Environmentally friendly polyurethane paint for interior decoration and production method thereof
Through the combination of modified nano-silica and modified polyurethane emulsion, a high porosity structure and a composite network structure are formed, which solves the problem of high VOC content and insufficient performance of unsaturated polyester paint, and realizes the low VOC and low performance of environmentally friendly polyurethane paint. Balance of high impact resistance and wear resistance.
Patent Information
- Application Number
- CN202410379127.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-03-29
AI Technical Summary
Existing unsaturated polyester paints have high VOC content, which affects environmental protection and human health. At the same time, it is difficult to effectively reduce the VOC content while ensuring the performance of the paint film, especially in terms of impact resistance and wear resistance.
A combination of modified nanosilica and modified polyurethane emulsion is used to react with raw materials such as modified siloxane, polyethylene glycol and isophorone diisocyanate to form a highly porous nanosilica structure, which is combined with light Ingredients such as initiator and sodium hydroxymethylcellulose in the emulsion form a stable composite network structure to improve the performance of the paint film.
It effectively reduces the VOC content of polyurethane paint, while improving the impact resistance and wear resistance of the paint film, ensuring a balance between the environmental performance and mechanical properties of environmentally friendly polyurethane paint.
Smart Images

Figure SMS_1 
Figure SMS_10 
Figure SMS_12
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyurethane paint processing, and in particular to an environmentally friendly polyurethane paint for interior decoration and a production method thereof. Background Art
[0002] With the improvement of people's quality of life, interior decoration has become an important part of modern life. Unsaturated polyester paint, as a commonly used paint, is widely popular due to its excellent color, glossiness and weather resistance. Unsaturated polyester paint is a multi-component paint, a thick paint made mainly of polyester resin as the main film-forming material. It has the advantages of rich colors, full paint film, thick layer, hard surface and large paint film thickness.
[0003] Unsaturated polyester paint in the prior art is usually composed of a mixture of multiple chemical substances. In order to adjust the viscosity, drying speed and other properties of the unsaturated polyester paint, it is usually necessary to add organic solvents, which causes the chemical substances inside the unsaturated polyester paint to undergo complex chemical reactions during the curing process. These reactions are often accompanied by the generation of volatile products, which in turn increase the VOC content. This not only pollutes the environment and is not environmentally friendly, but also poses a potential threat to human health. At present, the methods for reducing the VOC content of unsaturated polyester paint mainly include selecting raw materials with low VOC content, optimizing production processes, and using environmentally friendly additives. However, these methods often lead to a decrease in paint film performance, especially in terms of impact resistance and wear resistance. Therefore, how to effectively reduce the VOC content of unsaturated polyester paint while ensuring the performance of the paint film has become a difficulty in technological innovation in this field.
[0004] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention
[0005] The purpose of the present invention is to provide an environmentally friendly polyurethane paint for interior decoration and a production method thereof, so as to solve the technical problems in the prior art that the VOC content of polyurethane paint is high and not environmentally friendly, and the performance of polyurethane paint film needs to be further improved.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] An environmentally friendly polyurethane paint for interior decoration, comprising the following components by weight: 16-18 parts of modified nano silicon dioxide, 90-95 parts of modified polyurethane emulsion, 6-9 parts of purified water, 2-8 parts of pigment, 2-3 parts of additive, and 1.2-2.5 parts of photoinitiator;
[0008] The modified polyurethane emulsion is processed by the following steps:
[0009] A1. Add modified siloxane, polyethylene glycol 400 and tetrahydrofuran into a nitrogen-protected reactor and stir. Raise the temperature of the reactor to 55-60° C., slowly drop isophorone diisocyanate into the reactor, and heat-retain for 70-90 min. Add (E)-oct-4-ene-1,8-diacid into the reactor, and heat-retain for 3-5 h. Post-treat to obtain modified polyurethane.
[0010] The synthetic reaction principle of modified polyurethane is:
[0011]
[0012] Where:
[0013]
[0014] A2. Add the modified polyurethane and emulsion into a reaction kettle and stir at room temperature for 50-60 minutes to obtain a modified polyurethane emulsion.
[0015] Furthermore, the photoinitiator is 2-hydroxy-2-methyl-1-phenylpropanone, the pigment is an inorganic pigment with a particle size of 0.5-1.5 μm, and the additives are composed of a cosolvent, a defoamer, a wetting agent, a slip agent, and a leveling agent in a weight ratio of 5:1:2:1:1. The cosolvent is dipropylene glycol methyl ether, the defoamer is defoamer GP330, the wetting agent is an amide gemini quaternary ammonium salt, the slip agent is polyvinyl alcohol, and the leveling agent is an acrylic leveling agent.
[0016] Furthermore, in step A1, the amount ratio of modified siloxane, polyethylene glycol 400, isophorone diisocyanate and (E)-oct-4-ene-1,8-diacid is 2mol:5mol:7mol:2mol, and the amount ratio of polyethylene glycol 400 and tetrahydrofuran is 1g:6mL; the post-treatment operation in step A1 includes: after the reaction is completed, the temperature of the reactor is reduced to room temperature, 0.5mol / L sodium hydroxide solution is added dropwise to the reactor, the pH of the reaction system is adjusted to 7, the temperature of the reactor is increased to 55-60°C, and the solvent is evaporated under reduced pressure to obtain a modified polyurethane; in step A2, the emulsion is composed of sodium hydroxymethyl cellulose, polyethylene imine, sodium hexadecylbenzene sulfonate and purified water in a weight ratio of 2g:5g:3g:100mL, and the amount ratio of the modified polyurethane to the emulsion is 1g:3mL.
[0017] Furthermore, the preparation method of the modified siloxane is: 1,1,3,3,5,5,7,7,9,9-decamethylpentasiloxane, vinyl alcohol, tetrahydrofuran and a catalyst are added to a reactor and stirred, the temperature of the reactor is increased to reflux, the reaction is kept warm for 6-8 hours, and the modified siloxane is obtained by post-treatment.
[0018] The synthetic reaction principle of modified siloxane is:
[0019]
[0020] Furthermore, the amount ratio of the 1,1,3,3,5,5,7,7,9,9-decamethylpentasiloxane and vinyl alcohol is 1 mol:2 mol, the amount ratio of the 1,1,3,3,5,5,7,7,9,9-decamethylpentasiloxane, tetrahydrofuran and catalyst is 1 g:4 mL:0.02 g, the catalyst is chloroplatinic acid, and the post-treatment operation includes: the post-treatment operation includes, after the reaction is completed, evaporating the solvent under reduced pressure to obtain modified siloxane.
[0021] Further, the modified nano-silicon dioxide is processed by the following steps:
[0022] B1. Add the dispersion into a reactor, increase the stirring speed of the reactor to 680-780 r / min, add ethyl orthosilicate into the reactor, stir at room temperature for 60-80 min, and perform post-treatment to obtain a crude nano-silicon dioxide product;
[0023] B2. Put the crude nano-silicon dioxide into a muffle furnace, first increase the temperature of the muffle furnace to 95°C at a heating rate of 3°C / min, keep the temperature for 60 minutes, then increase the temperature of the muffle furnace to 600°C at a heating rate of 5°C / min, keep the temperature for 200 minutes, and naturally cool the muffle furnace to room temperature, and post-treat to obtain nano-silicon dioxide;
[0024] B3. Add nano-silica, modifier and 90 wt% methanol solution into a reactor, and perform ultrasonic dispersion for 30-50 min at room temperature. Add hydrochloric acid into the reactor, increase the temperature of the reactor to reflux the system, and keep the reaction warm for 4-5 h. Post-treat to obtain modified nano-silica.
[0025] The synthetic reaction principle of modified nano-silica is:
[0026]
[0027] Where: It is nano silicon dioxide.
[0028] Furthermore, the dispersion in step B1 is composed of diethanolamine, sodium p-fluorobenzoate, an active agent, and deionized water in a dosage ratio of 1g:5g:2g:40mL, and the active agent is one or two of polyquaternium-16 and guar gum; the post-processing operation in step B1 includes: after the reaction is completed, stopping stirring, filtering, transferring the filter cake to a drying oven with a temperature of 75-85°C, and vacuum drying to constant weight to obtain a crude nano-silicon dioxide product; the post-processing operation in step B2 includes: mixing the calcined particles and a 60vt% ethanol solution in a dosage ratio of 1g:10mL, ultrasonically dispersing for 6-8h, standing overnight, and skimming the upper layer. The suspended residue, the lower solid matter is filtered and washed with purified water for 3 times and then dried, the filter cake is transferred to a drying oven at a temperature of 75-85°C, and dried to constant weight to obtain nano silicon dioxide; in step B3, the amount ratio of nano silicon dioxide, modifier, 90wt% methanol solution and hydrochloric acid is 5g:3g:50mL:4mL, and the concentration of the hydrochloric acid is 11.5-12.5mol / L, and the post-treatment operation in step B3 includes: after the reaction is completed, filtering, washing the filter cake with purified water for 5 times and then drying, transferring the filter cake to a drying oven at a temperature of 65-75°C, and drying to constant weight to obtain modified nano silicon dioxide.
[0029] Further, the modifier is processed by the following steps:
[0030] C1, adding 3-aminoadipic acid, 2,4-octadiene-1-ol, a catalyst and toluene into a reaction kettle and stirring, raising the temperature of the reaction kettle to a micro-reflux of the system, keeping the temperature for reaction for 6-8 hours, and post-treating the intermediate I;
[0031] The synthetic reaction principle of intermediate I is:
[0032]
[0033] C2, adding intermediate I, benzyl chloroformate, sodium carbonate and tetrahydrofuran into a reaction kettle and stirring, raising the temperature of the reaction kettle to 50-60°C, keeping the temperature for 5-7h, and post-treating to obtain intermediate II;
[0034] The synthetic reaction principle of intermediate II is:
[0035]
[0036]
[0037] C3. Add intermediate II and tetrahydrofuran into a nitrogen-protected reactor and stir. Raise the temperature of the reactor to 45-55°C. Add isocyanatepropyltriethoxysilane into the reactor and keep the reaction temperature for 3-5h. Post-treat to obtain a modifier.
[0038] The synthetic reaction principle of the modifier is:
[0039]
[0040] Further, in step C1, the ratio of 3-aminoadipic acid and 2,4-octadiene-1-ol is 1 mol: 1 mol, and the ratio of 2,4-octadiene-1-ol, catalyst and toluene is 3 g: 0.1 g: 20 mL; the post-treatment operation in step C1 includes: after the reaction is completed, toluene is distilled off under reduced pressure to obtain intermediate I; in step C2, the ratio of intermediate I and benzyl chloroformate is 1 mol: 2.1 mol, and the benzyl chloroformate, sodium carbonate, tetrahydrofuran are used. The amount ratio of furan is 3g:2g:20mL; the post-processing operation in step C2 includes: after the reaction is completed, filtering, transferring the filtrate to a reactor, and distilling off the solvent under reduced pressure to obtain intermediate II; in step C3, the amount ratio of intermediate II and isocyanatepropyltriethoxysilane is 1mol:1mol, and the amount ratio of intermediate II and tetrahydrofuran is 1g:6mL; the post-processing operation in step C3 includes: after the reaction is completed, distilling off tetrahydrofuran under reduced pressure to obtain a modifier.
[0041] A method for producing an environmentally friendly polyurethane paint for interior decoration comprises the following steps:
[0042] S1, adding additives and purified water into the reactor and ultrasonically dispersing for 20-30 minutes;
[0043] S2. Continue to add pigment, modified nano-silicon dioxide, modified polyurethane emulsion and photoinitiator into the reaction kettle, and perform ultrasonic dispersion for 30-50 minutes to obtain polyurethane paint.
[0044] The present invention has the following beneficial effects:
[0045] 1. The present invention uses diethylene glycol amine as a pH regulator and sodium p-fluorobenzoate and an active agent as a surfactant to improve the dispersibility and stability of the dispersion system and prevent the agglomeration of nanoparticles. Ethyl orthosilicate is used as a raw material, and the ethyl orthosilicate is hydrolyzed and reorganized in the dispersion to prepare silicon dioxide with a three-dimensional network structure. High-speed stirring helps to maintain the uniformity of the system and prevent the generated silicon dioxide particles from agglomerating, thereby obtaining nano-scale silicon dioxide particles. High-temperature calcination treatment can promote the carbonization of organic matter remaining on the silicon dioxide and remove it from the silicon dioxide, making the silicon dioxide particles purer. At the same time, since there are a large number of hydroxyl groups on the surface of the silicon dioxide particles, these hydroxyl groups will undergo condensation reactions at high temperatures to release water and form new silicon-oxygen bonds. The space left by the water release forms channels on the silicon dioxide, thereby improving the porosity of the silicon dioxide particles. The high-porosity nano-silica structure provides a large number of adsorption sites and channels for VOC molecules, and fixes them on the surface by physical adsorption, so that the silicon dioxide has good adsorption performance for VOC molecules.
[0046] 2. The present invention uses a catalyst to catalyze the reaction of 3-aminoadipic acid and 2,4-octadiene-1-ol in proportion, so that the carboxyl group on the 3-aminoadipic acid and the hydroxyl group on the 2,4-octadiene-1-ol undergo an esterification reaction in toluene and a high temperature environment to form an intermediate I in which 2,4-octadiene-1-ol is grafted and modified on one end of the 3-aminoadipic acid; the amino group on the intermediate I undergoes a nucleophilic substitution reaction with benzyl chloroformate in a tetrahydrofuran environment with sodium carbonate as an acid binding agent to generate a benzyl-protected intermediate II; the carboxyl group on the intermediate II undergoes a condensation reaction with the isocyanate group on isocyanatopropyltriethoxysilane, A modifier modified with siloxane is formed; under acidic conditions, the siloxane bonds on the modifier are hydrolyzed and react with active functional groups on the surface of nano-silica to form chemical modification, and the benzyl groups on the modifier are hydrolyzed to reform amino groups to prepare modified nano-silica; the nano-silica itself has a high porosity and has adsorption properties for VOC waste gas, and the amino groups formed by hydrolysis on the modifier increase the number of surface active sites of the nano-silica, and hydrogen bonds or other interaction forces can be formed between the amino groups and the VOC molecules, and this interaction can further enhance the adsorption capacity of the nano-silica for VOC waste gas.
[0047] 3. The present invention forms a modified siloxane containing alcohol hydroxyl end-capping by a silylation reaction of 1,1,3,3,5,5,7,7,9,9-decamethylpentasiloxane and vinyl alcohol under catalyst conditions, and then uses the modified siloxane, polyethylene glycol and isophorone diisocyanate as raw materials and (E)-oct-4-ene-1,8-diacid as a chain extender for a condensation reaction to prepare a modified polyurethane with siloxane-ethylene blocks. Since the polyurethane itself has excellent mechanical properties and combined with the characteristics of the siloxane segment, the modified polyurethane can give the polyurethane paint coating higher impact resistance and wear resistance; the siloxane segment has excellent stability and low volatility. By adjusting the content and proportion of the siloxane segment in the modified polyurethane, the balance between the performance of the paint film and the VOC content is optimized, and the VOC content of the water-based paint is reduced while maintaining or improving the performance of the paint film; in an emulsion composed of sodium hydroxymethyl cellulose, polyethyleneimine, sodium hexadecylbenzenesulfonate and purified water, Sodium hydroxymethyl cellulose, polyethyleneimine and sodium hexadecylbenzene sulfonate can all be used as emulsifiers and stabilizers. They work together to effectively reduce the surface tension of the system, improve the stability of the emulsion, and promote the uniform dispersion of nano or micron particles in the system, so that the modified polyurethane is uniformly emulsified in the emulsion to form a stable aqueous emulsion. Polyethyleneimine is a polymer containing amino groups, which can interact with the amino groups on the surface of modified silica, further enhancing its dispersibility in the emulsion and promoting the uniform dispersion of modified nano silica in the emulsion; under the action of the photoinitiator, the unsaturated bonds on the modified nano silica and the modified polyurethane are cross-linked to form a stable composite interpenetrating network structure. This structure can effectively disperse stress and improve the impact resistance of the paint film, making it not easy to break when subjected to external forces. At the same time, the flexibility of polyurethane and the reinforcing effect of nano silica are combined to further improve the wear resistance of the paint film. DETAILED DESCRIPTION
[0048] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] Example 1
[0050] A method for producing an environmentally friendly polyurethane paint for interior decoration in this embodiment comprises the following steps:
[0051] S1. Preparation of silicon dioxide
[0052] Diethanolamine, sodium p-fluorobenzoate, polyquaternium-16 and deionized water were uniformly mixed in a dosage ratio of 1 g:5 g:2 g:40 mL to obtain a dispersion for later use;
[0053] Weigh: 500 mL of the dispersion was added to a reactor, the stirring speed of the reactor was increased to 680 r / min, 30 g of ethyl orthosilicate was added to the reactor, and the mixture was stirred at room temperature for 60 min. Stirring was stopped, and the filter cake was transferred to a drying oven at 75°C and vacuum dried to constant weight to obtain a crude nano-silicon dioxide product;
[0054] The crude nano-silicon dioxide was placed in a muffle furnace, which was first heated to 95°C at a heating rate of 3°C / min and kept warm for 60 minutes. The temperature of the muffle furnace was then raised to 600°C at a heating rate of 5°C / min and kept warm for 200 minutes. The muffle furnace was naturally cooled to room temperature, and the calcined particles and 60vt% ethanol solution were mixed at a dosage ratio of 1g:10mL, ultrasonically dispersed for 6h, allowed to stand overnight, and the upper suspended residue was skimmed off. The lower solid was filtered and washed 3 times with purified water to dryness. The filter cake was transferred to a drying oven at a temperature of 75°C and dried to constant weight to obtain nano-silicon dioxide.
[0055] S2. Preparation of modifier
[0056] Weigh: 16.1 g of 3-aminoadipic acid, 12.6 g of 2,4-octadien-1-ol, 0.42 g of tetraethyl titanate and 84 mL of toluene, add them into a reaction kettle and stir, raise the temperature of the reaction kettle to a micro-reflux state, keep the temperature for 6 hours, and evaporate toluene under reduced pressure to obtain intermediate I;
[0057] Weigh: 26.9 g of intermediate I, 34.1 g of benzyl chloroformate, 22.7 g of sodium carbonate, and 227 mL of tetrahydrofuran, add them into a reactor and stir, raise the temperature of the reactor to 50°C, keep the temperature for 5 hours, lower the temperature of the reactor to room temperature, filter, transfer the filtrate to the reactor, and evaporate the solvent under reduced pressure to obtain intermediate II;
[0058] Weigh: 53.7 g of intermediate II and 322 mL of tetrahydrofuran are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 45° C. 23.1 g of isocyanatepropyltriethoxysilane is added to the reactor. The reaction is kept warm for 3 h. The tetrahydrofuran is evaporated under reduced pressure to obtain a modifier.
[0059] S3. Preparation of modified silicon dioxide
[0060] Weigh: 50g of nano-silica, 30g of modifier and 500mL of 90wt% methanol solution and add them to a reactor. At room temperature, ultrasonically disperse for 30min, add 40mL of 11.5mol / L hydrochloric acid to the reactor, raise the temperature of the reactor to reflux the system, and keep the reaction for 4h. Lower the temperature of the reactor to room temperature, filter, wash the filter cake with purified water 5 times and then drain it, transfer the filter cake to a drying oven at a temperature of 65°C, and dry it to constant weight to obtain modified nano-silica.
[0061] S4. Preparation of modified polyurethane
[0062] Weigh: 35.6 g of 1,1,3,3,5,5,7,7,9,9-decamethylpentasiloxane, 88.1 g of vinyl alcohol, 142.4 mL of tetrahydrofuran and 0.71 g of chloroplatinic acid, add into a reaction kettle and stir, raise the temperature of the reaction kettle to reflux, keep the temperature to react for 6 hours, and evaporate the solvent under reduced pressure to obtain modified siloxane;
[0063] Weigh: 89.0 g of modified siloxane, 200 g of polyethylene glycol 400, and 1200 mL of tetrahydrofuran are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 55° C., 155.6 g of isophorone diisocyanate is slowly added dropwise to the reactor, and the reaction is kept warm for 70 min. 34.4 g of (E)-oct-4-ene-1,8-diacid is added to the reactor, and the reaction is kept warm for 3 h. The temperature of the reactor is lowered to room temperature, and 0.5 mol / L sodium hydroxide solution is added dropwise to the reactor, the pH of the reaction system is adjusted to 7, the temperature of the reactor is raised to 55° C., and the solvent is evaporated under reduced pressure to obtain a modified polyurethane.
[0064] S5. Preparation of modified polyurethane emulsion
[0065] Mix sodium hydroxymethylcellulose, polyethyleneimine, sodium hexadecylbenzenesulfonate and purified water in a weight ratio of 2g:5g:3g:100mL to obtain an emulsion for later use;
[0066] Weigh: 200 g of modified polyurethane and 600 mL of emulsion, add into a reactor, stir at room temperature for 50 min, and obtain modified polyurethane emulsion.
[0067] S6. Preparation of polyurethane paint
[0068] Dipropylene glycol methyl ether, defoamer GP330, amide-based gemini quaternary ammonium salt, polyvinyl alcohol, and acrylic leveling agent are uniformly mixed in a weight ratio of 5:1:2:1:1 to obtain an additive, which is set aside. The product model of the acrylic leveling agent is MONENG-1153;
[0069] Weigh: 200 g of additive and 600 g of purified water are added to a reactor and ultrasonically dispersed for 20 minutes. 200 g of inorganic pigment with a particle size of 0.5-1.5 μm, 1600 g of modified nano-silica, 9000 g of modified polyurethane emulsion and 120 g of 2-hydroxy-2-methyl-1-phenylacetone are continuously added to the reactor and ultrasonically dispersed for 30 minutes to obtain a polyurethane paint.
[0070] Example 2
[0071] A method for producing an environmentally friendly polyurethane paint for interior decoration in this embodiment comprises the following steps:
[0072] S1. Preparation of silicon dioxide
[0073] Diethanolamine, sodium p-fluorobenzoate, guar gum and deionized water were uniformly mixed in a dosage ratio of 1g:5g:2g:40mL to obtain a dispersion liquid for later use;
[0074] Weigh: 500 mL of the dispersion was added to a reactor, the stirring speed of the reactor was increased to 730 r / min, 30 g of ethyl orthosilicate was added to the reactor, and the mixture was stirred at room temperature for 70 min. Stirring was stopped, and the filter cake was transferred to a drying oven at 80° C. and vacuum dried to constant weight to obtain a crude nano-silicon dioxide product;
[0075] The crude nano-silicon dioxide was placed in a muffle furnace, which was first heated to 95°C at a heating rate of 3°C / min and kept warm for 60 minutes. The temperature of the muffle furnace was then raised to 600°C at a heating rate of 5°C / min and kept warm for 200 minutes. The muffle furnace was naturally cooled to room temperature, and the calcined particles and 60vt% ethanol solution were mixed at a dosage ratio of 1g:10mL, ultrasonically dispersed for 7h, allowed to stand overnight, and the upper suspended residue was skimmed off. The lower solid was filtered and washed 3 times with purified water to dryness. The filter cake was transferred to a drying oven at 80°C and dried to constant weight to obtain nano-silicon dioxide.
[0076] S2. Preparation of modifier
[0077] Weigh: 16.1 g of 3-aminoadipic acid, 12.6 g of 2,4-octadiene-1-ol, 0.42 g of tetraethyl titanate and 84 mL of toluene, add them into a reaction kettle and stir, raise the temperature of the reaction kettle to a micro-reflux state, keep the temperature for 7 h, and evaporate toluene under reduced pressure to obtain intermediate I;
[0078] Weigh: 26.9 g of intermediate I, 34.1 g of benzyl chloroformate, 22.7 g of sodium carbonate, and 227 mL of tetrahydrofuran, add them into a reactor and stir, raise the temperature of the reactor to 55° C., keep the temperature for 6 h, lower the temperature of the reactor to room temperature, filter, transfer the filtrate to the reactor, and evaporate the solvent under reduced pressure to obtain intermediate II;
[0079] Weigh: 53.7 g of intermediate II and 322 mL of tetrahydrofuran are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 50° C. 23.1 g of isocyanatepropyltriethoxysilane is added to the reactor. The reaction is kept warm for 4 hours, and the tetrahydrofuran is evaporated under reduced pressure to obtain a modifier.
[0080] S3. Preparation of modified silicon dioxide
[0081] Weigh: 50g of nano-silica, 30g of modifier and 500mL of 90wt% methanol solution and add them to a reactor. At room temperature, ultrasonically disperse for 40min, add 40mL of 12.0mol / L hydrochloric acid to the reactor, raise the temperature of the reactor to reflux the system, and keep the reaction for 4.5h. Lower the temperature of the reactor to room temperature, filter, wash the filter cake with purified water 5 times and then drain it, transfer the filter cake to a drying oven at a temperature of 70°C, and dry it to constant weight to obtain modified nano-silica.
[0082] S4. Preparation of modified polyurethane
[0083] Weigh: 35.6 g of 1,1,3,3,5,5,7,7,9,9-decamethylpentasiloxane, 88.1 g of vinyl alcohol, 142.4 mL of tetrahydrofuran and 0.71 g of chloroplatinic acid, add into a reaction kettle and stir, raise the temperature of the reaction kettle to reflux, keep the temperature to react for 7 hours, and evaporate the solvent under reduced pressure to obtain modified siloxane;
[0084] Weigh: 89.0 g of modified siloxane, 200 g of polyethylene glycol 400, and 1200 mL of tetrahydrofuran, add them into a nitrogen-protected reactor and stir, raise the temperature of the reactor to 57°C, slowly drop 155.6 g of isophorone diisocyanate into the reactor, and keep the temperature for 80 min, add 34.4 g of (E)-oct-4-ene-1,8-diacid into the reactor, keep the temperature for 4 h, lower the temperature of the reactor to room temperature, drop 0.5 mol / L sodium hydroxide solution into the reactor, adjust the pH of the reaction system to 7, raise the temperature of the reactor to 57°C, and evaporate the solvent under reduced pressure to obtain a modified polyurethane.
[0085] S5. Preparation of modified polyurethane emulsion
[0086] Mix sodium hydroxymethylcellulose, polyethyleneimine, sodium hexadecylbenzenesulfonate and purified water in a weight ratio of 2g:5g:3g:100mL to obtain an emulsion for later use;
[0087] Weigh: 200 g of modified polyurethane and 600 mL of emulsion, add into a reactor, stir at room temperature for 55 min, and obtain modified polyurethane emulsion.
[0088] S6. Preparation of polyurethane paint
[0089] Dipropylene glycol methyl ether, defoamer GP330, amide-based gemini quaternary ammonium salt, polyvinyl alcohol, and acrylic leveling agent are uniformly mixed in a weight ratio of 5:1:2:1:1 to obtain an additive, which is set aside. The product model of the acrylic leveling agent is MONENG-1153;
[0090] Weigh: 250 g of additive and 750 g of purified water are added to a reactor and ultrasonically dispersed for 25 minutes. 500 g of inorganic pigment with a particle size of 0.5-1.5 μm, 1700 g of modified nano-silica, 9250 g of modified polyurethane emulsion, and 185 g of 2-hydroxy-2-methyl-1-phenylacetone are continued to be added to the reactor, and ultrasonically dispersed for 40 minutes to obtain a polyurethane paint.
[0091] Example 3
[0092] A method for producing an environmentally friendly polyurethane paint for interior decoration in this embodiment comprises the following steps:
[0093] S1. Preparation of silicon dioxide
[0094] Diethanolamine, sodium p-fluorobenzoate, polyquaternium-16, guar gum, and deionized water were uniformly mixed in an amount ratio of 1g:5g:1g:1g:40mL to obtain a dispersion, which was set aside;
[0095] Weigh: 500 mL of the dispersion was added to a reactor, the stirring speed of the reactor was increased to 780 r / min, 30 g of ethyl orthosilicate was added to the reactor, and the mixture was stirred at room temperature for 80 min. Stirring was stopped, and the filter cake was transferred to a drying oven at 85°C and vacuum dried to constant weight to obtain a crude nano-silicon dioxide product;
[0096] The crude nano-silicon dioxide was placed in a muffle furnace, which was first heated to 95°C at a heating rate of 3°C / min and kept warm for 60 minutes. The temperature of the muffle furnace was then raised to 600°C at a heating rate of 5°C / min and kept warm for 200 minutes. The muffle furnace was naturally cooled to room temperature, and the calcined particles and 60vt% ethanol solution were mixed at a dosage ratio of 1g:10mL, ultrasonically dispersed for 8h, allowed to stand overnight, and the upper suspended residue was skimmed off. The lower solid was filtered and washed 3 times with purified water to dryness. The filter cake was transferred to a drying oven at 85°C and dried to constant weight to obtain nano-silicon dioxide.
[0097] S2. Preparation of modifier
[0098] Weigh: 16.1 g of 3-aminoadipic acid, 12.6 g of 2,4-octadien-1-ol, 0.42 g of tetraethyl titanate and 84 mL of toluene, add them into a reaction kettle and stir, raise the temperature of the reaction kettle to a micro-reflux state, keep the temperature for 8 h, and evaporate toluene under reduced pressure to obtain intermediate I;
[0099] Weigh: 26.9 g of intermediate I, 34.1 g of benzyl chloroformate, 22.7 g of sodium carbonate, and 227 mL of tetrahydrofuran, add them into a reactor and stir, raise the temperature of the reactor to 60°C, keep the temperature for 7 hours, lower the temperature of the reactor to room temperature, filter, transfer the filtrate to the reactor, and evaporate the solvent under reduced pressure to obtain intermediate II;
[0100] Weigh: 53.7 g of intermediate II and 322 mL of tetrahydrofuran are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 55° C. 23.1 g of isocyanatepropyltriethoxysilane is added to the reactor. The reaction is kept warm for 5 hours, and the tetrahydrofuran is evaporated under reduced pressure to obtain a modifier.
[0101] S3. Preparation of modified silicon dioxide
[0102] Weigh: 50g of nano-silica, 30g of modifier and 500mL of 90wt% methanol solution and add them to a reactor. At room temperature, ultrasonic dispersion is performed for 50min. 40mL of 12.5mol / L hydrochloric acid is added to the reactor. The temperature of the reactor is raised to reflux and the reaction is kept warm for 5h. The temperature of the reactor is lowered to room temperature and filtered. The filter cake is washed with purified water 5 times and then dried. The filter cake is transferred to a drying oven at 75°C and dried to constant weight to obtain modified nano-silica.
[0103] S4. Preparation of modified polyurethane
[0104] Weigh: 35.6 g of 1,1,3,3,5,5,7,7,9,9-decamethylpentasiloxane, 88.1 g of vinyl alcohol, 142.4 mL of tetrahydrofuran and 0.71 g of chloroplatinic acid, add into a reaction kettle and stir, raise the temperature of the reaction kettle to reflux, keep the temperature to react for 8 hours, and evaporate the solvent under reduced pressure to obtain modified siloxane;
[0105] Weigh: 89.0 g of modified siloxane, 200 g of polyethylene glycol 400, and 1200 mL of tetrahydrofuran are added to a nitrogen-protected reactor and stirred. The temperature of the reactor is raised to 60° C., 155.6 g of isophorone diisocyanate is slowly added dropwise to the reactor, and the reaction is kept warm for 90 min. 34.4 g of (E)-oct-4-ene-1,8-diacid is added to the reactor, and the reaction is kept warm for 5 h. The temperature of the reactor is lowered to room temperature, and 0.5 mol / L sodium hydroxide solution is added dropwise to the reactor, the pH of the reaction system is adjusted to 7, the temperature of the reactor is raised to 60° C., and the solvent is evaporated under reduced pressure to obtain a modified polyurethane.
[0106] S5. Preparation of modified polyurethane emulsion
[0107] Mix sodium hydroxymethylcellulose, polyethyleneimine, sodium hexadecylbenzenesulfonate and purified water in a weight ratio of 2g:5g:3g:100mL to obtain an emulsion for later use;
[0108] Weigh: 200 g of modified polyurethane and 600 mL of emulsion, add into a reactor, stir at room temperature for 60 min, and obtain modified polyurethane emulsion.
[0109] S6. Preparation of polyurethane paint
[0110] Dipropylene glycol methyl ether, defoamer GP330, amide-based gemini quaternary ammonium salt, polyvinyl alcohol, and acrylic leveling agent are uniformly mixed in a weight ratio of 5:1:2:1:1 to obtain an additive, which is set aside. The product model of the acrylic leveling agent is MONENG-1153;
[0111] Weigh: 300 g of additive and 900 g of purified water are added to a reactor and ultrasonically dispersed for 30 minutes. 800 g of inorganic pigment with a particle size of 0.5-1.5 μm, 1800 g of modified nano-silicon dioxide, 9500 g of modified polyurethane emulsion and 250 g of 2-hydroxy-2-methyl-1-phenylacetone are continuously added to the reactor and ultrasonically dispersed for 50 minutes to obtain a polyurethane paint.
[0112] Comparative Example 1
[0113] The difference between this comparative example and Example 3 is that steps S2-S3 are eliminated, and the modified nano-silicon dioxide in step S6 is replaced by the nano-silicon dioxide in step S1.
[0114] Comparative Example 2
[0115] The difference between this comparative example and Example 3 is that in step S2, 3-aminoadipic acid is replaced by an equimolar amount of adipic acid, and intermediate II is replaced by an equimolar amount of the prepared intermediate I.
[0116] Comparative Example 3
[0117] The difference between this comparative example and Example 3 is that the modified siloxane in step S4 is replaced by an equal molar amount of polyethylene glycol 400.
[0118] Comparative Example 4
[0119] The difference between this comparative example and Example 3 is that no photoinitiator is added in step S6.
[0120] Performance Test:
[0121] The environmental protection, impact resistance and wear resistance of the polyurethane paints prepared in Examples 1-3 and Comparative Examples 1-4 were tested, wherein the environmental protection performance of the polyurethane paint was determined by referring to the standard GB / T 23986-2009 "Determination of the volatile organic compound (VOC) content of paints and varnishes by gas chromatography" to determine the VOC content of the sample; the impact resistance, adhesion and wear resistance tests were performed by evenly coating the sample on a sanded wooden board, and then placing it in an oven with ultraviolet light irradiation at a wavelength of 365 nm, setting the oven temperature to 60°C, drying for 8 hours, and forming a paint film with a thickness of 50 μm on the wooden board. The impact resistance of the paint film was determined according to the standard GB / T1732-2020 "Determination of impact resistance of paint film", and the mass loss m1 of the paint film after the rubber grinding wheel rotates 500 times at 50 r / min was tested according to the standard GB / T 1768-2006 "Determination of wear resistance of paints and varnishes by rotating rubber grinding wheel method" was measured, and according to the formula Calculate the mass wear, where m0 is the initial weight of the paint film. The specific test results are shown in the following table:
[0122]
[0123]
[0124] Data Analysis:
[0125] A comparative analysis of the data in the above table shows that the polyurethane paint prepared by the present invention has a VOC content reduced to 20 g / L, an impact resistance of 50 kg·cm, and a mass wear reduced to 1.27%. All test data are better than those of the comparative example, indicating that the present invention optimizes the segment composition structure of the modified polyurethane and prepares highly porous modified silica to cooperate with each other, which not only effectively reduces the VOC content of the polyurethane paint, but also improves the impact resistance and wear resistance of the polyurethane paint film.
[0126] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
[0127] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0128] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. An environmentally friendly polyurethane paint for interior decoration, characterized in that: The invention comprises the following components in parts by weight: 16-18 parts of modified nano silicon dioxide, 90-95 parts of modified polyurethane emulsion, 6-9 parts of purified water, 2-8 parts of pigment, 2-3 parts of additive, and 1.2-2.5 parts of photoinitiator; The modified polyurethane emulsion is processed by the following steps: A1. Add modified siloxane, polyethylene glycol 400 and tetrahydrofuran into a nitrogen-protected reactor and stir. Raise the temperature of the reactor to 55-60° C., slowly drop isophorone diisocyanate into the reactor, and heat-retain for 70-90 min. Add (E)-oct-4-ene-1,8-diacid into the reactor, and heat-retain for 3-5 h. Post-treat to obtain modified polyurethane. A2, adding modified polyurethane and emulsion into a reactor, stirring at room temperature for 50-60min, to obtain a modified polyurethane emulsion, wherein the emulsion is composed of sodium hydroxymethyl cellulose, polyethyleneimine, sodium hexadecylbenzene sulfonate and purified water in a weight ratio of 2g:5g:3g:100mL, and the amount ratio of the modified polyurethane to the emulsion is 1g:3mL; The preparation method of modified siloxane is as follows: 1,1,3,3,5,5,7,7,9,9-decamethylpentasiloxane, vinyl alcohol, tetrahydrofuran and a catalyst are added into a reaction kettle and stirred, the temperature of the reaction kettle is increased to reflux of the system, the reaction is kept warm for 6-8 hours, and the modified siloxane is obtained by post-treatment, wherein the amount ratio of the 1,1,3,3,5,5,7,7,9,9-decamethylpentasiloxane to the vinyl alcohol is 1 mol:2 mol; Modified nano-silica is processed by the following steps: B1, the dispersion is added to a reactor, the reactor stirring speed is increased to 680-780r / min, tetraethyl orthosilicate is added to the reactor, stirred at room temperature for 60-80min, and post-processed to obtain a crude nano silicon dioxide product, wherein the dispersion is composed of diethanolamine, sodium p-fluorobenzoate, an activating agent, and deionized water in an amount ratio of 1g:5g:2g:40mL, and the activating agent is one or both of polyquaternium-16 and guar gum; B2. Put the crude nano-silicon dioxide into a muffle furnace, first increase the temperature of the muffle furnace to 95°C at a heating rate of 3°C / min, keep the temperature for 60 minutes, then increase the temperature of the muffle furnace to 600°C at a heating rate of 5°C / min, keep the temperature for 200 minutes, and naturally cool the muffle furnace to room temperature, and post-treat to obtain nano-silicon dioxide; B3, adding nano-silica, a modifier and a 90wt% methanol solution into a reactor, ultrasonically dispersing for 30-50min at room temperature, adding hydrochloric acid into the reactor, raising the temperature of the reactor to reflux the system, keeping the temperature for 4-5h, and post-treating to obtain modified nano-silica; The modifier is processed by the following steps: C1, adding 3-aminohexanedioic acid, 2,4-octadiene-1-ol, catalyst 2 and toluene into a reactor and stirring, raising the temperature of the reactor to a micro-reflux of the system, keeping the temperature for reaction for 6-8h, and post-treating the intermediate I, wherein the amount ratio of 3-aminohexanedioic acid to 2,4-octadiene-1-ol is 1mol:1mol; C2, adding intermediate I, benzyl chloroformate, sodium carbonate and tetrahydrofuran into a reaction kettle and stirring, raising the temperature of the reaction kettle to 50-60°C, keeping the temperature for 5-7h, and post-treating to obtain intermediate II, wherein the amount ratio of intermediate I to benzyl chloroformate is 1mol:2.1mol; C3. Add intermediate II and tetrahydrofuran into a nitrogen-protected reactor and stir. Raise the temperature of the reactor to 45-55°C. Add isocyanatepropyltriethoxysilane into the reactor and keep the reaction temperature for 3-5h. Post-treat to obtain a modifier, wherein the amount ratio of intermediate II to isocyanatepropyltriethoxysilane is 1 mol:1 mol.
2. The environmentally friendly polyurethane paint for interior decoration according to claim 1, characterized in that: The photoinitiator is 2-hydroxy-2-methyl-1-phenylpropanone, the pigment is an inorganic pigment with a particle size of 0.5-1.5 μm, and the additives are composed of a cosolvent, a defoamer, a wetting agent, a slip agent, and a leveling agent in a weight ratio of 5:1:2:1:
1. The cosolvent is dipropylene glycol methyl ether, the defoamer is defoamer GP330, the wetting agent is an amide-based gemini quaternary ammonium salt, the slip agent is polyvinyl alcohol, and the leveling agent is an acrylic leveling agent.
3. The environmentally friendly polyurethane paint for interior decoration according to claim 1, characterized in that: In step A1, the amount ratio of modified siloxane, polyethylene glycol 400, isophorone diisocyanate and (E)-oct-4-ene-1,8-diacid is 2 mol:5 mol:7 mol:2 mol, and the amount ratio of polyethylene glycol 400 and tetrahydrofuran is 1 g:6 mL.
4. The environmentally friendly polyurethane paint for interior decoration according to claim 1, characterized in that: The usage ratio of the 1,1,3,3,5,5,7,7,9,9-decamethylpentasiloxane, tetrahydrofuran and catalyst one is 1 g:4 mL:0.02 g, and the catalyst one is chloroplatinic acid.
5. The environmentally friendly polyurethane paint for interior decoration according to claim 1, characterized in that: In step B3, the usage ratio of nano-silica, modifier, 90wt% methanol solution and hydrochloric acid is 5g:3g:50mL:4mL, and the concentration of the hydrochloric acid is 11.5-12.5mol / L.
6. The environmentally friendly polyurethane paint for interior decoration according to claim 1, characterized in that: In step C1, the usage ratio of the 2,4-octadiene-1-ol, catalyst II and toluene is 3g:0.1g:20mL; in step C2, the usage ratio of benzyl chloroformate, sodium carbonate and tetrahydrofuran is 3g:2g:20mL; in step C3, the usage ratio of the intermediate II and tetrahydrofuran is 1g:6mL.
7. A method for producing an environmentally friendly polyurethane paint for interior decoration according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1, adding additives and purified water into the reactor and ultrasonically dispersing for 20-30 minutes; S2. Continue to add pigment, modified nano-silicon dioxide, modified polyurethane emulsion and photoinitiator into the reaction kettle, and perform ultrasonic dispersion for 30-50 minutes to obtain polyurethane paint.