A method for preparing a small-size in-situ observation sample for high-temperature laser scanning confocal microscope and its application
The handheld inlay specimens are prepared by metallographic specimens and combined with blind hole technology, the problems of handheld difficulty and grinding and flatness in the preparation of small-sized samples of high-temperature laser scanning confocal microscopes are solved, achieving efficient and convenient samples Prepare and observe the effects.
Patent Information
- Application Number
- CN202410161613.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-05
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-02-05
AI Technical Summary
The existing high-temperature laser scanning confocal microscope sample preparation methods include small sizes and difficult hand-held, easy to run, difficult to grind and throw, poor flatness, and requires specially designed fixtures and multiple inlays, which cause time-consuming and material-consuming and sample-consuming The problem of deformation.
Handheld inlay samples are prepared by using metallographic sample inlay mechanism. By forming blind holes on the inlay samples and combining them with small-sized samples, quickly bonding and grinding and polishing are used to achieve small-sized in-situ observation of the sample Preparation.
The sample preparation process is simplified, the sample flatness and parallelism are improved, the sample preparation difficulty and cost are reduced, the sample runs away and deformation are avoided, and the sample preparation is achieved efficient and convenient.
Smart Images

Figure CN118130191B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of in-situ observation sample preparation, and in particular to a method for preparing a small-size in-situ observation sample for a high-temperature laser scanning confocal microscope and an application thereof. Background Art
[0002] As a powerful tool for studying phase changes and microstructural changes of metal materials at high temperatures, high-temperature laser scanning confocal microscope can realize real-time, in-situ and high-definition observation and analysis of structural changes (melting, solidification, crystallization, solid-state phase change, etc.) of metal materials such as steel. It is mainly used in scientific research fields such as mineral processing, metal smelting, heat treatment of metal materials, and phase change mechanism research in steel. High-temperature laser scanning confocal microscope consists of two major parts: high-temperature image heating observation system and digital purple laser scanning confocal microscope. It can present large depth of field and high-quality images in the temperature range of room temperature to 1800℃ and save them continuously and automatically according to the programmed temperature control curve.
[0003] The current problem is that due to the unique structure of the heating furnace of the high-temperature laser scanning confocal microscope, the size of the in-situ observation sample is usually required to be a small cylinder with a diameter of less than 8mm and a height of less than 4mm. Before using the high-temperature laser scanning confocal microscope for in-situ observation experiments, it is necessary to prepare small-sized samples that meet the requirements. However, smaller-sized samples are not easy to hold and are easy to fly away, which greatly increases the difficulty of grinding and polishing. It will cause uneven force during grinding and polishing of small-sized samples, resulting in tilting, many surface scratches, and poor flatness. Finally, the inclined sample makes it difficult for the high-temperature laser scanning confocal microscope to focus in the plane and the imaging is flickering. At the same time, the scratches and gullies of varying depths will hinder the occurrence of solid-state phase change and the analysis of the kinetic process, seriously affecting the in-situ observation effect and image data processing results, losing the capture of details, and failing to give full play to the uniqueness of the in-situ observation function.
[0004] In order to solve the above problems, application number CN201911054641.4 discloses an observation aid for high-temperature laser confocal microscope samples and a method of use. The aid includes a seat, a screw and a disc sample. The seat is cylindrical, and a plurality of threaded holes are evenly arranged on the circumference of the seat. The screws are engaged in the threaded holes. The screws are made by grinding the top of traditional screws. The top surface of the screws is processed with a placement groove. The disc sample is fixed in the placement groove. The method of use includes sample installation, sample grinding and sample observation. However, this kind of aid limits the shape and size of the sample, and is only applicable to disc samples, and requires that the diameter of the disc sample is smaller than the diameter of the placement groove. In addition, when setting out and sampling, a hot air gun is required to blow rosin to fix it, and a glass sheet is used to manually adjust the flatness of the disc sample. The installation and disassembly are cumbersome, and it is not easy to ensure that the sample is completely flat. When grinding, the aid needs to be pressed down by hand, and the observation surface after sample preparation cannot be guaranteed to be flat. After grinding, the observation surface is prone to tilt.
[0005] Application number CN202110202128.6 discloses a method for preparing a steel sample for high-temperature confocal microscope observation, including: selecting a target sample, polishing the target sample after inlaying according to a conventional metallographic sample preparation method, and taking it out; placing the polished surface a of the target sample face down on the base of the first inlay tube, adding inlay material to obtain a first inlay block; placing the surface b opposite to the surface a of the first inlay block face down on the base of the second inlay tube, adding inlay material to obtain a second inlay block; polishing the surface b of the second inlay block until the cross section of the target sample is fully exposed, and automatically polishing; taking out the target sample from the treated second inlay block and cleaning it in an ultrasonic cleaner can be placed under a high-temperature confocal microscope for experiment. However, this method requires the sample to be inlaid three times, and after grinding and polishing the inlaid sample, it is also necessary to destroy the inlaid sample twice by hammering and cutting to remove the in-situ observation sample. On the one hand, this method greatly wastes the inlay raw materials, and on the other hand, when the polished sample undergoes two destruction samplings, it is easy to deform the cylindrical sample and contaminate the sample surface.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The first purpose of the present invention is to provide a method for preparing small-sized in-situ observation samples for a high-temperature laser scanning confocal microscope. The method is simple and convenient, and can be achieved by a conventional metallographic sample mounting machine. It solves the problems in the prior art that a specially designed fixture is required and the fixture cannot be worn, multiple mounting of samples is time-consuming and material-intensive and difficult to remove, and the upper and lower bottom surfaces of the samples cannot be absolutely parallel and are prone to scratches.
[0008] The second purpose of the present invention is to provide a method for preparing a small-size in-situ observation sample for a high-temperature laser scanning confocal microscope, and to apply the obtained small-size in-situ observation sample for a high-temperature laser scanning confocal microscope to observe and analyze phase changes and microstructural changes of metal materials.
[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0010] The present invention first provides a method for preparing a small-sized in-situ observation sample for a high-temperature laser scanning confocal microscope, comprising the following steps:
[0011] (a) obtaining one or more samples to be processed for observation;
[0012] (b) obtaining a handheld mounting sample by a metallographic sample mounting machine, and forming one or more blind holes on the handheld mounting sample to match the observation sample to be processed;
[0013] (c), placing each of the to-be-processed observation samples in each of the blind holes, and bonding the first plane of the to-be-processed observation sample to the bottom of the blind hole by an adhesive, and then performing a first grinding on the second plane;
[0014] (d) separating the sample to be processed from the blind hole, and bonding the second plane of the sample to be processed to the bottom of the blind hole by an adhesive, wherein the second plane is parallel to the first plane, and then performing a second grinding and polishing on the first plane. After the polishing is completed, separating the sample to be processed from the blind hole to obtain a processed high-temperature laser scanning confocal microscope small-size in-situ observation sample.
[0015] The present invention further provides a method for preparing a small-size in-situ observation sample for a high-temperature laser scanning confocal microscope, and uses the prepared small-size in-situ observation sample for a high-temperature laser scanning confocal microscope in observing and analyzing phase changes and microstructural changes of metal materials.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] (1) The method for preparing a small-sized in-situ observation sample for a high-temperature laser scanning confocal microscope provided by the present invention has an auxiliary device with a simple structure, which is convenient and easy to obtain. A solid inlaid sample is obtained on the basis of making full use of the tools used for preparing conventional metallographic samples in the field of metal materials (i.e., a metallographic sample inlaying machine). According to actual needs, the surface of the solid inlaid sample is flexibly processed to obtain blind holes of various sizes and shapes for combination and installation with the small-sized in-situ observation sample. The method does not require specially designed and customized small-sized sample fixtures, and the processed blind holes do not have high requirements for precision, which can truly achieve modification according to needs.
[0018] (2) The method for preparing a small-sized in-situ observation sample for a high-temperature laser scanning confocal microscope provided by the present invention is simple to install and disassemble, and can achieve efficient and convenient sample preparation. The handheld embedded sample with a blind hole and the small-sized sample to be processed can be quickly bonded together by an adhesive, and the structure is firm and stable, avoiding problems such as sample flying and tilting. At the same time, after grinding and polishing, the adhered glue is dissolved by an organic reagent, and the sample can be quickly disassembled, and the dissolution and separation process is completed under liquid sealing conditions, which solves the problem that the surface of some materials is easily oxidized after grinding and polishing. In addition, the handheld embedded sample used in the present invention can grind and polish multiple small-sized samples at one time, greatly improving the sample preparation efficiency and success rate.
[0019] (3) The method for preparing a small-sized in-situ observation sample for a high-temperature laser scanning confocal microscope provided by the present invention is easy to operate. The handheld embedded sample used in the present invention is easy to hold, which greatly reduces the difficulty of grinding and polishing of small-sized samples. It is not only suitable for experienced metallographic grinding and polishing personnel, but also for personnel who are new to the preparation of small-sized samples. By assembling a large shell with a small sample, the large can be made into a small one, which reduces the difficulty and completes the grinding and polishing, so as to obtain a flat, parallel, and nearly traceless in-situ observation surface.
[0020] (4) The method for preparing a small-sized in-situ observation sample for a high-temperature laser scanning confocal microscope provided by the present invention can improve the surface quality and reduce the cost of raw materials. Compared with customized permanent sample fixtures, they are usually not allowed to wear out due to their precision requirements. The in-situ observation handheld inlaid sample used by the present invention has low cost, can be used multiple times after one processing combination, and can be worn out during the grinding and polishing process of the small-sized sample surface, thus solving the problem that the grinding and polishing flatness of the small-sized sample surface is seriously dependent on the original machined surface, and has a correction function. Even if the upper and lower bottom surfaces of the original sample surface that has not been ground and polished are seriously non-parallel, the upper and lower bottom surfaces of the sample can be absolutely parallel and the small-sized sample can be firmly combined with the blind hole inlaid sample to obtain a sample with parallel upper and lower bottom surfaces. In addition, the present invention uses a handheld inlaid sample without the need to use multiple destructive means to take samples, thus saving raw material costs while ensuring the flatness of the sample surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 A schematic flow chart of a method for obtaining a handheld mounted sample by a metallographic sample mounting machine provided by the present invention;
[0023] Figure 2 A schematic diagram of the structure of a handheld inlaid sample with a blind hole provided by the present invention;
[0024] Figure 3 A schematic diagram of the installation of a handheld mounted sample and a sample to be processed for observation in Example 1 provided by the present invention;
[0025] Figure 4 The room temperature metallographic image of the small-sized in-situ observation sample obtained by the high-temperature laser scanning confocal microscope provided in Example 1 of the present invention;
[0026] Figure 5A real-time image of the phase change process of the welding heat affected zone of the sample observed in situ by a small-size high-temperature laser scanning confocal microscope obtained in Example 1 provided by the present invention;
[0027] Figure 6 A schematic diagram of the installation of a handheld mounted sample and a sample to be processed for observation in Example 2 provided by the present invention;
[0028] Figure 7 The room temperature metallographic image of the small-sized in-situ observation sample obtained by high-temperature laser scanning confocal microscope in Example 2 provided by the present invention;
[0029] Figure 8 A real-time image of the solidification process of the hand-held embedded sample and the sample to be processed in Example 2 provided by the present invention;
[0030] Fig. 9 A real-time image of the phase change process of the welding heat-affected zone of the defective sample prepared in Comparative Example 1 provided by the present invention;
[0031] Fig.10 The real-time image of the phase change process of the welding heat affected zone of the sample obtained by the high-temperature laser scanning confocal microscope of the comparative example 2 provided by the present invention is observed in situ with a small size. DETAILED DESCRIPTION
[0032] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0033] If there is no special explanation, in the present invention, "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "the first", "the second", "the third", "the fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0034] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0035] If there is no special explanation, in the present invention, "one or more" or "at least one" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.
[0036] In a first aspect, the present invention provides a method for preparing a small-sized in-situ observation sample for a high-temperature laser scanning confocal microscope, comprising the following steps:
[0037] (a) Obtain one or more (i.e., at least one) observation samples to be processed. For example, obtain one, two, three, four, five, six, seven, eight, nine, or ten observation samples to be processed.
[0038] In some specific implementations, one or more samples to be processed and observed are obtained by mechanical processing according to preset sizes.
[0039] (b) obtaining a hand-held mounted sample by a metallographic sample mounting machine, and forming one or more (i.e., at least one, such as one, two, three, four, five, six, seven, eight, nine or ten, which can be set as needed) blind holes matching the sample to be processed on a surface of the hand-held mounted sample, such as Figure 2 As shown. Among them, the blind hole refers to a hole that has not been penetrated, which can also be understood as a groove. Matching means that the size of the sample to be processed and observed matches the size of the blind hole.
[0040] (c) placing each of the samples to be processed in each of the blind holes of the metallographic sample mounting machine, and bonding the first plane of the sample to be processed to the bottom of the blind hole (i.e., the first plane is bonded to the bottom of the groove of the metallographic sample mounting machine) by an adhesive to form a bonded hand-held polishing sample, and then performing a first grinding on the exposed second plane.
[0041] The purpose of the first grinding is to make the second plane flat without depressions or protrusions, so as to avoid the unevenness of the second plane causing the first plane to tilt during observation and have shadows, thereby affecting the in-situ observation results.
[0042] (d) separating the sample to be processed from the blind hole, then turning the sample to be processed, and bonding the second plane of the sample to be processed to the bottom of the blind hole by an adhesive, wherein the second plane and the first plane are opposite and parallel to each other, such as the top surface and the bottom surface, and then performing a second grinding and polishing on the exposed first plane in sequence as an observation surface, and after the polishing is completed, separating the sample to be processed from the blind hole to obtain a processed (ground and polished) small-size in-situ observation sample for high-temperature laser scanning confocal microscope that can be used for in-situ observation.
[0043] The method for preparing a small-sized in-situ observation sample for a high-temperature laser scanning confocal microscope provided by the present invention directly uses a hot-mounted sample commonly used by sample preparation personnel for hand-held grinding and polishing, is simple to operate, does not require a customized fixture, and is not restricted by the fixture. Small-sized in-situ observation samples of various specifications can be processed and assembled at any time to obtain hand-held mounted samples, which helps to improve the surface quality of the sample and can obtain a flat, parallel, and nearly traceless in-situ observation surface. In addition, multiple samples can be prepared at one time, which greatly saves sample preparation time and sample preparation costs, improves the efficiency and success rate of small-sized sample preparation, and meets the in-situ observation effect.
[0044] The present invention proposes a new method for preparing samples by using a handheld hot-mounted sample combination to install a small-sized in-situ observation sample, that is, by drilling holes on the upper surface of the hot-mounted sample and adhering and fixing the small-sized sample in the hole, convenient and efficient grinding and polishing are achieved.
[0045] Specifically, in the present invention, in order to fully ensure the absolute parallelism of the upper and lower surfaces of the small-sized in-situ observation sample, the grinding and polishing process is carried out in two stages. First, for the assembled handheld mounted sample, the second plane of the in-situ observation sample is subjected to the first grinding in the first stage to obtain a flat plane. Then, based on the flat second plane, the first plane of the in-situ observation sample is subjected to the second grinding and polishing in the second stage to obtain a flat, parallel, and nearly traceless in-situ observation surface.
[0046] In addition, the present invention has no fixed restrictions on the size of the sample to be processed and the size of the handheld mounted sample. It can be flexibly modified according to the model of the experimental equipment and the personal habits of the polishing personnel, so that the preparation of small-size samples can be personalized, avoiding the high cost of customized fixtures while preparing multiple samples at one time, saving costs and improving efficiency and success rate.
[0047] In some specific implementations, in step (a), the shape of the to-be-processed observation sample includes at least one of a cylinder and a cube, which can be specifically set as needed.
[0048] In some specific implementations, in step (a), the observation sample to be processed is obtained by mechanical processing.
[0049] In some specific embodiments, the machining method includes at least one of electric spark wire cutting, diamond cutting, laser cutting and water cutting.
[0050] In some specific implementations, the observation sample to be processed is roughly ground and / or cleaned after the mechanical processing.
[0051] Preferably, one or more observation samples to be processed are obtained by mechanical processing, and then each observation sample to be processed is coarsely ground and cleaned in turn.
[0052] Preferably, the surface and circumference of the observation sample to be processed are roughly ground with sandpaper to remove line marks, oil stains and rust left by machining until the metallic luster is completely exposed. The roughly ground observation sample to be processed is then rinsed with water and dried with filter paper for later use.
[0053] As an example, the rough grinding may use 800# silicon carbide metallographic sandpaper, but is not limited thereto.
[0054] Among them, the size of the sample to be processed for observation can be set as needed. On the premise that the high-temperature laser scanning confocal microscope cavity can accommodate the sample, different specifications, sizes and shapes can be processed according to the purpose of in-situ observation and the size of the experimental crucible.
[0055] As an example, the observation sample to be processed is in the shape of a cylinder with a diameter of 5 mm and a thickness of 4 mm.
[0056] In some specific embodiments, in step (b), the method for obtaining a handheld mounted sample by a metallographic sample mounting machine comprises: placing a mounting material between an upper module and a lower module of the metallographic sample mounting machine, heating and extruding, and cooling to obtain the handheld mounted sample.
[0057] The size of the handheld inlaid specimen can be set as needed, including but not limited to a cylinder of Φ30×12 mm, and inlaid specimens of different diameters and thicknesses can also be used.
[0058] In some specific embodiments, the inlay material includes at least one of bakelite powder and a resin containing a filler.
[0059] In some specific embodiments, the resin containing fillers includes at least one of epoxy resin containing mineral fillers, phenolic resin containing carbon fillers, and phenolic resin containing wood powder fillers. The mineral fillers include at least one of quartz powder, glass fiber, metal powder, and carbon fiber; and the carbon fillers include at least one of light calcium carbonate, heavy calcium carbonate, fly ash, and boron carbide.
[0060] In some specific embodiments, the heating temperature is 130-180°C, including but not limited to any point value of 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C or a range value between any two of them.
[0061] In some specific embodiments, the extrusion pressure is 25-35 MPa, including but not limited to any point value of 25 MPa, 28 MPa, 30 MPa, 32 MPa, 35 MPa or a range value between any two of them.
[0062] In some specific embodiments, the heating and / or extrusion time is 5 to 15 min, including but not limited to any one of 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, and 15 min, or a range between any two of them.
[0063] As an example, in step (b), the handheld mounting sample is a solid handheld mounting sample, and the method for obtaining the handheld mounting sample by the metallographic sample mounting machine is as follows: Figure 1As shown, the steps include: turning the hand wheel of the metallographic sample embedding machine, adjusting the lower module for embedding material to move in the mold sleeve, making the lower module parallel to the platform, and then turning the hand wheel counterclockwise for 10 to 15 turns to sink the lower module, 30 to 35 mm away from the platform, filling the mold sleeve (above the lower module) with embedding material, such as bakelite powder, and making it parallel to the platform, then pressing the upper module on the embedding material, pressing the upper module, and turning the hand wheel counterclockwise at the same time, so that the upper module sinks until its upper surface is slightly lower than the platform, closing the embedding machine cover and tightening it, then setting the embedding machine temperature, and turning the hand wheel clockwise until the pressure light comes on and then continue to turn the hand wheel clockwise for 1 to 2 turns, such as 1.5 turns, to ensure that the filled embedding material is compacted, and starting to count down for 5 minutes after reaching the set temperature and appropriate pressure, during which the pressure light is kept on, and if the pressure light goes out during this process, the hand wheel should be turned clockwise again, such as 5 turns, to make the pressure light come on again, and finally the embedding material is thermoset. After that, demolding and sampling began. First, turn the handwheel counterclockwise to unload the pressure and turn off the pressure light. Then continue to turn the handwheel counterclockwise to separate the lower module from the inlaid sample to make room for demolding. Then turn the octagonal knob on the cover of the inlay machine clockwise to push the upper module downward to demold the compacted handheld inlaid sample. This step can ensure that the upper module does not collapse or bounce during sampling. Then turn the octagonal knob counterclockwise to open the cover, and turn the handwheel clockwise to push out the upper module until the lower surface of the upper module is parallel to the platform. Remove the upper module and place it next to the inlay machine (the upper module is hot at this time and cannot be touched directly by hand). Continue to turn the handwheel clockwise to raise the lower module to completely expose the prepared handheld inlaid sample, and then obtain the handheld inlaid sample.
[0064] In some specific implementations, in step (c), the adhesive includes at least one of 502 glue, 402 glue, 401 glue, rosin, epoxy resin glue and acrylic glue (i.e., acrylic ester adhesive).
[0065] Preferably, in step (c), the method of bonding the first plane of the sample to be processed to the bottom of the blind hole by means of an adhesive specifically comprises: dripping 2 to 4 drops (about 0.1 to 0.2 ml) of adhesive into each blind hole, then quickly placing the sample to be processed into the blind hole, and making one end of the sample to be processed fit with the bottom of the blind hole, and obtaining the bonded hand-held polishing sample after drying. More preferably, before dripping the adhesive, first clean the surface of the metallographic sample mounting machine and the blind hole to avoid dust and mounting material residue.
[0066] Preferably, in step (c), the first grinding method comprises: grinding the second plane using 400#, 800#, and 1000# silicon carbide metallographic sandpaper in sequence, wherein each mesh size of sandpaper is ground for 3 to 5 minutes, and then rinsed with water and dried.
[0067] Preferably, in step (d), the method of bonding the second plane of the sample to be processed to the bottom of the blind hole by means of an adhesive specifically comprises: dripping 2 to 4 drops (about 0.1 to 0.2 ml) of adhesive into each blind hole, then quickly placing the sample to be processed into the blind hole, and making the second plane of the sample to be processed fit with the bottom of the blind hole, and obtaining the bonded hand-held polishing sample after drying. More preferably, before dripping the adhesive, first clean the surface of the metallographic sample mounting machine and the blind hole to avoid dust and mounting material residue.
[0068] In some specific embodiments, in step (d), the second grinding and polishing is performed until no scratches are visible to the naked eye.
[0069] In some specific embodiments, in step (d), the second grinding method includes: first performing coarse grinding and then performing fine grinding until the scratches formed by the previous grinding disappear.
[0070] In some specific implementations, in step (d), the polishing method includes: polishing to a mirror surface using a polishing paste with a particle size of 0.25 μm to 0.05 μm.
[0071] In some specific embodiments, in step (d), the second grinding and polishing method specifically includes: using 400# and 800# silicon carbide metallographic sandpaper to coarsely grind the first plane in sequence, and then using 1000#, 1500#, and 2000# water sandpaper for fine grinding, the grinding direction between two adjacent sandpapers is 90°, and grinding until the scratches formed in the previous pass completely disappear, and then polishing to a mirror surface using water-soluble diamond polishing paste with a particle size of 0.25μm and 0.05μm on a gold velvet polishing cloth, and wiping and rinsing the sample surface with water-soaked absorbent cotton under water, and then spraying alcohol and drying.
[0072] In some specific embodiments, in step (c) and step (d), the separation method includes: immersing the handheld polishing sample after the observation sample to be processed and the blind hole are bonded in an organic solvent to dissolve the adhesive.
[0073] The bonding and separation of the handheld embedded sample and the small-sized observation sample to be processed in the present invention are achieved by adhesive and soaking in organic solvent, which is easy to operate and is completed under liquid sealing conditions, solving the problem of easy oxidation of the surface of metal materials such as aluminum and magnesium after grinding and polishing.
[0074] In some specific embodiments, the organic solvent includes at least one of acetone, thinner, dichloromethane and alcohol.
[0075] Among them, Tiana water is also known as banana water and pear oil, and its chemical formula is CH3CH(CH3)CH2CH2OOCCH3.
[0076] In some specific embodiments, the soaking time is 1 to 5 hours, including but not limited to any one of 1 hour, 2 hours, 3 hours, 4 hours, and 5 hours, or a range between any two of them.
[0077] In the second aspect, the present invention provides the application of the small-size in-situ observation sample of high-temperature laser scanning confocal microscope prepared by the above-mentioned preparation method of the small-size in-situ observation sample of high-temperature laser scanning confocal microscope in observing and analyzing the phase change and microstructure change of metal materials.
[0078] In some specific implementations, the metal material includes but is not limited to iron alloys, copper alloys, titanium alloys, aluminum alloys, and the like.
[0079] In some specific implementations, a first plane in a small-size in-situ observation sample of a high-temperature laser scanning confocal microscope is in-situ observed by a high-temperature laser scanning confocal microscope.
[0080] In some specific embodiments, the method for in-situ observation of the first plane in the small-size in-situ observation sample of the high-temperature laser scanning confocal microscope by using a high-temperature laser scanning confocal microscope includes: placing the prepared small-size in-situ observation sample of the high-temperature laser scanning confocal microscope into an alumina ceramic crucible, and then placing it on a Pt sample holder, sealing the heating furnace body and purging it with high-purity argon (99.99%) for 3 to 5 times to exhaust the air in the heating chamber, and at the same time, filling argon gas throughout the experiment to prevent oxidation of the small-size in-situ observation sample of the high-temperature laser scanning confocal microscope, then fixing the magnification, selecting an observation field of view with a flat surface and no scratches on the small-size in-situ observation sample of the high-temperature laser scanning confocal microscope, and finally setting a specific welding thermal cycle curve, which is specifically used to reproduce the welding thermal cycle process of the coarse-grained heat-affected zone under manual arc welding conditions with a heat input of 15 to 20 kJ / cm, and capturing real-time images at a rate of 10 to 20 frame / s through the charge coupled device (CCD) camera of the high-temperature laser scanning confocal microscope.
[0081] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0082] Example 1
[0083] This embodiment provides a method for preparing a small-sized sample for in-situ observation of solid-state phase transformation in a welding heat-affected zone of 1.25Cr-0.5Mo heat-resistant steel using a high-temperature laser scanning confocal microscope, comprising the following steps:
[0084] (1) Machining in-situ observation samples according to preset dimensions: First, five cylindrical samples with a diameter of 5 mm and a thickness of 4 mm (abbreviated as Φ5×4 mm) were taken from the delivered 1.25Cr-0.5Mo heat-resistant steel base material by wire-cut electrospark machining. Then, the upper and lower surfaces and the circumference of the cylindrical samples were roughly ground using 800# silicon carbide metallographic sandpaper to remove the line marks, oil stains, and rust left by machining until the metallic luster was completely exposed. Finally, the cylindrical samples were rinsed with water and dried with filter paper to obtain five observation samples to be processed for later use.
[0085] (2) Preparation and processing of hand-held mounted specimens: Use XQ-2B metallographic specimen mounting machine to prepare hand-held mounted specimens, such as Figure 2 As shown, first turn the hand wheel of the inlay machine to adjust the lower module of the pressed sample to move in the mold sleeve so that the lower module is parallel to the platform, then turn the hand wheel counterclockwise 13 times to sink the lower module, 31mm away from the platform, fill the mold sleeve with filler bakelite powder (phenolic molding compound, model PF2A2-141 black) and make it parallel to the platform, then press the steel upper module with a size of Φ30×20mm (diameter 30mm, height 20mm) on the filler bakelite powder, hold the upper module with the fingers of the left hand and apply downward pressure, and at the same time, turn the hand wheel counterclockwise with the right hand to sink the upper module until its upper surface is slightly lower than the platform, close the cover of the inlay machine and tighten it, then set the temperature of the inlay machine to 140℃, and turn the hand wheel clockwise until the pressure light comes on, and then continue to turn the hand wheel clockwise 1.5 times to ensure that the filled bakelite powder is compacted. When the set temperature of 140℃ and the appropriate After the pressure is applied, a countdown of 5 minutes begins (the pressure light remains on during this period). If the pressure light goes out during this process, the handwheel should be turned clockwise again to make it light up again, and finally the bakelite powder is thermoset. Then, demolding and sampling begins. First, turn the handwheel counterclockwise to unload the pressure and turn off the pressure light. Then, continue to turn the handwheel counterclockwise for 5 turns to separate the lower module from the inlaid sample to make room for demolding. Then, turn the octagonal knob on the cover of the inlay machine clockwise to push the upper module downward to demold the sample. Then, turn the octagonal knob counterclockwise to open the cover. Turn the handwheel clockwise to push out the upper module until the lower surface of the upper module is parallel to the platform. Wear heat-insulating gloves to remove the upper module and place it next to the inlay machine. Continue to turn the handwheel clockwise to raise the lower module to completely expose the inlaid sample. Then, take out a cylindrical handheld inlaid sample with a diameter of 30 mm and a thickness of 12 mm (abbreviated as Φ30×12 mm).
[0086] Then, a concentric circle with a diameter of 14 mm was made on the upper surface of the Φ30×12 mm cylindrical hand-held embedded specimen. Five points were taken at equal distances on the circumference of the circle, and five cylindrical blind holes with a diameter of 5 mm and a depth of 4 mm were drilled with these five points as the center, such as Figure 2 shown.
[0087] (3) Assembly of the observation specimen to be processed and the hand-held inlaid specimen: First, clean the surface and cylindrical blind hole of the hand-held inlaid specimen obtained in step (2) to avoid dust and inlaid powder residue. Then, drip 2 drops of 502 glue into each of the 5 cylindrical blind holes of the hand-held inlaid specimen. Then, use tweezers to quickly place the 5 Φ5×4 mm observation specimens to be processed obtained in step (1) into each of the cylindrical blind holes, with the A side facing up. Figure 3 As shown, it is then placed in a ventilated place until the 502 glue in the blind hole sticks the observation sample to be processed and the handheld embedded sample tightly to obtain a handheld polishing sample.
[0088] (4) Grinding the surface A of the hand-held polishing sample (i.e., the first grinding): Place the target grinding surface A of the observation sample to be processed in the hand-held polishing sample obtained in step (3) with the surface facing downward on the loading plate of the UNIPOL-1200M automatic pressure grinding and polishing machine, and use pneumatic pressure to fix the sample so that the loading plate is evenly stressed. Set the speed of the loading plate (upper plate) to 30 rpm and the speed of the polishing plate (lower plate) to 300 rpm. Then open the water pipe and use 400#, 800#, and 1000# silicon carbide metallographic sandpaper to grind the surface A in turn. Each mesh size of sandpaper is ground for 4 minutes. Then take it out of the loading plate, rinse it with water, spray it with alcohol, and blow it dry with a hair dryer.
[0089] (5) Grinding and polishing the B surface of the in-situ observation sample (i.e., the second grinding and polishing): Place the observation sample to be processed that has been ground in step (4) into a beaker containing acetone and soak for 1 hour to completely dissolve the 502 glue, then take out the observation sample to be processed, spray the observation sample to be processed and the mounted sample with alcohol to clean and blow dry, then drip 2 drops of 502 glue into each of the 5 cylindrical blind holes of the handheld mounted sample, and use tweezers to place the observation sample to be processed into the mounted sample hole, making sure that the ground A surface faces downward and the unground B surface faces upward, then place it in a ventilated place to dry, and wait until the 502 glue in the hole is tightly bonded to the observation sample to be processed, and then obtain a handheld grinding and polishing sample again.
[0090] Then, the target grinding surface B of the hand-held polishing specimen is facing down, and 400# and 800# silicon carbide metallographic sandpapers are used to coarsely grind the B surface in turn, and then 1000#, 1500#, and 2000# water sandpapers are used for fine grinding. The grinding direction between two adjacent sandpapers is 90°, and the grinding is carried out until the scratches formed in the previous pass completely disappear. Then, water-soluble diamond polishing pastes with particle sizes of 0.25μm and 0.05μm are used on gold velvet polishing cloth to polish to a mirror surface, and the sample surface is wiped and rinsed with water-soaked absorbent cotton under water, and then sprayed with alcohol, and quickly dried with a hair dryer at a 45° angle along the sample surface.
[0091] Then, the polished hand-held mounted sample was placed in a beaker of acetone again and soaked for 1 hour to completely dissolve the 502 glue. The sample to be processed was taken out with tweezers, sprayed with alcohol to clean it and blown dry to obtain the processed high-temperature laser scanning confocal microscope small-size in situ observation sample, which was wrapped with absorbent cotton and stored in a transparent bag.
[0092] (6) In-situ observation using a high-temperature laser scanning confocal microscope: First, the Φ5×4 mm high-temperature laser scanning confocal microscope small-size in-situ observation sample prepared in step (5) is placed in an alumina ceramic crucible with a diameter of 6.5 mm and a thickness of 4 mm, and then placed on a Pt sample holder. After sealing the heating furnace body, the air in the heating chamber is purged three times with high-purity argon (99.99%). At the same time, argon is filled throughout the experiment to prevent sample oxidation. Then, the magnification is fixed and the observation field of view is selected when the sample surface is flat and scratch-free, such as Figure 4 As shown in the figure, a specific welding thermal cycle curve is set up to reproduce the welding thermal cycle process of the coarse-grained heat-affected zone under the condition of manual arc welding with a heat input of 18 kJ / cm. The real-time image is captured at a rate of 15 frame / s by the charge coupled device (CCD) camera of the high-temperature laser scanning confocal microscope, and the in-situ observation results of the whole experiment are recorded in the video file, among which the continuous morphological evolution of some typical solid-state phase transformations is shown in the figure. Figure 5 shown.
[0093] Example 2
[0094] This embodiment provides a method for preparing a small-sized sample for in-situ observation of the solidification behavior of a copper-titanium alloy using a high-temperature laser scanning confocal microscope, comprising the following steps:
[0095] (1) Machining in-situ observation samples according to preset dimensions: First, five cylindrical samples with a diameter of 6.5 mm and a thickness of 3 mm (abbreviated as Φ6.5×3 mm) were taken from the molten copper-titanium alloy ingot by electric spark wire cutting machining, and then the upper and lower surfaces and circumference of the cylindrical samples were roughly ground using 800# silicon carbide metallographic sandpaper to remove the line marks, oil stains, and rust left by machining until the metallic luster was completely exposed. Finally, the cylindrical samples were rinsed with water and the moisture was absorbed with filter paper to obtain five observation samples to be processed for use.
[0096] (2) Preparation and processing of hand-held inlaid specimens: Use the XQ-2B metallographic specimen inlaying machine to prepare hand-held inlaid specimens. First, turn the hand wheel of the inlaying machine to adjust the lower die block of the pressed specimen to move in the die sleeve so that the lower die block is parallel to the platform. Then, turn the hand wheel counterclockwise 13 times to sink the lower die block to a distance of 31 mm from the platform. Fill the die sleeve with phenolic resin (PF2A4-161J red) containing wood powder filler and make it parallel to the platform. Then, press the steel upper die block with a size of Φ30×20 mm (30 mm in diameter and 20 mm in height) on the phenolic resin containing wood powder filler. Use the fingers of the left hand to support the upper die block and apply downward pressure. At the same time, turn the hand wheel counterclockwise with the right hand to sink the upper die block until its upper surface is slightly lower than the platform. Close the cover of the inlaying machine and tighten it. Then, set the temperature of the inlaying machine to 140°C, and turn the hand wheel clockwise until the pressure light comes on. Then, continue to turn the hand wheel clockwise for 1.5 turns to ensure that the phenolic resin containing wood powder filler is filled. The phenolic resin is pressed tightly, and a countdown of 5 minutes is started after reaching the set temperature of 140°C and the appropriate pressure (the pressure light is kept on during this period). If the pressure light goes out during this process, the hand wheel should be turned clockwise again to make the pressure light turn on again, and finally the phenolic resin containing wood powder filler is thermoset. After that, demoulding and sampling are started. First, the hand wheel is turned counterclockwise to unload the pressure to turn off the pressure light, and then the hand wheel is turned counterclockwise for 5 turns to separate the lower module from the inlaid sample to make room for demoulding. Then, the octagonal knob on the cover of the inlay machine is turned clockwise to push the upper module downward to demould the sample, and then the octagonal knob is turned counterclockwise to open the cover, and the hand wheel is turned clockwise to push out the upper module until the lower surface of the upper module is parallel to the platform. Wear heat-insulating gloves to remove the upper module and place it next to the inlay machine. Continue to turn the hand wheel clockwise to raise the lower module to completely expose the inlaid sample, and then take out a cylindrical handheld inlaid sample with a diameter of 30 mm and a thickness of 12 mm (abbreviated as Φ30×12 mm).
[0097] Then, a concentric circle with a diameter of 14 mm was made on the upper surface of the Φ30×12 mm cylindrical hand-held mounting specimen. Five points were taken at equal distances on the circumference of the circle, and five cylindrical blind holes with a diameter of 6.5 mm and a depth of 3 mm were drilled with these five points as the center, such as Figure 6 shown.
[0098] (3) Assembly of the observation specimen to be processed and the hand-held inlaid specimen: First, clean the surface and cylindrical blind hole of the hand-held inlaid specimen obtained in step (2) to avoid dust and inlaid powder residue. Then, drip 2 drops of epoxy resin glue (Deli 53574AB glue) into each of the 5 cylindrical blind holes of the hand-held inlaid specimen. Then, use tweezers to quickly place the 5 Φ6.5×3 mm observation specimens to be processed obtained in step (1) into each of the cylindrical blind holes, with the A side facing upward. Figure 6 As shown, it is then placed in a ventilated place until the epoxy resin glue in the blind hole bonds the observation sample to be processed and the handheld embedded sample to obtain a handheld polishing sample.
[0099] (4) Grinding the surface A of the hand-held polishing sample (i.e., the first grinding): Place the target grinding surface A of the observation sample to be processed in the hand-held polishing sample obtained in step (3) with the surface facing downward on the loading plate of the UNIPOL-1200M automatic pressure grinding and polishing machine, and use pneumatic pressure to fix the sample so that the loading plate is evenly stressed. Set the speed of the loading plate (upper plate) to 30 rpm and the speed of the polishing plate (lower plate) to 300 rpm. Then open the water pipe and use 400#, 800#, and 1000# silicon carbide metallographic sandpaper to grind the surface A in turn. Grind for 5 min for each mesh size of sandpaper. Then take it out of the loading plate, rinse it with water, spray it with alcohol, and blow it dry with a hair dryer.
[0100] (5) Grinding and polishing the B surface of the in-situ observation sample (i.e., the second grinding and polishing): Place the observation sample to be processed that has been ground in step (4) into a beaker containing alcohol and soak it for 1.5 hours to completely dissolve the epoxy resin glue, then take out the observation sample to be processed, spray the observation sample to be processed and the mounted sample with alcohol to clean and blow dry, then drip 2 drops of epoxy resin glue into each of the 5 cylindrical blind holes of the handheld mounted sample, and use tweezers to place the observation sample to be processed into the mounted sample hole, making sure that the ground A surface faces downward and the unground B surface faces upward, then place it in a ventilated place to dry, and wait until the epoxy resin glue in the hole is tightly bonded to the observation sample to be processed, and then obtain a handheld grinding and polishing sample again.
[0101] Then, the target grinding surface B of the hand-held polishing specimen is facing down, and 400# and 800# silicon carbide metallographic sandpapers are used to coarsely grind the B surface in turn, and then 1000#, 1500#, and 2000# water sandpapers are used for fine grinding. The grinding direction between two adjacent sandpapers is 90°, and the grinding is carried out until the scratches formed in the previous pass completely disappear. After that, water-soluble diamond polishing pastes with particle sizes of 0.25μm and 0.05μm are used on gold velvet polishing cloth to polish to a mirror surface, and the sample surface is wiped and rinsed with water-soaked absorbent cotton under water, and then sprayed with alcohol, and quickly dried with a hair dryer along the sample surface at a 45° angle.
[0102] After that, the polished hand-held mounted sample was placed in a beaker of alcohol and soaked for 1.5 hours to completely dissolve the epoxy resin glue. Then, the sample to be processed was taken out with tweezers, sprayed with alcohol to clean it and blown dry. The processed high-temperature laser scanning confocal microscope small-size in situ observation sample was obtained, which was wrapped with absorbent cotton and stored in a transparent bag.
[0103] (6) In-situ observation using a high-temperature laser scanning confocal microscope: First, the Φ6.5×3 mm high-temperature laser scanning confocal microscope small-size in-situ observation sample prepared in step (5) is placed in an alumina ceramic crucible with a diameter of 9 mm and a thickness of 4 mm, and then placed on a Pt sample holder. After sealing the heating furnace body, the air in the heating chamber is purged three times with high-purity argon (99.99%). At the same time, argon is filled throughout the experiment to prevent sample oxidation. Then, the magnification is fixed and the observation field of view is selected when the sample surface is flat and scratch-free, such as Figure 7 As shown in the figure, specific heating and cooling rates are set to reproduce the solidification process of copper-titanium alloy during melting. The charge coupled device (CCD) camera of the high-temperature laser scanning confocal microscope captures real-time images at a rate of 15 frames / s, and the in-situ observation results of the entire experiment are recorded in a video file. The continuous morphological evolution of some typical solidification behaviors is shown in the figure. Figure 8 shown.
[0104] Example 3
[0105] The preparation method of a small-sized specimen for in-situ observation of solid-state phase transformation in the heat-affected zone of 1.25Cr-0.5Mo heat-resistant steel welding by high-temperature laser scanning confocal microscopy provided in this embodiment is basically the same as that in Example 1, with the only difference being that the bakelite powder is replaced by a phenolic resin containing carbon filler (Meijun HM3).
[0106] Example 4
[0107] The preparation method of a small-sized sample for in-situ observation of solid-state phase transformation in the heat-affected zone of 1.25Cr-0.5Mo heat-resistant steel welding by high-temperature laser scanning confocal microscopy provided in this embodiment is basically the same as that in Example 1, except that 502 glue is replaced by rosin, and the amount of rosin used is 0.1 g.
[0108] Example 5
[0109] The method for preparing a small-sized specimen for in-situ observation of solid-state phase transformation in the heat-affected zone of 1.25Cr-0.5Mo heat-resistant steel welding by high-temperature laser scanning confocal microscopy provided in this embodiment is basically the same as that in Example 1, with the only difference being that, in step (1), eight cubic samples with an edge length of 4 mm are taken from the as-delivered 1.25Cr-0.5Mo heat-resistant steel base material by electric spark wire cutting machining; and in step (2), eight cubic blind holes with an edge length of 4 mm are drilled on the upper surface of the cylindrical hand-held embedded specimen.
[0110] Comparative Example 1
[0111] The method for preparing a small-size sample for in-situ observation of solid-state phase transformation in the heat-affected zone of 1.25Cr-0.5Mo heat-resistant steel welding by high-temperature laser scanning confocal microscope provided in this comparative example is prepared by conventional technology, which is completely different from Example 1, and specifically includes the following steps:
[0112] (1) Take a cylindrical sample with a diameter of 5 mm and a thickness of 4 mm (abbreviated as Φ5×4 mm) from the delivered 1.25Cr-0.5Mo heat-resistant steel base material by wire-cut electrospark machining, and use 800# silicon carbide metallographic sandpaper to roughly grind the upper and lower surfaces and circumference of the cylindrical sample to remove the line marks, oil stains, and rust left by machining until the metallic luster is completely exposed. Finally, rinse the cylindrical sample with water to obtain the cylindrical sample to be observed;
[0113] (2) placing the cylindrical sample to be observed obtained in step (1) into a metallographic sample mounting machine for direct hot mounting, and then grinding and polishing the mounted sample according to a conventional metallographic sample preparation method; after the grinding and polishing are completed, the mounted sample is broken with a hammer to remove the cylindrical sample to be observed, and then it is subsequently cleaned, and then a high-temperature laser scanning confocal in-situ observation experiment is performed.
[0114] The in-situ observation real-time image results obtained in this comparative example are as follows Fig. 9 As shown, it can be clearly seen that there are many problems on the surface of the sample, such as a large number of scratches, poor flatness, and many contaminants, impurities and black spots. These defects not only make it difficult for the high-temperature laser scanning confocal microscope to focus in the plane and the imaging is flickering, resulting in poor continuous in-situ observation of fixed areas in the plane and reduced selectivity, but also the scratches and grooves of varying depths will hinder the occurrence of solid-state phase change and the analysis of the kinetic process, seriously affecting the in-situ observation effect of the solid-state phase change and the image data processing results, losing the capture of details, and ultimately failing to give full play to the uniqueness of the in-situ observation function.
[0115] Comparative Example 2
[0116] The preparation method of a small-sized sample for in-situ observation of solid-state phase transformation in the heat-affected zone of 1.25Cr-0.5Mo heat-resistant steel welding by high-temperature laser scanning confocal microscope provided in this embodiment is basically the same as that in embodiment 1, except that surface A is not ground in step (4). This causes the bottom of the sample to be uneven, resulting in difficulty in focusing the observation plane and inconsistent depth of field, which ultimately leads to problems such as inconsistent brightness and darkness in the same plane and decreased clarity in the in-situ observation real-time image. Fig.10 As shown, it seriously affects the capture of experimental details and the analysis of quantitative results.
[0117] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A method for preparing a small-sized in-situ observation sample for a high-temperature laser scanning confocal microscope, characterized in that: The steps include: (a) obtaining one or more observation samples to be processed; (b) obtaining a handheld mounting sample by a metallographic sample mounting machine, and forming one or more blind holes on the handheld mounting sample to match the observation sample to be processed; (c) placing each of the observation samples to be processed in each of the blind holes, and bonding the first plane of the observation sample to be processed to the bottom of the blind hole by an adhesive, and then performing a first grinding on the exposed second plane; (d) separating the sample to be processed from the blind hole, and bonding the second plane of the sample to be processed to the bottom of the blind hole by an adhesive, wherein the second plane is parallel to the first plane, and then performing a second grinding and polishing on the first plane. After the polishing is completed, separating the sample to be processed from the blind hole to obtain a processed small-size in-situ observation sample for high-temperature laser scanning confocal microscopy; Wherein, in step (b), the method for obtaining a handheld mounted sample by a metallographic sample mounting machine comprises: placing a mounting material between an upper module and a lower module of the metallographic sample mounting machine, heating and extruding and then cooling to obtain the handheld mounted sample; the mounting material comprises at least one of bakelite powder and a resin containing filler; the heating temperature is 130-180° C.; the extrusion pressure is 25-35 MPa; the heating and / or extrusion time is 5-15 min; In step (c), the adhesive includes at least one of 502 glue, 402 glue, 401 glue, rosin, epoxy resin glue and acrylic glue; In step (d), the separation method comprises: immersing the handheld polishing sample after the observation sample to be processed and the blind hole are bonded in an organic solvent to dissolve the adhesive.
2. The method for preparing a small-sized in-situ observation sample for a high-temperature laser scanning confocal microscope according to claim 1, characterized in that: In step (a), the shape of the to-be-processed observation sample includes at least one of a cylinder and a cube.
3. The method for preparing a small-sized in-situ observation sample for a high-temperature laser scanning confocal microscope according to claim 1, characterized in that: In step (a), the observation sample to be processed is obtained by mechanical processing.
4. The method for preparing a small-sized in-situ observation sample for a high-temperature laser scanning confocal microscope according to claim 3, characterized in that: The machining method includes at least one of electric spark wire cutting, diamond cutting, laser cutting and water cutting; And / or, after the mechanical processing, the observation sample to be processed is roughly ground and / or cleaned.
5. The method for preparing a small-sized in-situ observation sample for a high-temperature laser scanning confocal microscope according to claim 1, characterized in that: In step (d), the second grinding and polishing is performed until there are no scratches visible to the naked eye.
6. The method for preparing a small-sized in-situ observation sample for a high-temperature laser scanning confocal microscope according to claim 1, characterized in that: In step (d), the second grinding method includes: firstly performing coarse grinding and then performing fine grinding until the scratches formed in the previous pass disappear; And / or, in step (d), the polishing method comprises: polishing to a mirror surface using a polishing paste with a particle size of 0.25 μm to 0.05 μm.
7. The method for preparing a small-sized in-situ observation sample for a high-temperature laser scanning confocal microscope according to claim 1, characterized in that: The organic solvent includes at least one of acetone, thinner, dichloromethane and alcohol.
8. The method for preparing a small-sized in-situ observation sample for a high-temperature laser scanning confocal microscope according to claim 1, characterized in that: The soaking time is 1 to 5 hours.
9. Application of the small-size in-situ observation sample for high-temperature laser scanning confocal microscope prepared by the method for preparing the small-size in-situ observation sample for high-temperature laser scanning confocal microscope as described in any one of claims 1 to 8 in observing and analyzing the phase change and microstructural change of metal materials.
10. The use according to claim 9, characterized in that: The first plane in the small-size in-situ observation sample of the high-temperature laser scanning confocal microscope is in-situ observed by using the high-temperature laser scanning confocal microscope.