Preparation method of nano NiAg / porous heterojunction Bi2MoO6 / TiO2 visible light photocatalyst for water splitting

The nano NiAg/porous heterojunction Bi2MoO6/TiO2 photocatalyst addresses the limitations of existing catalysts by enhancing visible light utilization and electron-hole separation, enabling efficient water splitting into hydrogen and oxygen without additional agents.

CN118142546BActive Publication Date: 2024-12-06SHENZHEN HONGYUE ENTERPRISE MANAGEMENT CONSULTING CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410264001.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-08
Publication Date
2024-12-06
Estimated Expiration
2044-03-08

AI Technical Summary

Technical Problem

Existing photocatalysts for water splitting have limited sunlight utilization due to narrow light absorption ranges, low electron-hole separation ability, and photocorrosion issues, and they often require sacrificial agents or co-catalysts, limiting their efficiency and applicability.

Method used

A nano NiAg/porous heterojunction Bi2MoO6/TiO2 photocatalyst is prepared through a method involving the synthesis of nano-TiO2 nanotubes, formation of a porous Bi2MoO6/TiO2 heterojunction, and incorporation of NiAg alloy to enhance visible light photocatalytic activity without additional agents.

Benefits of technology

The catalyst achieves high visible light photocatalytic efficiency for water splitting, with improved electron-hole pair separation and catalytic activity, producing hydrogen and oxygen simultaneously under visible light without sacrificial agents or co-catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118142546B_ABST
    Figure CN118142546B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of catalyst technology, and in particular to a method for preparing a nano NiAg / porous heterojunction Bi2MoO6 / TiO2 visible light photocatalyst for water splitting, comprising: S1, synthesis of nano TiO2; S2, synthesis of TiO2 nanotubes; S3, synthesis of porous heterojunction Bi2MoO6 / TiO2; S4, synthesis of nano NiAg / porous heterojunction Bi2MoO6 / TiO2. The present invention is composited with porous heterojunction Bi2MoO6 / TiO2 and nano NiAg alloy. The nano NiAg / porous heterojunction Bi2MoO6 / TiO2 prepared by the present invention has a large specific surface area, a small particle size, a band gap energy of 2.38 eV, greatly improved separation efficiency and photocatalytic activity of photogenerated electron-hole pairs, and high visible light photocatalytic water splitting efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalyst technology, and in particular to a nano NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 A method for preparing a visible light photocatalyst for water splitting. Background Art

[0002] Hydrogen (H 2 ) has the advantages of high energy density, wide range of sources, and environmental friendliness. It can release energy through direct combustion or hydrogen fuel cells and is considered to be one of the most ideal substitutes for fossil fuels. Solar catalytic hydrogen production refers to the process of using photon energy to decompose water into H under the irradiation of light through a catalyst. 2 and O 2 Solar energy has the advantages of being inexhaustible, clean, pollution-free and renewable. As people are increasingly concerned about the reduction of energy resources and the deterioration of the environment, solar energy has become a very promising alternative to fossil fuels. Using solar energy to produce hydrogen with water as raw material is one of the ideal ways to fundamentally solve the problems of energy and environmental pollution.

[0003] Commonly used photocatalysts in the photocatalytic process are precious metals, metal oxides such as TiO 2 、SrTiO 3 、BiVO 4 、Metal sulfide CdS、ZnIn 2 S 4 , gC 3 N 4and metal organic frameworks (MOFs). However, from the perspective of the efficiency of utilizing sunlight, these catalysts have a narrow light absorption range, mainly absorbing energy in the ultraviolet region, and have low sunlight utilization. In addition, metal oxides and metal sulfides have weak electron-hole separation ability and photocorrosion problems, resulting in low photocatalytic hydrogen production activity. Alkaline earth metal tantalates have special structures and high conduction bands, and their photocatalytic water decomposition has certain advantages. However, their bandgap width is very large, which greatly reduces the utilization rate of solar energy. It is necessary to improve energy utilization through doping or modification methods. On the premise of ensuring that oxygen can be precipitated, the valence band can be adjusted and controlled by anion doping methods such as carbon doping, nitrogen doping, sulfur doping, and fluorine doping to narrow the bandgap width, or by using other elements such as doping silver ions, bismuth ions, etc. to create new valence bands and improve photocatalytic performance. Ion exchange layered perovskite photocatalysts such as niobate photocatalysts cannot undergo hydration when they exist in their original state. However, they can be hydrated when the alkali metal cations between the layers are exchanged by protons. After exchanging protons and loading Pt, this type of catalyst can significantly improve the efficiency of photocatalytic water decomposition to release hydrogen. However, even if this type of catalyst is loaded with a co-catalyst, it cannot release hydrogen and oxygen simultaneously by photocatalytic water decomposition, and a sacrificial agent is required. This is because the complete decomposition of water into hydrogen and oxygen must be carried out under alkaline conditions, and this type of catalyst cannot undergo hydration under alkaline conditions (proton exchange cannot occur), thereby inhibiting its catalytic activity. In the solar spectrum, ultraviolet light (below 400nm) accounts for less than 5%, while visible light with a wavelength of 400-750nm accounts for 43%. In order to effectively utilize sunlight, it is of great significance to study cheap, environmentally friendly and high-performance visible light photocatalysts for water decomposition. Photocatalysts with visible light activity include Pt / CdS, WO 3 , AgNbO 3 ,Bi 2 WO 6 ,Bi 2 MoO 6 ,In 2 O 3 (ZnO) 3 , Pt / In 2 O 3 (ZnO) 3 , Pt / SrTiO 3 :Cr, Sb, Cu-ZnS, etc. Most of these catalysts are used for visible light photocatalytic degradation of wastewater and exhaust gas. Nano NiAg / porous heterojunction Bi with high visible light photocatalytic activity 2 MoO 6 / TiO 2 Photocatalytic water splitting catalysts have not been reported. Summary of the invention

[0004] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a nano NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 The invention discloses a method for preparing a visible light photocatalytic water splitting catalyst. The prepared catalyst has high visible light photocatalytic activity and high visible light photocatalytic efficiency for water splitting without adding a sacrificial agent or a co-catalyst.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A nano NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 The preparation method of the visible light photocatalyst for water splitting comprises the following steps:

[0007] S1, Nano-TiO 2 Synthesis: dissolve butyl titanate in anhydrous ethanol, add a mixture of anhydrous ethanol, glacial acetic acid and deionized water dropwise while stirring, hydrolyze to form a sol and continue stirring until a gel is formed, let stand for 2-3 days, vacuum dry at 80-100℃ for 8-10 hours, grind, and air roast at 500℃ for 3.5 hours to obtain nano TiO 2 ;

[0008] S2、TiO 2 Synthesis of nanotubes: Nano-TiO prepared by S1 2 The mixture was mixed with 50-60 mL of 10 mol / L NaOH solution, and the mixed solution was added into a 100 mL polytetrafluoroethylene-lined stainless steel high-pressure hydrothermal reactor, reacted at 180 ° C for 24 h, and naturally cooled to room temperature; the precipitate in the reactor was washed with 0.1 mol / L HCl solution and deionized water for 3 times, dried in an oven, and calcined in a muffle furnace at 500 ° C for 3.5 hours to obtain TiO 2 Nanotubes;

[0009] S3, porous heterojunction Bi 2 MoO 6 / TiO 2 Synthesis: Weigh a certain amount of Bi(NO 3 ) 3 ·5H 2 O、(NH 4 ) 6 Mo 7 O 24 ·4H 2 TiO synthesized from O and S2 2The nanotubes were dissolved in a certain amount of ethylene glycol, and the dispersion formed by stirring was transferred into a 100 mL polytetrafluoroethylene-lined stainless steel hydrothermal reactor, reacted at 160°C for 15 h, and naturally cooled to room temperature; the precipitate in the reactor was washed with deionized water 6 times and dried to obtain a porous heterojunction Bi 2 MoO 6 / TiO 2 ;

[0010] S4, Nano-NiAg / Porous Heterojunction Bi 2 MoO 6 / TiO 2 Synthesis: A certain amount of porous heterojunction Bi prepared by S3 2 MoO 6 / TiO 2 Add 10-20 mg / ml into deionized water and disperse evenly by ultrasonic to form Bi 2 MoO 6 / TiO 2 dispersion, adding a certain amount of NiSO 4 Solution and AgNO 3 The solution was stirred and the pH value of the dispersion was adjusted to 8.5-12 with aqueous ammonia. A certain amount of KBH 4 The solution was stirred for 2-6 hours, filtered after the reaction was completed, washed with deionized water until there were no chloride ions and sulfate ions in the filtrate, and dried in a vacuum at 80-120°C to obtain NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 Visible light photocatalyst for water splitting.

[0011] Preferably, in step S1, the molar ratio of butyl titanate, anhydrous ethanol, glacial acetic acid and deionized water is 1:(20-40):(1-2.5):(2-6).

[0012] Preferably, in step S3, Bi(NO 3 ) 3 ·5H 2 O and (NH 4 ) 6 Mo 7 O 24 ·4H 2 The molar ratio of O n[Bi(NO 3 ) 3 ·5H 2 O]:n[(NH 4 ) 6 Mo 7 O 24 ·4H 2 O] is 14:1.

[0013] Preferably, in step S3, the amount of ethylene glycol is 50 mL.

[0014] Preferably, in step S3, TiO 2 The mass is Bi 2 MoO 6 Precursor Bi(NO 3 ) 3 ·5H 2 O and (NH 4 ) 6 Mo 7 O 24 ·4H 2 O synthesizes Bi 2 MoO 6 The quality of TiO 2 The mass ratio is 1:(1~4).

[0015] Preferably, in step S4, the certain amount of NiSO 4 Solution and AgNO 3 NiSO in solution 4 and AgNO 3 The molar ratio is 7:3, 1:1 or 3:7.

[0016] Preferably, in step S4, the certain amount of NiSO 4 Solution and AgNO 3 The sum of the contents of NiAg nanoalloy and NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 1-5% of the total amount.

[0017] Preferably, in step S4, KBH 4 The amount of NiSO added is 4 and AgNO 3 5 times the sum of the molar numbers.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. Nano NiAg / porous heterojunction Bi prepared by the present invention 2 MoO 6 / TiO 2 The characteristic diffraction peaks also contain Bi 2 MoO 6 With anatase TiO 2 The characteristic peaks of the porous heterojunction Bi 2 MoO 6 / TiO 2 , NiAg / porous heterojunction Bi2 MoO 6 / TiO 2 The characteristic diffraction peaks of Bi 2 MoO 6 and TiO 2 Compared with the NiAg alloy, there is a small offset between the porous heterojunction Bi 2 MoO 6 / TiO 2 There is a strong interaction between the nano-NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 The presence of lattice defects improves the catalytic activity.

[0020] 2. Nano NiAg / porous heterojunction Bi prepared by the present invention 2 MoO 6 / TiO 2 The specific surface area is larger and the catalytic performance is improved.

[0021] 3. Due to nano Bi 2 MoO 6 The band gap energy is about 2.64eV, and the anatase nano-TiO 2 The band gap energy of the nano NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 The band gap energy is only 2.38 eV, which further reduces the TiO 2 The band gap energy is beneficial to improve the separation efficiency of electron-hole pairs and enhance the visible light photocatalytic performance.

[0022] 4. In the present invention, under visible light excitation, Bi 2 MoO 6 and TiO 2 Electrons and holes can be generated separately, and electrons are generated from Bi 2 MoO 6 and TiO 2 The respective valence band (VB) transitions to the conduction band (CB), leaving holes in the VB, and TiO 2 The electrons in the CB are transferred from TiO 2 Transfer to Bi 2 MoO 6 , then Bi 2 MoO 6 The holes in VB are from Bi 2 MoO 6 Transfer to TiO 2 , gathered in Bi 2 MoO 6 The electrons on the CB participate in the H+ The restoration of Bi 2 MoO 6 The NiAg alloy on the surface has a high electron conductivity, which accelerates the electron transfer speed and greatly improves the efficiency of photocatalytic hydrogen production; TiO 2 The holes in the VB can decompose H 2 O generates O 2 , NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 It can significantly improve the separation efficiency and photocatalytic activity of photogenerated electron-hole pairs, and has high visible light photocatalytic efficiency for water splitting. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The TiO prepared in Example 1 of the present invention 2 TEM test results of nanotubes;

[0024] Figure 2 The nano NiAg / porous heterojunction Bi prepared in Example 1 of the present invention 2 MoO 6 / TiO 2 SEM images of

[0025] Figure 3 The TiO prepared in Example 1 of the present invention 2 、Bi 2 MoO 6 and nano-NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 UV-Vis diffuse reflectance spectrum;

[0026] Figure 4 The nano Bi of Example 1 of the present invention 2 WO 6 -TiO 2 Schematic diagram of photolysis of water under visible light excitation;

[0027] Figure 5 TiO 2 Nanotubes, Bi 2 MoO 6 and Example 1 Nano NiAg / Porous Heterojunction Bi 2 MoO 6 / TiO 2 XRD spectrum of

[0028] Among them, (a) TiO 2 ; (b)Bi 2 MoO 6 ; (c) NiAg / Bi2 MoO 6 / TiO 2 . DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings, so that those skilled in the art can better understand the advantages and features of the present invention, thereby making a clearer definition of the protection scope of the present invention. The embodiments described in the present invention are only a part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0030] Embodiment 1:

[0031] A nano NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 The preparation method of the visible light photocatalyst for water splitting comprises the following steps:

[0032] S1, Nano-TiO 2 Synthesis: 17 mL of butyl titanate was dissolved in 22 mL of anhydrous ethanol, and a mixture of 22 mL of anhydrous ethanol, 3.6 mL of glacial acetic acid and 3.6 mL of deionized water was added dropwise under stirring. After hydrolysis to form a sol, stirring was continued. After the gel was formed, it was allowed to stand for 2-3 days. The powder was dried at 80 ° C in vacuum for 8-10 hours and then ground and calcined in a muffle furnace at 500 ° C for 3.5 hours to obtain 4 g of nano-TiO 2 .

[0033] S2、TiO 2 Synthesis of nanotubes: Nano-TiO prepared by S1 2 Mix with 50mL of 10mol / L NaOH solution, add the mixed solution into 100mL polytetrafluoroethylene-lined stainless steel high-pressure hydrothermal reactor, react at 180℃ for 24h, and cool naturally to room temperature. The precipitate in the reactor was washed 3 times with 0.1mol / L HCl solution and deionized water respectively, dried in an oven, and calcined in air at 500℃ in a muffle furnace for 3.5 hours to obtain TiO 2 Nanotubes.

[0034] S3, porous heterojunction Bi 2 MoO 6 / TiO 2 Synthesis: Weigh 1.59 g of Bi(NO 3 ) 3 ·5H 2 O, 0.29 g (NH 4 )6 Mo 7 O 24 ·4H 2 TiO synthesized from O and S2 2 1g of nanotubes was dissolved in 50mL of ethylene glycol, and the resulting dispersion was transferred into a 100mL stainless steel hydrothermal reactor lined with polytetrafluoroethylene, and reacted at 160°C for 15h, and then cooled naturally to room temperature. The precipitate in the reactor was washed with deionized water 6 times and dried to obtain about 2g of Bi 2 MoO 6 The quality of TiO 2 The porous heterojunction Bi with a mass ratio of 1:1 2 MoO 6 / TiO 2 .

[0035] S4, Nano-NiAg / Porous Heterojunction Bi 2 MoO 6 / TiO 2 Synthesis: 1g of porous heterojunction Bi prepared by S3 2 MoO 6 / TiO 2 Add to 50mL deionized water and disperse evenly by ultrasonic to form Bi 2 MoO 6 / TiO 2 Dispersion, add 1.86mL of 0.1mol / L NiSO 4 solution and 1.86 mL of 0.1 mol / L AgNO 3 The solution was stirred and the pH value of the dispersion was adjusted to 8.5-12 with aqueous ammonia. 7.42 mL of 0.25 mol / L KBH 4 The solution is stirred for reaction for 2-6 hours, filtered after the reaction is completed, washed with deionized water until there is no chloride ion and sulfate ion in the filtrate, and dried in vacuum at 80-120°C to obtain a NiAg molar ratio of 1:1, and the sum of the contents of the NiAg nanoalloy is NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 3% of the total amount, Bi 2 MoO 6 The quality of TiO 2 The mass ratio of NiAg / porous heterojunction Bi is 1:1 2 MoO 6 / TiO 2 Visible light photocatalyst for water splitting.

[0036] Embodiment 2:

[0037] A nano NiAg / porous heterojunction Bi2 MoO 6 / TiO 2 The preparation method of the visible light photocatalyst for water splitting comprises the following steps:

[0038] S1, Nano-TiO 2 Synthesis: 17 mL of butyl titanate was dissolved in 22 mL of anhydrous ethanol, and a mixture of 22 mL of anhydrous ethanol, 3.6 mL of glacial acetic acid and 3.6 mL of deionized water was added dropwise under stirring. After hydrolysis to form a sol, stirring was continued. After the gel was formed, it was allowed to stand for 2-3 days. The powder was dried at 80 ° C in vacuum for 8-10 hours and then ground and calcined in a muffle furnace at 500 ° C for 3.5 hours to obtain 4 g of nano-TiO 2 .

[0039] S2、TiO 2 Synthesis of nanotubes: Nano-TiO prepared by S1 2 Mix with 50mL of 10mol / L NaOH solution, add the mixed solution into 100mL polytetrafluoroethylene-lined stainless steel high-pressure hydrothermal reactor, react at 180℃ for 24h, and cool naturally to room temperature. The precipitate in the reactor was washed 3 times with 0.1mol / L HCl solution and deionized water respectively, dried in an oven, and calcined in air at 500℃ in a muffle furnace for 3.5 hours to obtain TiO 2 Nanotubes.

[0040] S3, porous heterojunction Bi 2 MoO 6 / TiO 2 Synthesis: Weigh 1.59 g of Bi(NO 3 ) 3 ·5H 2 O, 0.29 g (NH 4 ) 6 Mo 7 O 24 ·4H 2 TiO synthesized from O and S2 2 2g of nanotubes were dissolved in 50mL of ethylene glycol, and the resulting dispersion was transferred into a 100mL stainless steel hydrothermal reactor lined with polytetrafluoroethylene, and reacted at 160°C for 15h, and then cooled naturally to room temperature. The precipitate in the reactor was washed with deionized water 6 times and dried to obtain about 3g of Bi 2 MoO 6 The quality of TiO 2 The porous heterojunction Bi with a mass ratio of 1:2 2 MoO 6 / TiO 2 .

[0041] S4, Nano-NiAg / Porous Heterojunction Bi 2MoO 6 / TiO 2 Synthesis: 1g of porous heterojunction Bi prepared by S3 2 MoO 6 / TiO 2 Add to 50mL deionized water, disperse evenly by ultrasonic to form Bi 2 MoO 6 / TiO 2 Dispersion, add 5.02mL of 0.1mol / L NiSO 4 solution and 2.15 mL of 0.1 mol / L AgNO 3 The solution was stirred and the pH value of the dispersion was adjusted to 8.5-12 with aqueous ammonia. 7.2 mL of 0.5 mol / L KBH 4 The solution was stirred for reaction for 2-6 hours, filtered after the reaction was completed, washed with deionized water until there was no chloride ion and sulfate ion in the filtrate, and dried in vacuum at 80-120°C to obtain a NiAg molar ratio of 7:3, and the sum of the contents of the NiAg nanoalloy was NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 5% of the total amount, Bi 2 MoO 6 The quality of TiO 2 The mass ratio of NiAg / porous heterojunction Bi is 1:2 2 MoO 6 / TiO 2 Visible light photocatalyst for water splitting.

[0042] Embodiment 3:

[0043] A nano NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 The preparation method of the visible light photocatalyst for water splitting comprises the following steps:

[0044] S1, Nano-TiO 2 Synthesis: 17 mL of butyl titanate was dissolved in 22 mL of anhydrous ethanol, and a mixture of 22 mL of anhydrous ethanol, 3.6 mL of glacial acetic acid and 3.6 mL of deionized water was added dropwise under stirring. After hydrolysis to form a sol, stirring was continued. After the gel was formed, it was allowed to stand for 2-3 days. The powder was dried at 80 ° C in vacuum for 8-10 hours and then ground and calcined in a muffle furnace at 500 ° C for 3.5 hours to obtain 4 g of nano-TiO 2 .

[0045] S2、TiO 2 Synthesis of nanotubes: Nano-TiO prepared by S1 2Mix with 50mL of 10mol / L NaOH solution, add the mixed solution into 100mL polytetrafluoroethylene-lined stainless steel high-pressure hydrothermal reactor, react at 180℃ for 24h, and cool naturally to room temperature. The precipitate in the reactor was washed 3 times with 0.1mol / L HCl solution and deionized water respectively, dried in an oven, and calcined in air at 500℃ in a muffle furnace for 3.5 hours to obtain TiO 2 Nanotubes.

[0046] S3, porous heterojunction Bi 2 MoO 6 / TiO 2 Synthesis: Weigh 1.59 g of Bi(NO 3 ) 3 ·5H 2 O, 0.29 g (NH 4 ) 6 Mo 7 O 24 ·4H 2 TiO synthesized from O and S2 2 3g of nanotubes were dissolved in 50mL of ethylene glycol, and the resulting dispersion was transferred into a 100mL stainless steel hydrothermal reactor lined with polytetrafluoroethylene, and reacted at 160°C for 15h, and then cooled naturally to room temperature. The precipitate in the reactor was washed with deionized water 6 times and dried to obtain about 4g of Bi 2 MoO 6 The quality of TiO 2 The porous heterojunction Bi with a mass ratio of 1:3 2 MoO 6 / TiO 2 .

[0047] S4, Nano-NiAg / Porous Heterojunction Bi 2 MoO 6 / TiO 2 Synthesis: 1g of porous heterojunction Bi prepared by S3 2 MoO 6 / TiO 2 Add to 50mL deionized water, disperse evenly by ultrasonic to form Bi 2 MoO 6 / TiO 2 Dispersion, add 0.65mL of 0.05mol / L NiSO 4 solution and 0.76 mL of 0.1 mol / L AgNO 3 The solution was stirred and the pH value of the dispersion was adjusted to 8.5-12 with aqueous ammonia. 5.42 mL of 0.1 mol / L KBH 4The solution was stirred for reaction for 2-6 hours, filtered after the reaction was completed, washed with deionized water until there was no chloride ion and sulfate ion in the filtrate, and dried in vacuum at 80-120°C to obtain a NiAg molar ratio of 3:7, and the sum of the contents of the NiAg nanoalloy was NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 1% of the total amount, Bi 2 MoO 6 The quality of TiO 2 The mass ratio of NiAg / porous heterojunction Bi is 1:3 2 MoO 6 / TiO 2 Visible light photocatalyst for water splitting.

[0048] Embodiment 4:

[0049] A nano NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 The preparation method of the visible light photocatalyst for water splitting comprises the following steps:

[0050] S1, Nano-TiO 2 Synthesis: 17 mL of butyl titanate was dissolved in 22 mL of anhydrous ethanol, and a mixture of 22 mL of anhydrous ethanol, 3.6 mL of glacial acetic acid and 3.6 mL of deionized water was added dropwise under stirring. After hydrolysis to form a sol, stirring was continued. After the gel was formed, it was allowed to stand for 2-3 days. The powder was dried at 80 ° C in vacuum for 8-10 hours and then ground and calcined in a muffle furnace at 500 ° C for 3.5 hours to obtain 4 g of nano-TiO 2 .

[0051] S2、TiO 2 Synthesis of nanotubes: Nano-TiO prepared by S1 2 Mix with 50mL of 10mol / L NaOH solution, add the mixed solution into 100mL polytetrafluoroethylene-lined stainless steel high-pressure hydrothermal reactor, react at 180℃ for 24h, and cool naturally to room temperature. The precipitate in the reactor was washed 3 times with 0.1mol / L HCl solution and deionized water respectively, dried in an oven, and calcined in air at 500℃ in a muffle furnace for 3.5 hours to obtain TiO 2 Nanotubes.

[0052] S3, porous heterojunction Bi 2 MoO 6 / TiO 2 Synthesis: Weigh 1.59 g of Bi(NO 3 ) 3 ·5H 2 O, 0.29 g (NH4 ) 6 Mo 7 O 24 ·4H 2 TiO synthesized from O and S2 2 3g of nanotubes were dissolved in 50mL of ethylene glycol, and the resulting dispersion was transferred into a 100mL stainless steel hydrothermal reactor lined with polytetrafluoroethylene, and reacted at 160°C for 15h, and then cooled naturally to room temperature. The precipitate in the reactor was washed with deionized water 6 times and dried to obtain about 4g of Bi 2 MoO 6 The quality of TiO 2 The porous heterojunction Bi with a mass ratio of 1:3 2 MoO 6 / TiO 2 .

[0053] S4, Nano-NiAg / Porous Heterojunction Bi 2 MoO 6 / TiO 2 Synthesis: 1g of porous heterojunction Bi prepared by S3 2 MoO 6 / TiO 2 Add to 50mL deionized water and disperse evenly by ultrasonic to form Bi 2 MoO 6 / TiO 2 Dispersion, add 1.86mL of 0.1mol / L NiSO 4 solution and 1.86 mL of 0.1 mol / L AgNO 3 The solution was stirred and the pH value of the dispersion was adjusted to 8.5-12 with aqueous ammonia. 7.42 mL of 0.25 mol / L KBH 4 The solution is stirred for reaction for 2-6 hours, filtered after the reaction is completed, washed with deionized water until there is no chloride ion and sulfate ion in the filtrate, and dried in vacuum at 80-120°C to obtain a NiAg molar ratio of 1:1, and the sum of the contents of the NiAg nanoalloy is NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 3% of the total amount, Bi 2 MoO 6 The quality of TiO 2 The mass ratio of NiAg / porous heterojunction Bi is 1:3 2 MoO 6 / TiO 2 Visible light photocatalyst for water splitting.

[0054] Figure 1It can be seen that it has a tubular structure, has a large specific surface area, and has improved catalytic performance.

[0055] Figure 2 It shows that TiO 2 The surface is a thin layer of Bi 2 MoO 6 , forming a heterojunction structure, on the surface of which smaller silver nanoparticles can be seen.

[0056] Figure 3 As shown, the tangent line of the UV-visible diffuse reflectance spectrum curve is drawn, and TiO 2 、Bi 2 MoO 6 and nano-NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 The absorption edges of Bi 2 MoO 6 and nano-NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 The excitation band has been extended from ultraviolet light to visible light.

[0057] According to the bandgap calculation formula: Eg = 1240 / λ

[0058] The calculated Bi prepared in Example 1 is 2 MoO 6 and nano-NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 The band gap widths of nano-NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 Make TiO 2 The band gap energy is further reduced from 3.2 eV to 2.38 eV under visible light excitation, which can greatly improve the catalytic performance.

[0059] Figure 4 As shown, under visible light excitation, Bi 2 MoO 6 and TiO 2 Electrons and holes can be generated separately, and electrons are generated from Bi 2 MoO 6 and TiO 2 The respective valence band (VB) transitions to the conduction band (CB), leaving holes in the VB, and TiO 2 The electrons in the CB are transferred from TiO 2 Transfer to Bi2 MoO 6 , then Bi 2 MoO 6 The holes in VB are from Bi 2 MoO 6 Transfer to TiO 2 , gathered in Bi 2 MoO 6 The electrons on the CB participate in the H + The restoration of Bi 2 MoO 6 The NiAg alloy on the surface has a high electron conductivity, which accelerates the electron transfer speed and greatly improves the efficiency of photocatalytic hydrogen production; TiO 2 The holes in the VB can decompose H 2 O generates O 2 , NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 It can significantly improve the separation efficiency and photocatalytic activity of photogenerated electron-hole pairs, and has high visible light photocatalytic efficiency for water splitting.

[0060] Figure 5 It can be seen that nano NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 The characteristic diffraction peaks also contain Bi 2 MoO 6 With anatase TiO 2 The characteristic peaks of the porous heterojunction Bi 2 MoO 6 / TiO 2 , NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 The characteristic diffraction peaks of Bi 2 MoO 6 and TiO 2 Compared with the NiAg alloy, there is a small offset between the porous heterojunction Bi 2 MoO 6 / TiO 2 There is a strong interaction between the nano-NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 The presence of lattice defects improves the catalytic activity.

[0061] Table 1 shows the TiO2 nanotubes, nano Bi2MoO6 synthesized in Example 1 without adding TiO2 nanotubes, and nanoporous heterojunction Bi 2 MoO6 / TiO 2 and nano-NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 Surface area test results.

[0062] Table 1 Specific surface area test results of samples

[0063] Sample name <![CDATA[Specific surface area / m 2 > <![CDATA[TiO 2 Nanotubes]]> 83.4 <![CDATA[Bi 2 MoO 6 ]]> 26.4 <![CDATA[Nano-porous heterojunction Bi 2 MoO 6 / TiO 2 > 103.2 <![CDATA[Nano NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 > 98.6

[0064] Table 1 shows that TiO2 nanotubes, nano Bi2MoO6 synthesized in Example 1 without adding TiO2 nanotubes, and nanoporous heterojunction Bi 2 MoO 6 / TiO 2 and nano-NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 Both have a large specific surface area, which is beneficial to the nano-NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 Improved catalytic performance.

[0065] Photocatalytic water splitting experiment of the present invention: In a photocatalytic reaction device, 50 mg of NiAg / porous heterojunction Bi prepared in Example 1 was stirred under magnetic stirring. 2 MoO 6 / TiO 2 The photocatalyst was dispersed in 100 mL of deionized water, nitrogen was passed through for 10 minutes, and vacuum was drawn. A 300 W xenon lamp was used as the light source, the cooling water temperature in the cooling circulation system was maintained at 5 °C, the online GC-7920 gas chromatograph was equipped with a thermal conductivity detector and a 0.5 nm molecular sieve column, the column box temperature was 60 °C, the injector temperature was 120 °C, the bridge current was 60 mA, the detection temperature of the detector was 120 °C, high-purity nitrogen was used as the carrier gas, and the flow rate was 18 mL min -1 , and detect the evolved gas. The photocatalytic decomposition of deionized water without any sacrificial agent or co-catalyst generates H 2 and O 2 The rates were 3.06 μmol·h -1 ·g -1 and 1.48 μmol·h -1 ·g -1 , indicating that NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 The photocatalyst for water splitting has high visible light catalytic performance and high visible light photocatalytic efficiency for water splitting.

[0066] The description and practice disclosed in the present invention are easy to think and understand for ordinary technicians in this technical field, and several improvements and modifications can be made without departing from the principles of the present invention. Therefore, modifications or improvements made without departing from the spirit of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A nano-NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 Preparation method of visible light photocatalyst for water splitting, It is characterized in that The following steps are involved: S1, Nano-TiO 2 Synthesis: dissolve butyl titanate in anhydrous ethanol, add a mixture of anhydrous ethanol, glacial acetic acid and deionized water dropwise while stirring, hydrolyze to form a sol and continue stirring until a gel is formed, let stand for 2-3 days, vacuum dry at 80-100℃ for 8-10 hours, grind, and air roast at 500℃ for 3.5 hours to obtain nano TiO 2 ; S2、TiO 2 Synthesis of nanotubes: Nano-TiO prepared by S1 2 The mixture was mixed with 50-60 mL of 10 mol / L NaOH solution, and the mixed solution was added into a 100 mL polytetrafluoroethylene-lined stainless steel high-pressure hydrothermal reactor, reacted at 180 °C for 24 h, and naturally cooled to room temperature; the precipitate in the reactor was washed with 0.1 mol / L HCl solution and deionized water for 3 times, dried in an oven, and calcined in a muffle furnace at 500 °C for 3.5 hours to obtain TiO 2 Nanotubes; S3, porous heterojunction Bi 2 MoO 6 / TiO 2 Synthesis: Weigh a certain amount of Bi(NO 3 ) 3 ·5H 2 O、(NH 4 ) 6 Mo 7 O 24 ·4H 2 TiO synthesized from O and S2 2 The nanotubes were dissolved in a certain amount of ethylene glycol, and the dispersion formed by stirring was transferred into a 100 mL polytetrafluoroethylene-lined stainless steel hydrothermal reactor, reacted at 160°C for 15 h, and naturally cooled to room temperature; the precipitate in the reactor was washed with deionized water 6 times and dried to obtain a porous heterojunction Bi 2 MoO 6 / TiO 2 ; S4, Nano-NiAg / Porous Heterojunction Bi 2 MoO 6 / TiO 2 Synthesis: A certain amount of porous heterojunction Bi prepared by S3 2 MoO 6 / TiO 2 Add 10-20 mg / ml into deionized water and disperse evenly by ultrasonic to form Bi 2 MoO 6 / TiO 2 dispersion, adding a certain amount of NiSO 4 Solution and AgNO 3 The solution was stirred and the pH value of the dispersion was adjusted to 8.5-12 with aqueous ammonia. A certain amount of KBH 4 The solution was stirred for 2-6 hours, filtered after the reaction was completed, washed with deionized water until there were no chloride ions and sulfate ions in the filtrate, and dried in a vacuum at 80-120°C to obtain NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 Visible light photocatalyst for water splitting.

2. A nano NiAg / porous heterojunction Bi according to claim 1 2 MoO 6 / TiO 2 Preparation method of visible light photocatalyst for water splitting, It is characterized in that In step S1, the molar ratio of butyl titanate, anhydrous ethanol, glacial acetic acid and deionized water is 1:(20-40):(1-2.5):(2-6).

3. A nano NiAg / porous heterojunction Bi according to claim 1 2 MoO 6 / TiO 2 Preparation method of visible light photocatalyst for water splitting, It is characterized in that In step S3, the molar ratio n[Bi(NO 3 ) 3 ·5H 2 O]:n[(NH 4 ) 6 Mo 7 O 24 ·4H 2 O] of Bi(NO 3 ) 3 ·5H 2 O and (NH 4 ) 6 Mo 7 O 24 ·4H 2 O is 14:

1.

4. A nano NiAg / porous heterojunction Bi according to claim 1 2 MoO 6 / TiO 2 Preparation method of visible light photocatalyst for water splitting, It is characterized in that In step S3, the amount of ethylene glycol is 50 mL.

5. A nano NiAg / porous heterojunction Bi according to claim 1 2 MoO 6 / TiO 2 Preparation method of visible light photocatalyst for water splitting, It is characterized in that In step S3, Bi 2 MoO 6 Precursor Bi(NO 3 ) 3 ·5H 2 O and (NH 4 ) 6 Mo 7 O 24 ·4H 2 O synthesizes Bi 2 MoO 6 The quality of TiO 2 The mass ratio is 1:(1~4).

6. A nano NiAg / porous heterojunction Bi according to claim 1 2 MoO 6 / TiO 2 Preparation method of visible light photocatalyst for water splitting, It is characterized in that In step S4, the certain amount of NiSO 4 Solution and AgNO 3 NiSO in solution 4 and AgNO 3 The molar ratio is 7:3, 1:1 or 3:

7.

7. A nano NiAg / porous heterojunction Bi according to claim 1 2 MoO 6 / TiO 2 Preparation method of visible light photocatalyst for water splitting, It is characterized in that In step S4, the certain amount of NiSO 4 Solution and AgNO 3 The sum of the contents of NiAg nanoalloy and NiAg / porous heterojunction Bi 2 MoO 6 / TiO 2 1~5% of the total amount.

8. A nano NiAg / porous heterojunction Bi according to claim 1 2 MoO 6 / TiO 2 Preparation method of visible light photocatalyst for water splitting, It is characterized in that In step S4, KBH 4 The amount of NiSO added is 4 and AgNO 3 5 times the sum of the molar numbers.

Citation Information

Patent Citations

  • Molybdenum and bismuth composite oxide, preparation method thereof, and organic solar cell

    CN106784319A

  • Preparation method of nano Bi2WO6-TiO2 visible light water splitting catalyst

    CN116920823A