phase solidifies to form a solid matrix, and the non-solvent-rich polymer-poor phase forms pores in the matrix. The film-making characteristics of the template method are: using a template material with a certain shape and size, mixing it with a polymer material, and then removing the template to make holes, and finally obtaining a polymer film material with a certain pore structure; and the preparation characteristics of the stretching method are: using the extrusion and film blowing methods to make the molten polymer into a sheet film, and forming a slit-shaped porous structure at high temperature through a uniaxial stretching or biaxial stretching process.
[0003] Although these three types of porous polymer film preparation methods have matured in industrial applications, the natural defects of these existing processes in principle are difficult to solve through equipment innovation. In the traditional phase separation process, the amount of highly volatile organic solvents used is huge, and the back-end process must evaporate these organic solvents by heating the carrier to form a film, which will produce a large amount of organic volatile pollutants, making environmental protection treatment more difficult and the cost of waste gas / wastewater treatment soaring. In addition, due to the complexity of the phase separation process, the stability and uniformity of the pore structure are also difficult to control. In the template process, the preparation method of uniformly sized pores requires selectively removing the template components in the material to produce pores. The addition and subsequent removal of the template material often makes the pore-making process complicated and inefficient, and brings greater uncertainty to the control of the uniformity of the pore structure; while in the melt extrusion / stretching method, the melting temperature of the polymer is generally as high as 200-500°C, while the temperature of the cooling roller is generally as low as 0-5°C. In large-scale industrial production, the demand for energy consumption is very large, and the process equipment and process are relatively complex, and the preparation cost is huge. Summary of the invention
[0004] In view of this, the present invention proposes a porous polymer membrane and a preparation method thereof to solve the problems in the prior art that it is difficult to ensure the uniformity of the membrane pore size and the preparation process is complicated during the preparation of the porous polymer membrane.
[0005] In the prior art, the conventional scraping method is often used to prepare porous membranes by phase separation. In this method, the polymer solution is first scraped onto a supporting substrate, and then the substrate with the polymer liquid layer formed by scraping is immersed in an aqueous coagulation bath, and the polymer liquid layer is formed into a porous membrane through a solvent diffusion process. However, the above film formation process requires substrate support on the one hand, and it is difficult to control the pore size and uniformity of the porous membrane on the other hand.
[0006] The technical solution of the present invention is achieved in this way:
[0007] In a first aspect, the present invention provides a method for preparing a porous polymer membrane, comprising the following steps:
[0008] S1, dissolving the polymer in an organic solvent to obtain a polymer solution;
[0009] S2, mixing cellulose ether, an organic solvent and water to obtain a coagulation bath solution;
[0010] S3, pouring the polymer solution onto the surface of the coagulation bath solution to form a porous polymer film after solidification.
[0011] In the present invention, a polymer is dissolved in an organic solvent to form a polymer solution, cellulose ether, an organic solvent and water are mixed in a certain proportion to obtain a coagulation bath solution, and then by adjusting the viscosity of the polymer solution, the surface tension of the coagulation bath solution, and the ambient temperature and humidity during the curing process, the viscosity and surface tension of the polymer solution and the coagulation bath solution at the moment of contact and during the film formation of the polymer solution are finally matched with each other, thereby achieving the control of the pore size in the film during the film formation of the polymer film. Specifically, when the polymer solution contacts the coagulation bath liquid surface, the polymer solution, under the action of the surface tension of the coagulation bath solution, first spreads out to the surroundings on the coagulation bath liquid surface to form a uniform liquid film; at the same time, the organic solvent in the spreading liquid film, driven by the concentration difference of the coagulation bath, will diffuse into the coagulation bath and undergo a phase separation process. This process will cause the solvent in the polymer liquid film to exchange solvent-water with the water in the coagulation bath, thereby forming a porous structure in the polymer film formed by curing. Compared with the traditional scraping phase separation process, the film formation process of the polymer solution on the surface of the coagulation bath does not require a substrate. The liquid film formed by spreading directly undergoes a phase separation process on the surface of the coagulation bath to form a self-supporting porous film. By adjusting the viscosity of the polymer solution, the surface tension of the coagulation bath, and the temperature and humidity of the ambient air, the diffusion rate of the organic solvent in the spreading liquid film to the coagulation bath can be controlled, thereby regulating the size of the membrane pore size during the spreading film formation process and forming a uniformly distributed pore structure.
[0012] On the basis of the above technical solution, preferably, the viscosity of the polymer solution is 23 mPa·s to 170000 mPa·s, and the viscosity is regulated by the mass percentage of the polymer solution and the temperature of the polymer solution.
[0013] On the basis of the above technical solution, preferably, the mass percentage of the polymer solution is 0.1% to 60%, and the temperature of the polymer solution is 10°C to 70°C.
[0014] Specifically, by changing the mass percentage of the polymer in the solvent, the concentration of the polymer in the solution can be adjusted, thereby affecting the viscosity of the solution. Increasing the mass percentage of the polymer will increase the viscosity of the solution. The increase in the concentration of the polymer will increase the interaction between molecules, thereby increasing the viscosity of the solution. On the contrary, reducing the mass percentage of the polymer will cause the viscosity of the solution to decrease. However, when the mass fraction of the polymer solution is too high, it will lead to an increase in the aggregation of the polymer, causing the dispersion of the polymer in the solvent to deteriorate, thereby affecting the uniformity and quality of the film. The temperature of the solution will also affect its viscosity. As the temperature increases, the viscosity of the solution will decrease. High temperature will increase the thermal mobility of the molecules, thereby reducing the interaction between molecules and reducing the viscosity of the solution. Increasing the temperature can partially offset the increase in viscosity caused by the increase in the mass percentage of the polymer solution. Therefore, the mass percentage of the polymer solution and the temperature of the polymer solution can synergistically regulate the viscosity of the polymer solution, making the viscosity of the solution change more slowly, thereby causing the viscosity to be between 23mPa·s and 170000mPa·s.
[0015] Based on the above technical solution, preferably, the surface tension of the coagulation bath solution is 71mN / m to 33mN / m, and the surface tension of the coagulation bath solution is regulated by the ratio of cellulose ether, organic solvent and water and the temperature of the coagulation bath solution.
[0016] On the basis of the above technical solution, preferably, the mass ratio of organic solvent, cellulose ether and water is (99.9-0.2):(0.1-9.8):(0-90), and the temperature of the coagulation bath solution is 0°C-70°C.
[0017] Specifically, cellulose ether in the solution will interact with water molecules through hydrogen bonds, van der Waals forces and other interactions. When the cellulose ether increases, the interaction between molecules will increase, making the molecular structure of the solution tighter, thereby increasing the surface tension. The increase in the temperature of the coagulation bath solution will cause the surface tension of the coagulation bath solution to decrease. Therefore, the ratio of cellulose, organic solvent and water and the temperature of the coagulation bath solution work synergistically to more accurately adjust the surface tension of the coagulation bath solution, causing its surface tension to be 71mN / m~33mN / m.
[0018] On the basis of the above technical solution, preferably, the polymer includes any one of polyvinylidene fluoride and its copolymer, polyimide, aramid, cellulose acetate and thermoplastic polyurethane.
[0019] On the basis of the above technical solution, preferably, the organic solvent includes any one of N,N-dimethylformamide, N-methylpyrrolidone, dimethylacetamide, dimethyl sulfoxide and cyclohexanone.
[0020] On the basis of the above technical solution, preferably, the cellulose ether includes methyl cellulose ether or hydroxypropyl methyl cellulose ether.
[0021] On the basis of the above technical solution, preferably, during the curing in step S3, the ambient humidity is 30% to 80%, and the ambient temperature is 15° C. to 47° C.
[0022] Specifically, high ambient temperature and low humidity during curing will accelerate the evaporation rate of the solvent, which is conducive to the formation of a larger pore structure; at the same time, the accelerated evaporation rate of the solvent will also cause the polymer film to shrink too quickly, causing deformation and dimensional changes in the pore structure.
[0023] In a second aspect, the present invention provides a porous polymer membrane, wherein the porous polymer membrane is prepared by the preparation method as described above, and the pore size of the porous polymer membrane is 0.03 μm to 1.75 μm.
[0024] In the present invention, the viscosity and surface tension of the polymer solution and the coagulation bath solution at the moment of contact and during the film-forming process of the polymer solution are matched with each other, that is, the viscosity of the polymer solution is in the range of 23mPa·s to 170000mPa·s, and at the same time, the surface tension of the coagulation bath is in the range of 71mN / m to 33mN / m. At this time, a porous polymer membrane with a pore size of 0.03μm to 1.75μm and uniform pore size distribution can be prepared, and the pore size uniformity of the porous polymer membrane can be as high as 91% to 99%.
[0025] The porous polymer membrane and the preparation method thereof of the present invention have the following beneficial effects compared with the prior art:
[0026] (1) The preparation method can achieve the control of the pore size in the polymer film formation process by matching the viscosity and surface tension of the polymer solution and the coagulation bath solution at the moment of contact and during the film formation process of the polymer solution, so that the prepared porous polymer film has a wide pore size control range, a narrow pore size distribution range, and a uniformity of up to 91% to 99%;
[0027] (2) The preparation method of the porous polymer membrane provided by the present invention does not require high-temperature or low-temperature heat treatment, nor does it require a supporting substrate. The porous polymer membrane can be solidified to form a porous polymer membrane only through solvent-water exchange between the solvent in the polymer solution and the water in the coagulation bath. After the film is solidified, it can be directly taken out from the surface of the coagulation bath and dried at room temperature. It has the advantages of simple operation and low energy consumption. At the same time, the generation of organic volatile gases in the film-forming process is extremely small, and the film can be reused many times, achieving zero wastewater discharge, low pollution, and good environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 Schematic diagram of the film-forming principle of the porous polymer film of the present invention;
[0030] Figure 2 This is a cross-sectional SEM image of the porous polymer membrane prepared in Example 1 of the present invention;
[0031] Figure 3 This is a pore size distribution diagram of the porous polymer membrane prepared in Example 1 of the present invention;
[0032] Figure 4 This is a cross-sectional SEM image of the porous polymer membrane prepared in Example 2 of the present invention;
[0033] Figure 5 This is a pore size distribution diagram of the porous polymer membrane prepared in Example 2 of the present invention;
[0034] Figure 6 This is a cross-sectional SEM image of the porous polymer membrane prepared in Example 3 of the present invention;
[0035] Figure 7 This is a pore size distribution diagram of the porous polymer membrane prepared in Example 3 of the present invention;
[0036] Figure 8 This is a cross-sectional SEM image of the porous polymer membrane prepared in Example 4 of the present invention;
[0037] Fig. 9 This is a pore size distribution diagram of the porous polymer membrane prepared in Example 4 of the present invention;
[0038] Fig.10 This is a cross-sectional SEM image of the porous polymer membrane prepared in Example 5 of the present invention;
[0039] Fig.11 This is a pore size distribution diagram of the porous polymer membrane prepared in Example 5 of the present invention;
[0040] Fig.12 This is a cross-sectional SEM image of the porous polymer membrane prepared in Example 6 of the present invention;
[0041] Fig.13 This is a pore size distribution diagram of the porous polymer membrane prepared in Example 6 of the present invention;
[0042] Fig.14 This is a cross-sectional SEM image of the porous polymer membrane prepared in Example 7 of the present invention;
[0043] Fig.15 This is a pore size distribution diagram of the porous polymer membrane prepared in Example 7 of the present invention;
[0044] Fig.16 The optical images and cross-sectional SEM images of different regions of the porous polymer membrane prepared in Example 7 of the present invention;
[0045] Fig.17 This is a cross-sectional SEM image of the porous polymer membrane prepared in Example 8 of the present invention;
[0046] Fig.18 This is a pore size distribution diagram of the porous polymer membrane prepared in Example 8 of the present invention;
[0047] Fig.19 This is a cross-sectional SEM image of the porous polymer membrane prepared in Example 9 of the present invention;
[0048] Fig. 20 This is a pore size distribution diagram of the porous polymer membrane prepared in Example 9 of the present invention;
[0049] Fig.21 This is a cross-sectional SEM image of the porous polymer membrane prepared in Example 10 of the present invention;
[0050] Fig. 22 This is a pore size distribution diagram of the porous polymer membrane prepared in Example 10 of the present invention;
[0051] Fig.23 This is a cross-sectional SEM image of the porous polymer membrane prepared in Example 11 of the present invention;
[0052] Fig.24 This is a pore size distribution diagram of the porous polymer membrane prepared in Example 11 of the present invention;
[0053] Fig.25This is a cross-sectional SEM image of the porous polymer membrane prepared in Example 12 of the present invention;
[0054] Fig.26 This is a pore size distribution diagram of the porous polymer membrane prepared in Example 12 of the present invention;
[0055] Fig. 27 This is a cross-sectional SEM image of the porous polymer membrane prepared in Example 13 of the present invention;
[0056] Fig.28 This is a pore size distribution diagram of the porous polymer membrane prepared in Example 13 of the present invention;
[0057] Fig.29 The optical images and cross-sectional SEM images of different regions of the porous polymer membrane prepared in Comparative Example 2 of the present invention are shown;
[0058] Fig.30 The optical images and cross-sectional SEM images of different regions of the porous polymer membrane prepared in Comparative Example 3 of the present invention are shown;
[0059] Fig.31 This is a cross-sectional SEM image of the porous polymer membrane prepared in Comparative Example 4 of the present invention;
[0060] Fig.32 This is a pore size distribution diagram of the porous polymer membrane prepared in Comparative Example 4 of the present invention;
[0061] Fig.33 This is an optical picture of the porous polymer film prepared in Comparative Example 5 of the present invention. DETAILED DESCRIPTION
[0062] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0063] Example 1
[0064] This embodiment provides a porous polymer membrane and a method for preparing the same, comprising the following steps:
[0065] S1, dissolving polyvinylidene fluoride (PVDF) in N,N-dimethylformamide (DMF) to form a PVDF / DMF solution with a mass fraction of 5%, and adjusting the temperature of the PVDF / DMF solution to 10° C. so that the viscosity of the PVDF / DMF solution is 23 mPa·s;
[0066] S2, DMF: methyl cellulose ether: water are mixed in a ratio of 1:9:90 to obtain a coagulation bath solution, and the temperature of the coagulation bath is adjusted to 10° C. so that the surface tension of the coagulation bath is 62 mN / m;
[0067] S3. Regulate the relative humidity of the ambient air to 30% and the ambient air temperature to 15° C., pour the PVDF / DMF solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer membrane.
[0068] Figure 1 The film-forming principle of the porous polymer film of the present invention is shown, that is, in the polymer liquid film spread on the surface of the coagulation bath, the solvent diffuses into the coagulation bath, resulting in a solvent-water exchange process, thereby forming a pore structure. Figure 2 The cross-sectional SEM image of the porous polymer membrane prepared in this embodiment is shown. Figure 3 The pore size distribution diagram of the porous polymer membrane prepared in this embodiment is shown. It can be seen from the figure that the pore size distribution of the membrane is uniform, the average pore size is 1.73μm, and the pore size distribution of the membrane in the range of 1.62μm to 1.94μm accounts for about 96%.
[0069] Example 2
[0070] This embodiment provides a porous polymer membrane and a method for preparing the same, comprising the following steps:
[0071] S1, dissolving PVDF in DMF to form a PVDF / DMF solution with a mass fraction of 6%, and adjusting the temperature of the PVDF / DMF solution to 10° C. so that the viscosity of the PVDF / DMF solution is 200 mPa·s;
[0072] S2, DMF: hydroxypropyl methylcellulose ether: water are mixed in a ratio of 6:9:85 to obtain a coagulation bath solution, and the temperature of the coagulation bath is adjusted to 10° C. so that the surface tension of the coagulation bath is 60 mN / m;
[0073] S3. Regulate the relative humidity of the ambient air to 30% and the ambient air temperature to 15° C., pour the PVDF / DMF solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer membrane.
[0074] Figure 4 The cross-sectional SEM image of the porous polymer membrane prepared in this embodiment is shown. Figure 5 The pore size distribution diagram of the porous polymer membrane prepared in this embodiment is shown. It can be seen from the figure that the pore size distribution of the membrane is uniform, the average pore size is 1.29μm, and the pores with a pore size range of 0.98μm to 1.32μm account for about 99%.
[0075] Example 3
[0076] This embodiment provides a porous polymer membrane and a method for preparing the same, comprising the following steps:
[0077] S1, dissolving PVDF in DMF to form a PVDF / DMF solution with a mass fraction of 8%, and adjusting the temperature of the PVDF / DMF solution to 15° C. so that the viscosity of the PVDF / DMF solution is 800 mPa·s;
[0078] S2, DMF: hydroxypropyl methylcellulose ether: water are mixed in a ratio of 12:8:80 to obtain a coagulation bath solution, and the temperature of the coagulation bath is adjusted to 15° C. so that the surface tension of the coagulation bath is 58 mN / m;
[0079] S3. Adjust the relative humidity of the ambient air to 30% and the ambient air temperature to 15° C., pour the PVDF / DMF solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer membrane.
[0080] Figure 6 The cross-sectional SEM image of the porous polymer membrane prepared in this embodiment is shown. Figure 7 The pore size distribution diagram of the porous polymer membrane prepared in this embodiment is shown. It can be seen from the figure that the pore size distribution of the membrane is uniform, the average pore size is 1.04μm, and the pore size distribution of the membrane in the range of 0.93μm to 1.04μm accounts for about 99%.
[0081] Example 4
[0082] This embodiment provides a porous polymer membrane and a method for preparing the same, comprising the following steps:
[0083] S1, dissolving PVDF in DMF to form a PVDF / DMF solution with a mass fraction of 17%, and adjusting the temperature of the PVDF / DMF solution to 60° C. so that the viscosity of the PVDF / DMF solution is 35736 mPa·s;
[0084] S2, DMF: methyl cellulose ether: water are mixed in a ratio of 50:5:45 to obtain a coagulation bath solution, and the temperature of the coagulation bath is adjusted to 60° C. so that the surface tension of the coagulation bath is 48 mN / m;
[0085] S3. Regulate the relative humidity of the ambient air to 50% and the ambient air temperature to 25° C., pour the PVDF / DMF solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer membrane.
[0086] Figure 8 The cross-sectional SEM image of the porous polymer membrane prepared in this embodiment is shown. Fig. 9The pore size distribution diagram of the porous polymer membrane prepared in this embodiment is shown. It can be seen from the figure that the pore size distribution of the membrane is uniform, the average pore size is 0.12μm, and the pore size distribution of the membrane in the range of 0.11μm to 0.12μm accounts for about 92%.
[0087] Example 5
[0088] This embodiment provides a porous polymer membrane and a method for preparing the same, comprising the following steps:
[0089] S1, dissolving PVDF in N-methylpyrrolidone (NMP) to form a PVDF / NMP solution with a mass fraction of 25%, and adjusting the temperature of the PVDF / NMP solution to 70° C. so that the viscosity of the PVDF / DMF solution is 69957 mPa·s;
[0090] S2, mixing NMP: methyl cellulose ether: water in a ratio of 94:1:5 to obtain a coagulation bath solution, and adjusting the temperature of the coagulation bath to 60° C. so that the surface tension of the coagulation bath is 33 mN / m;
[0091] S3. Adjust the relative humidity of the ambient air to 50% and the ambient air temperature to 25° C., pour the PVDF / NMP solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer membrane.
[0092] Fig.10 The cross-sectional SEM image of the porous polymer membrane prepared in this embodiment is shown. Fig.11 The pore size distribution diagram of the porous polymer membrane prepared in this embodiment is shown. It can be seen from the figure that the pore size distribution of the membrane is uniform, the average pore size is 0.04μm, and the pore size distribution of the membrane in the range of 0.03μm to 0.04μm accounts for about 91%.
[0093] Example 6
[0094] This embodiment provides a porous polymer membrane and a method for preparing the same, comprising the following steps:
[0095] S1, dissolving PVDF in NMP to form a PVDF / NMP solution with a mass fraction of 20%, and adjusting the temperature of the PVDF / NMP solution to 65° C. so that the viscosity of the PVDF / DMF solution is 83448 mPa·s;
[0096] S2, mixing NMP: hydroxypropyl methylcellulose ether: water in a ratio of 82:3:15 to obtain a coagulation bath solution, and adjusting the temperature of the coagulation bath to 65° C. so that the surface tension of the coagulation bath is 40 mN / m;
[0097] S3. Adjust the relative humidity of the ambient air to 50% and the ambient air temperature to 25° C., pour the PVDF / NMP solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer membrane.
[0098] Fig.12 The cross-sectional SEM image of the porous polymer membrane prepared in this embodiment is shown. Fig.13 The pore size distribution diagram of the porous polymer membrane prepared in this embodiment is shown. It can be seen from the figure that the pore size distribution of the membrane is uniform, the average pore size is 0.05μm, and the pore size distribution of the membrane in the range of 0.05μm to 0.051μm accounts for about 97%.
[0099] Example 7
[0100] This embodiment provides a porous polymer membrane and a method for preparing the same, comprising the following steps:
[0101] S1, dissolving PVDF in NMP to form a PVDF / NMP solution with a mass fraction of 14%, and adjusting the temperature of the PVDF / NMP solution to 40° C. so that the viscosity of the PVDF / DMF solution is 9800 mPa·s;
[0102] S2, mixing NMP: methyl cellulose ether: water in a ratio of 39:6:55 to obtain a coagulation bath solution, and adjusting the temperature of the coagulation bath to 40° C. so that the surface tension of the coagulation bath is 50 mN / m;
[0103] S3. Regulate the relative humidity of the ambient air to 40% and the ambient air temperature to 20° C., pour the PVDF / NMP solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer membrane.
[0104] Fig.14 The cross-sectional SEM image of the porous polymer membrane prepared in this embodiment is shown. Fig.15 The pore size distribution diagram of the porous polymer membrane prepared in this embodiment is shown. It can be seen from the figure that the pore size distribution of the membrane is uniform, the average pore size is 0.20 μm, and the pores with a pore size range of 0.18 μm to 0.20 μm account for about 99%. Fig.16 The optical images and cross-sectional SEM images of different regions of the porous polymer film prepared in this example are shown. It can be seen from the figures that the thickness uniformity of the film is good.
[0105] Example 8
[0106] This embodiment provides a porous polymer membrane and a method for preparing the same, comprising the following steps:
[0107] S1, dissolving PVDF in DMF to form a PVDF / DMF solution with a mass fraction of 13%, and adjusting the temperature of the PVDF / DMF solution to 35° C. so that the viscosity of the PVDF / DMF solution is 7977 mPa·s;
[0108] S2, DMF: hydroxypropyl methylcellulose ether: water in a ratio of 33:7:60 is mixed to obtain a coagulation bath solution, and the temperature of the coagulation bath is adjusted to 35° C. so that the surface tension of the coagulation bath is 52 mN / m;
[0109] S3. Regulate the relative humidity of the ambient air to 40% and the ambient air temperature to 20° C., pour the PVDF / DMF solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer membrane.
[0110] Fig.17 The cross-sectional SEM image of the porous polymer membrane prepared in this embodiment is shown. Fig.18 The pore size distribution diagram of the porous polymer membrane prepared in this embodiment is shown. It can be seen from the figure that the pore size distribution of the membrane is uniform, the average pore size is 0.24μm, and the pore size distribution of the membrane in the range of 0.23μm to 0.25μm accounts for about 99%.
[0111] Example 9
[0112] This embodiment provides a porous polymer membrane and a method for preparing the same, comprising the following steps:
[0113] S1, dissolving PVDF in DMF to form a PVDF / DMF solution with a mass fraction of 11%, and adjusting the temperature of the PVDF / DMF solution to 25° C. so that the viscosity of the PVDF / DMF solution is 3020 mPa·s;
[0114] S2, DMF: hydroxypropyl methylcellulose ether: water in a ratio of 23:7:70 is mixed to obtain a coagulation bath solution, and the temperature of the coagulation bath is adjusted to 25° C. so that the surface tension of the coagulation bath is 54 mN / m;
[0115] S3. Regulate the relative humidity of the ambient air to 40% and the ambient air temperature to 20° C., pour the PVDF / DMF solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer membrane.
[0116] Fig.19 The cross-sectional SEM image of the porous polymer membrane prepared in this embodiment is shown. Fig. 20 The pore size distribution diagram of the porous polymer membrane prepared in this embodiment is shown. It can be seen from the figure that the pore size distribution of the membrane is uniform, the average pore size is 0.37μm, and the pore size distribution of the membrane in the range of 0.33μm to 0.41μm accounts for about 99%.
[0117] Example 10
[0118] This embodiment provides a porous polymer membrane and a method for preparing the same, comprising the following steps:
[0119] S1, dissolving aramid fiber (ANF) in dimethyl sulfoxide (DMSO) to form a 5% by mass PVDF / DMSO solution, and adjusting the temperature of the ANF / DMSO solution to 35° C. so that the viscosity of the ANF / DMSO solution is 53319 mPa·s;
[0120] S2, DMSO: methyl cellulose ether: water are mixed in a ratio of 76:4:20 to obtain a coagulation bath solution, and the temperature of the coagulation bath is adjusted to 65° C. so that the surface tension of the coagulation bath is 45 mN / m;
[0121] S3. Adjust the relative humidity of the ambient air to 450% and the ambient air temperature to 25° C., pour the ANF / DMSO solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer membrane.
[0122] Fig.21 The cross-sectional SEM image of the porous polymer membrane prepared in this embodiment is shown. Fig. 22 The pore size distribution diagram of the porous polymer membrane prepared in this embodiment is shown. It can be seen from the figure that the pore size distribution of the membrane is uniform, the average pore size is 0.04μm, and the pores with a pore size in the range of 0.035μm to 0.036μm account for about 98%.
[0123] Embodiment 11
[0124] This embodiment provides a porous polymer membrane and a method for preparing the same, comprising the following steps:
[0125] S1. dissolving thermoplastic polyurethane (TPU) in cyclohexanone (CYC) to form a TPU / CYC solution with a mass fraction of 15%, and adjusting the temperature of the TPU / CYC solution to 50° C. so that the viscosity of the TPU / CYC solution is 9985 mPa·s;
[0126] S2, mixing CYC: methyl cellulose ether: water in a ratio of 42:6:52 to obtain a coagulation bath solution, and adjusting the temperature of the coagulation bath to 50° C. so that the surface tension of the coagulation bath is 49 mN / m;
[0127] S3. Adjust the relative humidity of the ambient air to 50% and the ambient air temperature to 25° C., pour the TPU / CYC solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer film.
[0128] Fig.23The cross-sectional SEM image of the porous polymer membrane prepared in this embodiment is shown. Fig.24 The pore size distribution diagram of the porous polymer membrane prepared in this embodiment is shown. It can be seen from the figure that the pore size distribution of the membrane is uniform, the average pore size is 0.20μm, and the pore size distribution of the membrane in the range of 0.18μm to 0.20μm accounts for about 99%.
[0129] Example 12
[0130] This embodiment provides a porous polymer membrane and a method for preparing the same, comprising the following steps:
[0131] S1, dissolving cellulose acetate (CA) in dimethylacetamide (DMAC) to form a CA / DMAC solution with a mass fraction of 13%, and adjusting the temperature of the CA / DMAC solution to 25° C. so that the viscosity of the CA / DMAC solution is 2200 mPa·s;
[0132] S2, DMAC: methyl cellulose ether: water are mixed in a ratio of 21:7:72 to obtain a coagulation bath solution, and the temperature of the coagulation bath is adjusted to 25° C. so that the surface tension of the coagulation bath is 57 mN / m;
[0133] S3. Regulate the relative humidity of the ambient air to 40% and the ambient air temperature to 20° C., pour the CA / DMAC solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer membrane.
[0134] Fig.25 The cross-sectional SEM image of the porous polymer membrane prepared in this embodiment is shown. Fig.26 The pore size distribution diagram of the porous polymer membrane prepared in this embodiment is shown. It can be seen from the figure that the pore size distribution of the membrane is uniform, the average pore size is 0.14μm, and the pore size distribution of the membrane in the range of 0.13μm to 0.14μm accounts for about 91%.
[0135] Example 13
[0136] This embodiment provides a porous polymer membrane and a method for preparing the same, comprising the following steps:
[0137] S1, dissolving polyimide (PI) in NMP to form a PI / NMP solution with a mass fraction of 15%, and adjusting the temperature of the PI / NMP solution to 60° C. so that the viscosity of the PI / NMP solution is 25399 mPa·s;
[0138] S2, mixing NMP: methyl cellulose ether: water in a ratio of 81:0.6:18.4 to obtain a coagulation bath solution, and adjusting the temperature of the coagulation bath to 60° C. so that the surface tension of the coagulation bath is 49 mN / m;
[0139] S3. Adjust the relative humidity of the ambient air to 50% and the ambient air temperature to 25° C., pour the PI / NMP solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer membrane.
[0140] Fig. 27 The cross-sectional SEM image of the porous polymer membrane prepared in this embodiment is shown. Fig.28 The pore size distribution diagram of the porous polymer membrane prepared in this embodiment is shown. It can be seen from the figure that the pore size distribution of the membrane is uniform, the average pore size is 0.12μm, and the pores with a pore size range of 0.11μm to 0.12μm account for about 92%.
[0141] Comparative Example 1
[0142] This comparative example provides a polymer membrane and a preparation method thereof, and the specific operation steps are the same as those in Example 1, except that: in step S2, no methyl cellulose ether is added, and the surface tension of the coagulation bath is 60 mM / m. The porous polymer membrane prepared in this example has a wide pore size distribution and an uneven pore size distribution.
[0143] Comparative Example 2
[0144] This comparative example provides a porous polymer membrane and a preparation method thereof, comprising the following steps:
[0145] S1, dissolving PVDF in DMF to form a PVDF / DMF solution with a mass fraction of 30%, and adjusting the temperature of the PVDF / DMF solution to 70° C. so that the viscosity of the PVDF / DMF solution is 112300 mPa·s;
[0146] S2, DMF: hydroxypropyl methylcellulose ether: water are mixed in a ratio of 94:1:5 to obtain a coagulation bath solution, and the temperature of the coagulation bath is adjusted to 70° C. so that the surface tension of the coagulation bath is 33 mN / m;
[0147] S3. Regulate the relative humidity of the ambient air to 40% and the ambient air temperature to 20° C., pour the PVDF / DMF solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer membrane.
[0148] Fig.29 The optical images of the porous polymer membrane prepared in this comparative example and the cross-sectional SEM images of different areas are shown. It can be seen from the figure that the thickness of the polymer membrane in different areas is quite different and the thickness uniformity of the membrane is poor. This may be due to the excessive mass fraction of the polymer in the polymer solution, which leads to excessive viscosity of the solution and cannot match the surface tension of the coagulation bath, resulting in poor spreading and film-forming effect.
[0149] Comparative Example 3
[0150] This comparative example provides a porous polymer membrane and a preparation method thereof, comprising the following steps:
[0151] S1, dissolving PVDF in DMF to form a PVDF / DMF solution with a mass fraction of 1%, and adjusting the temperature of the PVDF / DMF solution to 10° C. so that the viscosity of the PVDF / DMF solution is 4 mPa·s;
[0152] S2, DMF: hydroxypropyl methylcellulose ether: water are mixed in a ratio of 94:1:5 to obtain a coagulation bath solution, and the temperature of the coagulation bath is adjusted to 70° C. so that the surface tension of the coagulation bath is 33 mN / m;
[0153] S3. Regulate the relative humidity of the ambient air to 40% and the ambient air temperature to 20° C., pour the PVDF / DMF solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer membrane.
[0154] Fig.30 The optical images of the porous polymer membrane prepared in this comparative example and the cross-sectional SEM images of different areas are shown. It can be seen from the figure that the structural integrity of the porous polymer membrane is poor, which may be due to the fact that the mass fraction of the polymer in the polymer solution is too small, resulting in too small a solution viscosity, which cannot match the surface tension of the coagulation bath, resulting in incomplete spreading of the membrane.
[0155] Comparative Example 4
[0156] This comparative example provides a porous polymer membrane and a preparation method thereof, comprising the following steps:
[0157] S1, dissolving PVDF in DMF to form a PVDF / DMF solution with a mass fraction of 8%, and adjusting the temperature of the PVDF / DMF solution to 10° C. so that the viscosity of the PVDF / DMF solution is 800 mPa·s;
[0158] S2, DMF: hydroxypropyl methylcellulose ether: water are mixed in a ratio of 1:0:99 to obtain a coagulation bath solution, and the temperature of the coagulation bath is adjusted to 10° C. so that the surface tension of the coagulation bath is 68 mN / m;
[0159] S3. Adjust the relative humidity of the ambient air to 30% and the ambient air temperature to 15° C., pour the PVDF / DMF solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer membrane.
[0160] Fig.31 The cross-sectional SEM image of the porous polymer membrane prepared in this comparative example is shown. Fig.32The pore size distribution diagram of the porous polymer membrane prepared in this comparative example is shown. It can be seen from the figure that the pore size distribution of the membrane is mainly distributed at 0.5812μm and 0.7520μm, and the pore size distribution of the membrane in the range of 0.4762μm to 0.5816μm and 0.622μm to 1.2060μm accounts for about 42% and 45% respectively. The pore size distribution of the membrane is wide and uneven. Because the surface tension of the coagulation bath is too large and cannot match the viscosity of the polymer solution, the solvent in the polymer solution diffuses too quickly into the coagulation bath during the spreading process, resulting in uneven distribution of the pore structure.
[0161] Comparative Example 5
[0162] This comparative example provides a porous polymer membrane and a preparation method thereof, comprising the following steps:
[0163] S1, dissolving PVDF in DMF to form a PVDF / DMF solution with a mass fraction of 8%, and adjusting the temperature of the PVDF / DMF solution to 10° C. so that the viscosity of the PVDF / DMF solution is 800 mPa·s;
[0164] S2, DMF: hydroxypropyl methylcellulose ether: water in a ratio of 75:20:5 is mixed to obtain a coagulation bath solution, and the temperature of the coagulation bath is adjusted to 10° C. so that the surface tension of the coagulation bath is 29 mN / m;
[0165] S3. Adjust the relative humidity of the ambient air to 30% and the ambient air temperature to 15° C., pour the PVDF / DMF solution onto the liquid surface of the coagulation bath solution, and solidify to obtain a porous polymer membrane.
[0166] Fig.33 The optical picture of the porous polymer film prepared in this comparative example is shown, from which it can be seen that the spreading film area of the porous polymer film is small and the film formation is uneven. Since the surface tension of the coagulation bath is too small to match the viscosity of the polymer solution, the polymer solution cannot be effectively spread.
[0167] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a porous polymer membrane, characterized in that: The following steps are involved: S1, dissolving the polymer in an organic solvent to obtain a polymer solution; S2, mixing cellulose ether, an organic solvent and water to obtain a coagulation bath solution; S3, pouring the polymer solution onto the surface of the coagulation bath solution to form a porous polymer film after solidification; In step S1, the viscosity of the polymer solution is 23mPa·s to 170000mPa·s; the mass percentage of the polymer solution is 0.1% to 25%, and the temperature of the polymer solution is 10°C to 70°C; In step S2, the mass ratio of the organic solvent, the cellulose ether and the water is (99.9-0.2):(0.1-9.8):(0-90), and the temperature of the coagulation bath solution is 0° C.-70° C.; The ambient humidity during curing in step S3 is 30% to 80%, and the ambient temperature is 15° C. to 47° C.
2. The method for preparing a porous polymer membrane according to claim 1, characterized in that: The surface tension of the coagulation bath solution is 33 mN / m to 71 mN / m.
3. The method for preparing a porous polymer membrane according to claim 1, characterized in that: The polymer includes any one of polyvinylidene fluoride and its copolymer, polyimide, aramid, cellulose acetate and thermoplastic polyurethane.
4. The method for preparing a porous polymer membrane according to claim 1, characterized in that: The organic solvent includes any one of N,N-dimethylformamide, N-methylpyrrolidone, dimethylacetamide, dimethyl sulfoxide and cyclohexanone.
5. The method for preparing a porous polymer membrane according to claim 1, characterized in that: The cellulose ether includes methyl cellulose ether or hydroxypropyl methyl cellulose ether.
6. A porous polymer membrane, characterized in that: The porous polymer membrane is prepared by the preparation method according to any one of claims 1 to 5, and the pore size of the porous polymer membrane is 0.03 μm to 1.75 μm.
Citation Information
Patent Citations
Porous membrane for permeation separation of small molecules, and preparation method and application thereof
CN110665372A
Preparation method of polymer film
CN116751382A
Method for producing porous resin
JP2009120740A
Porous polyvinylidene fluoride membrane for water treatment, and method for producing porous polyvinylidene fluoride membrane for water treatment
JP2016183301A
Cited By
A polyvinylidene fluoride film used as a battery separator and a preparation method thereof