A high thermal conductivity metal filler and preparation method thereof
By preparing high-thermal conductivity metal filler and adding it to the resin matrix, the problem of insufficient bonding of metal filler and matrix is solved, the thermal conductivity and strength of the material are improved, and the glue material with high thermal conductivity is achieved.
Patent Information
- Application Number
- CN202410363286.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-28
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-03-28
AI Technical Summary
The existing metal fillers are not fully combined with the matrix, resulting in insufficient thermal conductivity and strength.
A high-thermal conductivity metal filler is prepared by placing aqueous solutions of glycol and palladium nitrate, polyvinylpyrrolidone solution and vulcanized nano-silver powder, and a series of stirring, feeding and calcining steps to form a high-thermal conductivity metal filler and add it to it. In the resin matrix, the bonding of filler and matrix is promoted.
It has achieved a glue material with good thermal conductivity and high thermal conductivity, which is suitable for materials with high thermal conductivity requirements.
Smart Images

Figure BDA0004763381230000131 
Figure BDA0004763381230000141
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal fillers, and in particular to a high thermal conductivity metal filler and a preparation method thereof. Background Art
[0002] With the development of modern high-tech, the application of thermal conductive fillers is becoming more and more extensive. Adding thermal conductive fillers to adhesives, inks, coatings, rubber plastics and other materials will give these materials special properties, making thermal conductive fillers widely used in aerospace, electronic communications, electronic printing and other industries. There are many ways to classify fillers. Commonly used high thermal conductive fillers in existing studies include carbon-based materials, metals and their oxides and nitrides. The metal material fillers currently used in research include metal foams, metal nanoparticles and metal oxide nanoparticles, such as nickel foam, copper foam, nanosilver particles, silver nanowires, etc. However, improper selection of metal fillers can easily lead to insufficient bonding between the filler and the matrix, resulting in poor overall thermal conductivity of the matrix and low strength. Summary of the invention
[0003] To this end, the present invention provides a method for preparing a high thermal conductivity metal filler, the steps comprising:
[0004] (1) preparing an aqueous solution of ethylene glycol and an aqueous solution of palladium nitrate; keeping the aqueous solution of ethylene glycol constant at 60±3° C. in a water bath, stirring the aqueous solution of ethylene glycol, adding acetylacetone and n-butyl titanate to the solution while stirring, stirring the mixed solution at 60±3° C. for 5 to 8 minutes after the addition is completed, adjusting the pH of the mixed solution to 3 with a nitric acid solution after the stirring is completed; then stirring the mixed solution at 60±3° C., adding the aqueous solution of palladium nitrate to the mixed solution while stirring, and continuing to stir the mixed solution at 60±3° C. for 20 to 30 minutes after the addition is completed; obtaining a mixed solution A;
[0005] (2) dissolving polyvinyl pyrrolidone in deionized water kept at 80±5° C. to obtain a polyvinyl pyrrolidone solution; adding a silver nitrate solution to the polyvinyl pyrrolidone solution under a heat preservation condition of 80±5° C., and stirring the solution at 80±5° C. for 10 to 15 minutes after the addition is completed, and then adding a sodium borohydride solution to the solution under stirring, and stirring the solution at 80±5° C. for 10 minutes after the addition is completed, and then adding a sodium sulfide solution to the solution under stirring, and stirring the solution at 80±5° C. for 80 to 100 minutes after the addition is completed, and then separating the solid and liquid, washing the solid phase with deionized water, and drying at 80° C. for more than 30 minutes to obtain sulfide nano silver powder;
[0006] (3) adding the sulfide nanosilver powder to an ethanol solution of polyvinyl pyrrolidone to form a suspension; keeping the suspension constant temperature at 70±5° C. in a water bath, stirring the suspension, and then adding the mixed solution A to the suspension under stirring; continuing to stir at 70±5° C. for 10 to 20 min after the addition is completed; then adding an aqueous solution of hydrazine hydrate under stirring, stirring at 70±5° C. for more than 2 h after the addition is completed, then separating the solid from the liquid, and calcining the solid phase at 300° C. in an argon atmosphere for 4 h to obtain a solid phase B;
[0007] (4) preparing an aqueous solution of cysteamine hydrochloride; adding the solid phase B to deionized water to form an aqueous suspension; stirring the aqueous suspension, and then adding the aqueous solution of cysteamine hydrochloride to the aqueous suspension under stirring; continuing to stir for more than 3 hours after the addition is completed, and then separating the solid and liquid, drying the solid phase at 60° C. for more than 40 minutes, adding the dried solid phase to an aqueous solution of tris(hydroxymethyl)aminomethane, stirring the solution, and then adding tannic acid and copper chloride to the solution under stirring, continuing to stir the solution for more than 1 hour after the addition is completed, and then separating the solid and liquid, washing the solid phase with deionized water, and drying at 60° C. for more than 80 minutes to obtain the high thermal conductivity metal filler.
[0008] Furthermore, in the step (1), in the aqueous solution of ethylene glycol, the volume percentage of ethylene glycol is 20% to 30%, and the solvent is water; in the aqueous solution of palladium nitrate, the concentration of palladium nitrate is 7 to 8 g / L, and the solvent is water; acetylacetone and n-butyl titanate are added to the aqueous solution of ethylene glycol at the volume ratio of ethylene glycol aqueous solution: acetylacetone: n-butyl titanate = 50:2:3 to 4; the concentration of the solute in the nitric acid solution is 2.5 mol / L; the ratio of the added volume of the aqueous solution of palladium nitrate to the added volume of n-butyl titanate is the aqueous solution of palladium nitrate: n-butyl titanate = 1 to 4:3 to 4.
[0009] Furthermore, in the step (2), in the polyvinyl pyrrolidone solution, the concentration of polyvinyl pyrrolidone is 0.6-0.8 g / L, in the silver nitrate solution, the concentration of silver nitrate is 10-15 g / L, and the solvent is water; in the sodium borohydride solution, the concentration of sodium borohydride is 3-4 g / L, and the solvent is water; in the sodium sulfide solution, the concentration of sodium sulfide is 50-60 g / L, and the solvent is water; the volume ratio of the silver nitrate solution, the sodium borohydride solution, the sodium sulfide solution and the polyvinyl pyrrolidone solution is polyvinyl pyrrolidone solution: silver nitrate solution: sodium borohydride solution: sodium sulfide solution = 100:6-10:20-22:0.03-0.04.
[0010] Furthermore, in the step (3), the solid-liquid mass ratio of the sulfide nano-silver powder added to the ethanol solution of polyvinyl pyrrolidone is sulfide nano-silver powder: ethanol solution of polyvinyl pyrrolidone = 1:200; wherein the concentration of polyvinyl pyrrolidone in the ethanol solution of polyvinyl pyrrolidone is 2 g / L, and the volume ratio of the mixed liquid A added to the suspension is suspension: mixed liquid A = 1:1; in the aqueous solution of hydrazine hydrate, the mass percentage of hydrazine hydrate is 30%; and the volume ratio of the added volume of the aqueous solution of hydrazine hydrate to the suspension is suspension: aqueous solution of hydrazine hydrate = 10:6-8.
[0011] Furthermore, in the step (4), the concentration of cysteamine hydrochloride in the aqueous solution of cysteamine hydrochloride is 10 g / L, and the solvent is water; the solid-liquid ratio of the solid phase B added to deionized water to form an aqueous suspension is solid phase B: deionized water = 1 g: 50 mL, and the volume ratio of the aqueous solution of cysteamine hydrochloride added to the aqueous suspension is aqueous suspension: aqueous solution of cysteamine hydrochloride = 10:1.
[0012] Furthermore, in the step (4), the concentration of tris(hydroxymethyl)aminomethane in the aqueous solution of tris(hydroxymethyl)aminomethane is 6-8 g / L, the solid-liquid mass ratio of the dried solid phase added to the aqueous solution of tris(hydroxymethyl)aminomethane is the dried solid phase: aqueous solution of tris(hydroxymethyl)aminomethane = 1:50, and the mass ratio of tannic acid and copper chloride added to the solution to the aqueous solution of tris(hydroxymethyl)aminomethane is tannic acid: copper chloride: aqueous solution of tris(hydroxymethyl)aminomethane = 0.02-0.03:0.01:50.
[0013] The beneficial effect of the present invention is that after the filler prepared by the method of the present invention is added to the resin matrix, a glue material with good thermal conductivity can be obtained, which has a high thermal conductivity and is suitable for occasions with high requirements for material thermal conductivity. DETAILED DESCRIPTION
[0014] The present invention will be further described below in conjunction with the embodiments.
[0015] Example 1
[0016] A method for preparing a high thermal conductivity metal filler, comprising the steps of:
[0017] (1) preparing an aqueous solution of ethylene glycol and an aqueous solution of palladium nitrate; in the aqueous solution of ethylene glycol, the volume percentage of ethylene glycol is 20%, and the solvent is water; in the aqueous solution of palladium nitrate, the concentration of palladium nitrate is 7 g / L, and the solvent is water; keeping the aqueous solution of ethylene glycol constant at 60±3° C. in a water bath, stirring the aqueous solution of ethylene glycol, and simultaneously adding acetylacetone and n-butyl titanate to the solution under stirring, wherein the volume ratio of acetylacetone and n-butyl titanate added to the aqueous solution of ethylene glycol is ethylene glycol aqueous solution: acetylacetone: n-butyl titanate = 50:2:3; after the addition is completed, the mixed solution is stirred at a constant temperature of 60±3°C for 5 minutes, and after the stirring is completed, the pH of the mixed solution is adjusted to 3 with a nitric acid solution, and the concentration of the solute in the nitric acid solution is 2.5 mol / L; then the mixed solution is stirred at a constant temperature of 60±3°C, and the aqueous solution of palladium nitrate is added to the mixed solution under stirring, and the added volume ratio of the aqueous solution of palladium nitrate to the added volume of n-butyl titanate is the aqueous solution of palladium nitrate: n-butyl titanate = 1:3; after the addition is completed, the mixed solution is stirred at a constant temperature of 60±3°C for 30 minutes; a mixed solution A is obtained;
[0018] (2) dissolving polyvinyl pyrrolidone in deionized water kept at 80±5° C. to obtain a polyvinyl pyrrolidone solution; in the polyvinyl pyrrolidone solution, the concentration of polyvinyl pyrrolidone is 0.6 g / L; adding a silver nitrate solution to the polyvinyl pyrrolidone solution under the condition of keeping warm at 80±5° C., wherein the concentration of silver nitrate in the silver nitrate solution is 10 g / L, and the solvent is water; after the addition is completed, the solution is kept warm at 80±5° C. and stirred for 10 minutes, and then a sodium borohydride solution is added to the solution under stirring, wherein the concentration of sodium borohydride in the sodium borohydride solution is 3 g / L, and the solvent is water; after the addition is completed, The solution was stirred at 80±5°C for 10 minutes, and then a sodium sulfide solution was added to the solution under stirring, wherein the concentration of sodium sulfide in the sodium sulfide solution was 50 g / L, and the solvent was water; the volume ratio of the silver nitrate solution, the sodium borohydride solution, the sodium sulfide solution and the polyvinyl pyrrolidone solution was polyvinyl pyrrolidone solution: silver nitrate solution: sodium borohydride solution: sodium sulfide solution = 100:6:20:0.03; after the addition was completed, the solution was stirred at 80±5°C for 80 minutes, and then the solid-liquid separation was carried out, the solid phase was washed with deionized water, and dried at 80°C for 30 minutes to obtain sulfide nano silver powder;
[0019] (3) adding the sulfide nano-silver powder to an ethanol solution of polyvinyl pyrrolidone to form a suspension; the solid-liquid mass ratio of the sulfide nano-silver powder to the ethanol solution of polyvinyl pyrrolidone is sulfide nano-silver powder: ethanol solution of polyvinyl pyrrolidone = 1:200; wherein the concentration of polyvinyl pyrrolidone in the ethanol solution of polyvinyl pyrrolidone is 2 g / L, the suspension is kept at a constant temperature of 70±5° C. in a water bath, the suspension is stirred, and then the mixed solution A is added to the suspension under stirring; and the suspension is added to the mixed solution. The volume ratio of the mixed liquid A added to the suspension is suspension: mixed liquid A = 1:1; after the addition is completed, the mixture is stirred at a constant temperature of 70±5°C for 20 minutes; then an aqueous solution of hydrazine hydrate is added under stirring, wherein the mass percentage of hydrazine hydrate in the aqueous solution of hydrazine hydrate is 30%; the volume ratio of the added volume of the aqueous solution of hydrazine hydrate to the suspension is suspension: aqueous solution of hydrazine hydrate = 10:6; after the addition is completed, the mixture is stirred at a constant temperature of 70±5°C for 2 hours, and then the solid-liquid is separated, and the solid phase is calcined at 300°C in an argon atmosphere for 4 hours to obtain a solid phase B;
[0020] (4) preparing an aqueous solution of cysteamine hydrochloride; in the aqueous solution of cysteamine hydrochloride, the concentration of cysteamine hydrochloride is 10 g / L, and the solvent is water; adding the solid phase B into deionized water to form an aqueous suspension; the solid-liquid ratio of the solid phase B added into deionized water to form an aqueous suspension is solid phase B: deionized water = 1 g: 50 mL, stirring the aqueous suspension, and then adding the aqueous solution of cysteamine hydrochloride to the aqueous suspension under stirring; the volume ratio of the aqueous solution of cysteamine hydrochloride added into the aqueous suspension is aqueous suspension: aqueous solution of cysteamine hydrochloride = 10:1; stirring is continued for 3 hours after the addition is completed, and then solid-liquid separation is performed, the solid phase is dried at 60° C. for 40 minutes, and the dried solid phase is added to an aqueous solution of tris(hydroxymethyl)aminomethane. In the aqueous solution of tris(hydroxymethyl)aminomethane, the concentration of tris(hydroxymethyl)aminomethane is 6g / L, the dried solid phase is added to the aqueous solution of tris(hydroxymethyl)aminomethane in a solid-liquid mass ratio of the dried solid phase: aqueous solution of tris(hydroxymethyl)aminomethane=1:50, the solution is stirred, and then tannic acid and copper chloride are added to the solution under stirring, and the mass ratio of tannic acid and copper chloride added to the solution to the aqueous solution of tris(hydroxymethyl)aminomethane is tannic acid: copper chloride: aqueous solution of tris(hydroxymethyl)aminomethane=0.02:0.01:50; after the addition is completed, the solution is continued to be stirred for 1h, and then the solid and liquid are separated, the solid phase is washed with deionized water, and dried at 60°C for 80min to obtain the high thermal conductivity metal filler.
[0021] Example 2
[0022] A method for preparing a high thermal conductivity metal filler, comprising the steps of:
[0023] (1) preparing an aqueous solution of ethylene glycol and an aqueous solution of palladium nitrate; in the aqueous solution of ethylene glycol, the volume percentage of ethylene glycol is 20%, and the solvent is water; in the aqueous solution of palladium nitrate, the concentration of palladium nitrate is 7 g / L, and the solvent is water; keeping the aqueous solution of ethylene glycol constant at 60±3° C. in a water bath, stirring the aqueous solution of ethylene glycol, and simultaneously adding acetylacetone and n-butyl titanate to the solution under stirring, wherein the volume ratio of acetylacetone and n-butyl titanate added to the aqueous solution of ethylene glycol is ethylene glycol aqueous solution: acetylacetone: n-butyl titanate = 50:2:3; after the addition is completed, the mixed solution is stirred at a constant temperature of 60±3°C for 5 minutes, and after the stirring is completed, the pH of the mixed solution is adjusted to 3 with a nitric acid solution, and the concentration of the solute in the nitric acid solution is 2.5 mol / L; then the mixed solution is stirred at a constant temperature of 60±3°C, and the aqueous solution of palladium nitrate is added to the mixed solution under stirring, and the added volume ratio of the aqueous solution of palladium nitrate to the added volume of n-butyl titanate is the aqueous solution of palladium nitrate: n-butyl titanate = 2:3; after the addition is completed, the mixed solution is stirred at a constant temperature of 60±3°C for 30 minutes; a mixed solution A is obtained;
[0024] (2) dissolving polyvinyl pyrrolidone in deionized water kept at 80±5° C. to obtain a polyvinyl pyrrolidone solution; in the polyvinyl pyrrolidone solution, the concentration of polyvinyl pyrrolidone is 0.7 g / L; adding a silver nitrate solution to the polyvinyl pyrrolidone solution under the condition of keeping warm at 80±5° C., wherein the concentration of silver nitrate in the silver nitrate solution is 12 g / L, and the solvent is water; after the addition is completed, the solution is kept warm at 80±5° C. and stirred for 10 minutes, and then a sodium borohydride solution is added to the solution under stirring, wherein the concentration of sodium borohydride in the sodium borohydride solution is 3 g / L, and the solvent is water; after the addition is completed, The solution was stirred at 80±5°C for 10 minutes, and then a sodium sulfide solution was added to the solution under stirring, wherein the concentration of sodium sulfide in the sodium sulfide solution was 54 g / L, and the solvent was water; the volume ratio of the silver nitrate solution, the sodium borohydride solution, the sodium sulfide solution and the polyvinyl pyrrolidone solution was polyvinyl pyrrolidone solution: silver nitrate solution: sodium borohydride solution: sodium sulfide solution = 100:8:21:0.03; after the addition was completed, the solution was stirred at 80±5°C for 80 minutes, and then the solid-liquid separation was carried out, the solid phase was washed with deionized water, and dried at 80°C for 30 minutes to obtain sulfide nano silver powder;
[0025] (3) adding the sulfide nano-silver powder to an ethanol solution of polyvinyl pyrrolidone to form a suspension; the solid-liquid mass ratio of the sulfide nano-silver powder to the ethanol solution of polyvinyl pyrrolidone is sulfide nano-silver powder: ethanol solution of polyvinyl pyrrolidone = 1:200; wherein the concentration of polyvinyl pyrrolidone in the ethanol solution of polyvinyl pyrrolidone is 2 g / L, the suspension is kept at a constant temperature of 70±5° C. in a water bath, the suspension is stirred, and then the mixed solution A is added to the suspension under stirring; and the suspension is added to the mixed solution. The volume ratio of the mixed liquid A added to the suspension is suspension: mixed liquid A = 1:1; after the addition is completed, the mixture is stirred at a constant temperature of 70±5°C for 20 minutes; then an aqueous solution of hydrazine hydrate is added under stirring, wherein the mass percentage of hydrazine hydrate in the aqueous solution of hydrazine hydrate is 30%; the volume ratio of the added volume of the aqueous solution of hydrazine hydrate to the suspension is suspension: aqueous solution of hydrazine hydrate = 10:7; after the addition is completed, the mixture is stirred at a constant temperature of 70±5°C for 2 hours, and then the solid-liquid is separated, and the solid phase is calcined at 300°C in an argon atmosphere for 4 hours to obtain a solid phase B;
[0026] (4) preparing an aqueous solution of cysteamine hydrochloride; in the aqueous solution of cysteamine hydrochloride, the concentration of cysteamine hydrochloride is 10 g / L, and the solvent is water; adding the solid phase B into deionized water to form an aqueous suspension; the solid-liquid ratio of the solid phase B added into deionized water to form an aqueous suspension is solid phase B: deionized water = 1 g: 50 mL, stirring the aqueous suspension, and then adding the aqueous solution of cysteamine hydrochloride to the aqueous suspension under stirring; the volume ratio of the aqueous solution of cysteamine hydrochloride added into the aqueous suspension is aqueous suspension: aqueous solution of cysteamine hydrochloride = 10:1; stirring is continued for 3 hours after the addition is completed, and then solid-liquid separation is performed, the solid phase is dried at 60° C. for 40 minutes, and the dried solid phase is added to an aqueous solution of tris(hydroxymethyl)aminomethane. In the aqueous solution of tris(hydroxymethyl)aminomethane, the concentration of tris(hydroxymethyl)aminomethane is 7g / L, the solid-liquid mass ratio of the dried solid phase added to the aqueous solution of tris(hydroxymethyl)aminomethane is the dried solid phase: aqueous solution of tris(hydroxymethyl)aminomethane=1:50, the solution is stirred, and then tannic acid and copper chloride are added to the solution under stirring, and the mass ratio of tannic acid and copper chloride added to the solution to the aqueous solution of tris(hydroxymethyl)aminomethane is tannic acid: copper chloride: aqueous solution of tris(hydroxymethyl)aminomethane=0.02:0.01:50; after the addition is completed, the solution is continued to be stirred for 1h, and then the solid and liquid are separated, the solid phase is washed with deionized water, and dried at 60°C for 80min to obtain the high thermal conductivity metal filler.
[0027] Example 3
[0028] A method for preparing a high thermal conductivity metal filler, comprising the steps of:
[0029] (1) preparing an aqueous solution of ethylene glycol and an aqueous solution of palladium nitrate; in the aqueous solution of ethylene glycol, the volume percentage of ethylene glycol is 30%, and the solvent is water; in the aqueous solution of palladium nitrate, the concentration of palladium nitrate is 8 g / L, and the solvent is water; keeping the aqueous solution of ethylene glycol constant at 60±3° C. in a water bath, stirring the aqueous solution of ethylene glycol, and simultaneously adding acetylacetone and n-butyl titanate to the solution under stirring, wherein the volume ratio of acetylacetone and n-butyl titanate added to the aqueous solution of ethylene glycol is ethylene glycol aqueous solution: acetylacetone: n-butyl titanate = 50:2:4; after the addition is completed, the mixed solution is stirred at a constant temperature of 60±3°C for 5 minutes, and after the stirring is completed, the pH of the mixed solution is adjusted to 3 with a nitric acid solution, and the concentration of the solute in the nitric acid solution is 2.5 mol / L; then the mixed solution is stirred at a constant temperature of 60±3°C, and the aqueous solution of palladium nitrate is added to the mixed solution under stirring, and the added volume ratio of the aqueous solution of palladium nitrate to the added volume of n-butyl titanate is the aqueous solution of palladium nitrate: n-butyl titanate = 3:4; after the addition is completed, the mixed solution is stirred at a constant temperature of 60±3°C for 30 minutes; a mixed solution A is obtained;
[0030] (2) dissolving polyvinyl pyrrolidone in deionized water kept at 80±5° C. to obtain a polyvinyl pyrrolidone solution; in the polyvinyl pyrrolidone solution, the concentration of polyvinyl pyrrolidone is 0.7 g / L; adding a silver nitrate solution to the polyvinyl pyrrolidone solution under the condition of keeping warm at 80±5° C., wherein the concentration of silver nitrate is 14 g / L, and the solvent is water; after the addition is completed, the solution is kept warm at 80±5° C. and stirred for 10 minutes, and then a sodium borohydride solution is added to the solution under stirring, wherein the concentration of sodium borohydride is 4 g / L, and the solvent is water; after the addition is completed, The solution was stirred at 80±5°C for 10 minutes, and then a sodium sulfide solution was added to the solution under stirring, wherein the concentration of sodium sulfide in the sodium sulfide solution was 58 g / L, and the solvent was water; the volume ratio of the silver nitrate solution, the sodium borohydride solution, the sodium sulfide solution and the polyvinyl pyrrolidone solution was polyvinyl pyrrolidone solution: silver nitrate solution: sodium borohydride solution: sodium sulfide solution = 100:8:21:0.04; after the addition was completed, the solution was stirred at 80±5°C for 80 minutes, and then the solid-liquid separation was carried out, the solid phase was washed with deionized water, and dried at 80°C for 30 minutes to obtain sulfide nano silver powder;
[0031] (3) adding the sulfide nano-silver powder to an ethanol solution of polyvinyl pyrrolidone to form a suspension; the solid-liquid mass ratio of the sulfide nano-silver powder to the ethanol solution of polyvinyl pyrrolidone is sulfide nano-silver powder: ethanol solution of polyvinyl pyrrolidone = 1:200; wherein the concentration of polyvinyl pyrrolidone in the ethanol solution of polyvinyl pyrrolidone is 2 g / L, the suspension is kept at a constant temperature of 70±5° C. in a water bath, the suspension is stirred, and then the mixed solution A is added to the suspension under stirring; and the suspension is added to the mixed solution. The volume ratio of the mixed liquid A added to the suspension is suspension: mixed liquid A = 1:1; after the addition is completed, the mixture is stirred at a constant temperature of 70±5°C for 20 minutes; then an aqueous solution of hydrazine hydrate is added under stirring, wherein the mass percentage of hydrazine hydrate in the aqueous solution of hydrazine hydrate is 30%; the volume ratio of the added volume of the aqueous solution of hydrazine hydrate to the suspension is suspension: aqueous solution of hydrazine hydrate = 10:7; after the addition is completed, the mixture is stirred at a constant temperature of 70±5°C for 2 hours, and then the solid-liquid is separated, and the solid phase is calcined at 300°C in an argon atmosphere for 4 hours to obtain a solid phase B;
[0032] (4) preparing an aqueous solution of cysteamine hydrochloride; in the aqueous solution of cysteamine hydrochloride, the concentration of cysteamine hydrochloride is 10 g / L, and the solvent is water; adding the solid phase B into deionized water to form an aqueous suspension; the solid-liquid ratio of the solid phase B added into deionized water to form an aqueous suspension is solid phase B: deionized water = 1 g: 50 mL, stirring the aqueous suspension, and then adding the aqueous solution of cysteamine hydrochloride to the aqueous suspension under stirring; the volume ratio of the aqueous solution of cysteamine hydrochloride added into the aqueous suspension is aqueous suspension: aqueous solution of cysteamine hydrochloride = 10:1; stirring is continued for 3 hours after the addition is completed, and then solid-liquid separation is performed, the solid phase is dried at 60° C. for 40 minutes, and the dried solid phase is added to an aqueous solution of tris(hydroxymethyl)aminomethane. In the aqueous solution of tris(hydroxymethyl)aminomethane, the concentration of tris(hydroxymethyl)aminomethane is 7g / L, the solid-liquid mass ratio of the dried solid phase added to the aqueous solution of tris(hydroxymethyl)aminomethane is the dried solid phase: aqueous solution of tris(hydroxymethyl)aminomethane=1:50, the solution is stirred, and then tannic acid and copper chloride are added to the solution under stirring, and the mass ratio of tannic acid and copper chloride added to the solution to the aqueous solution of tris(hydroxymethyl)aminomethane is tannic acid: copper chloride: aqueous solution of tris(hydroxymethyl)aminomethane=0.03:0.01:50; after the addition is completed, the solution is continued to be stirred for 1h, and then the solid-liquid is separated, the solid phase is washed with deionized water, and dried at 60°C for 80min to obtain the high thermal conductivity metal filler.
[0033] Example 4
[0034] A method for preparing a high thermal conductivity metal filler, comprising the steps of:
[0035] (1) preparing an aqueous solution of ethylene glycol and an aqueous solution of palladium nitrate; in the aqueous solution of ethylene glycol, the volume percentage of ethylene glycol is 30%, and the solvent is water; in the aqueous solution of palladium nitrate, the concentration of palladium nitrate is 8 g / L, and the solvent is water; keeping the aqueous solution of ethylene glycol constant at 60±3° C. in a water bath, stirring the aqueous solution of ethylene glycol, and simultaneously adding acetylacetone and n-butyl titanate to the solution under stirring, wherein the volume ratio of acetylacetone and n-butyl titanate added to the aqueous solution of ethylene glycol is ethylene glycol aqueous solution: acetylacetone: n-butyl titanate = 50:2:4; after the addition is completed, the mixed solution is stirred at a constant temperature of 60±3°C for 5 minutes, and after the stirring is completed, the pH of the mixed solution is adjusted to 3 with a nitric acid solution, and the concentration of the solute in the nitric acid solution is 2.5 mol / L; then the mixed solution is stirred at a constant temperature of 60±3°C, and the aqueous solution of palladium nitrate is added to the mixed solution under stirring, and the added volume ratio of the aqueous solution of palladium nitrate to the added volume of n-butyl titanate is the aqueous solution of palladium nitrate: n-butyl titanate = 4:4; after the addition is completed, the mixed solution is stirred at a constant temperature of 60±3°C for 30 minutes; a mixed solution A is obtained;
[0036] (2) dissolving polyvinyl pyrrolidone in deionized water kept at 80±5° C. to obtain a polyvinyl pyrrolidone solution; in the polyvinyl pyrrolidone solution, the concentration of polyvinyl pyrrolidone is 0.8 g / L; adding a silver nitrate solution to the polyvinyl pyrrolidone solution under a keeping temperature of 80±5° C., wherein the concentration of silver nitrate is 15 g / L, and the solvent is water; after the addition is completed, the solution is kept at 80±5° C. and stirred for 10 minutes, and then a sodium borohydride solution is added to the solution under stirring, wherein the concentration of sodium borohydride is 4 g / L, and the solvent is water; after the addition is completed, The solution was stirred at 80±5°C for 10 minutes, and then a sodium sulfide solution was added to the solution under stirring, wherein the concentration of sodium sulfide in the sodium sulfide solution was 60 g / L, and the solvent was water; the volume ratio of the silver nitrate solution, the sodium borohydride solution, the sodium sulfide solution and the polyvinyl pyrrolidone solution was polyvinyl pyrrolidone solution: silver nitrate solution: sodium borohydride solution: sodium sulfide solution = 100:10:22:0.04; after the addition was completed, the solution was stirred at 80±5°C for 80 minutes, and then the solid-liquid separation was carried out, the solid phase was washed with deionized water, and dried at 80°C for 30 minutes to obtain sulfide nano silver powder;
[0037] (3) adding the sulfide nano-silver powder to an ethanol solution of polyvinyl pyrrolidone to form a suspension; the solid-liquid mass ratio of the sulfide nano-silver powder to the ethanol solution of polyvinyl pyrrolidone is sulfide nano-silver powder: ethanol solution of polyvinyl pyrrolidone = 1:200; wherein the concentration of polyvinyl pyrrolidone in the ethanol solution of polyvinyl pyrrolidone is 2 g / L, the suspension is kept at a constant temperature of 70±5° C. in a water bath, the suspension is stirred, and then the mixed solution A is added to the suspension under stirring; and the suspension is added to the mixed solution. The volume ratio of the mixed liquid A added to the suspension is suspension: mixed liquid A = 1:1; after the addition is completed, the mixture is stirred at a constant temperature of 70±5°C for 20 minutes; then an aqueous solution of hydrazine hydrate is added under stirring, wherein the mass percentage of hydrazine hydrate in the aqueous solution of hydrazine hydrate is 30%; the volume ratio of the added volume of the aqueous solution of hydrazine hydrate to the suspension is suspension: aqueous solution of hydrazine hydrate = 10:8; after the addition is completed, the mixture is stirred at a constant temperature of 70±5°C for 2 hours, and then the solid-liquid is separated, and the solid phase is calcined at 300°C in an argon atmosphere for 4 hours to obtain a solid phase B;
[0038] (4) preparing an aqueous solution of cysteamine hydrochloride; in the aqueous solution of cysteamine hydrochloride, the concentration of cysteamine hydrochloride is 10 g / L, and the solvent is water; adding the solid phase B into deionized water to form an aqueous suspension; the solid-liquid ratio of the solid phase B added into deionized water to form an aqueous suspension is solid phase B: deionized water = 1 g: 50 mL, stirring the aqueous suspension, and then adding the aqueous solution of cysteamine hydrochloride to the aqueous suspension under stirring; the volume ratio of the aqueous solution of cysteamine hydrochloride added into the aqueous suspension is aqueous suspension: aqueous solution of cysteamine hydrochloride = 10:1; stirring is continued for 3 hours after the addition is completed, and then solid-liquid separation is performed, the solid phase is dried at 60° C. for 40 minutes, and the dried solid phase is added to an aqueous solution of tris(hydroxymethyl)aminomethane. In the aqueous solution of tris(hydroxymethyl)aminomethane, the concentration of tris(hydroxymethyl)aminomethane is 8g / L, the solid-liquid mass ratio of the dried solid phase added to the aqueous solution of tris(hydroxymethyl)aminomethane is the dried solid phase: aqueous solution of tris(hydroxymethyl)aminomethane=1:50, the solution is stirred, and then tannic acid and copper chloride are added to the solution under stirring, and the mass ratio of tannic acid and copper chloride added to the solution to the aqueous solution of tris(hydroxymethyl)aminomethane is tannic acid: copper chloride: aqueous solution of tris(hydroxymethyl)aminomethane=0.03:0.01:50; after the addition is completed, the solution is continued to be stirred for 1h, and then the solid and liquid are separated, the solid phase is washed with deionized water, and dried at 60°C for 80min to obtain the high thermal conductivity metal filler.
[0039] Comparative Example 1
[0040] A comparative filler preparation method comprises the following steps:
[0041] (1) preparing an aqueous solution of ethylene glycol; in the aqueous solution of ethylene glycol, the volume percentage of ethylene glycol is 20%, and the solvent is water; keeping the aqueous solution of ethylene glycol constant temperature at 60±3° C. in a water bath, stirring the aqueous solution of ethylene glycol, and adding acetylacetone and n-butyl titanate to the solution under stirring, wherein the volume ratio of acetylacetone and n-butyl titanate added to the aqueous solution of ethylene glycol is ethylene glycol aqueous solution: acetylacetone: n-butyl titanate = 50:2:3; after the addition is completed, stirring the mixed solution at a constant temperature of 60±3° C. for 5 minutes, and after the stirring is completed, adjusting the pH of the mixed solution to 3 with a nitric acid solution, wherein the concentration of the solute in the nitric acid solution is 2.5 mol / L; then stirring the mixed solution at a constant temperature of 60±3° C. for 30 minutes; obtaining a mixed solution A;
[0042] (2) dissolving polyvinyl pyrrolidone in deionized water kept at 80±5° C. to obtain a polyvinyl pyrrolidone solution; in the polyvinyl pyrrolidone solution, the concentration of polyvinyl pyrrolidone is 0.7 g / L; adding a silver nitrate solution to the polyvinyl pyrrolidone solution under the condition of keeping warm at 80±5° C., wherein the concentration of silver nitrate in the silver nitrate solution is 12 g / L, and the solvent is water; after the addition is completed, the solution is kept warm at 80±5° C. and stirred for 10 minutes, and then a sodium borohydride solution is added to the solution under stirring, wherein the concentration of sodium borohydride in the sodium borohydride solution is 3 g / L, and the solvent is water; after the addition is completed, The solution was stirred at 80±5°C for 10 minutes, and then a sodium sulfide solution was added to the solution under stirring, wherein the concentration of sodium sulfide in the sodium sulfide solution was 54 g / L, and the solvent was water; the volume ratio of the silver nitrate solution, the sodium borohydride solution, the sodium sulfide solution and the polyvinyl pyrrolidone solution was polyvinyl pyrrolidone solution: silver nitrate solution: sodium borohydride solution: sodium sulfide solution = 100:8:21:0.03; after the addition was completed, the solution was stirred at 80±5°C for 80 minutes, and then the solid-liquid separation was carried out, the solid phase was washed with deionized water, and dried at 80°C for 30 minutes to obtain sulfide nano silver powder;
[0043] (3) adding the sulfide nano-silver powder to an ethanol solution of polyvinyl pyrrolidone to form a suspension; the solid-liquid mass ratio of the sulfide nano-silver powder to the ethanol solution of polyvinyl pyrrolidone is sulfide nano-silver powder: ethanol solution of polyvinyl pyrrolidone = 1:200; wherein the concentration of polyvinyl pyrrolidone in the ethanol solution of polyvinyl pyrrolidone is 2 g / L, the suspension is kept at a constant temperature of 70±5° C. in a water bath, the suspension is stirred, and then the mixed solution A is added to the suspension under stirring; and the suspension is added to the mixed solution. The volume ratio of the mixed liquid A added to the suspension is suspension: mixed liquid A = 1:1; after the addition is completed, the mixture is stirred at a constant temperature of 70±5°C for 20 minutes; then an aqueous solution of hydrazine hydrate is added under stirring, wherein the mass percentage of hydrazine hydrate in the aqueous solution of hydrazine hydrate is 30%; the volume ratio of the added volume of the aqueous solution of hydrazine hydrate to the suspension is suspension: aqueous solution of hydrazine hydrate = 10:7; after the addition is completed, the mixture is stirred at a constant temperature of 70±5°C for 2 hours, and then the solid-liquid is separated, and the solid phase is calcined at 300°C in an argon atmosphere for 4 hours to obtain a solid phase B;
[0044] (4) preparing an aqueous solution of cysteamine hydrochloride; in the aqueous solution of cysteamine hydrochloride, the concentration of cysteamine hydrochloride is 10 g / L, and the solvent is water; adding the solid phase B into deionized water to form an aqueous suspension; the solid-liquid ratio of the solid phase B added into deionized water to form an aqueous suspension is solid phase B: deionized water = 1 g: 50 mL, stirring the aqueous suspension, and then adding the aqueous solution of cysteamine hydrochloride to the aqueous suspension under stirring; the volume ratio of the aqueous solution of cysteamine hydrochloride added into the aqueous suspension is aqueous suspension: aqueous solution of cysteamine hydrochloride = 10:1; stirring is continued for 3 hours after the addition is completed, and then solid-liquid separation is performed, the solid phase is dried at 60° C. for 40 minutes, and the dried solid phase is added to an aqueous solution of tris(hydroxymethyl)aminomethane. In the aqueous solution of tris(hydroxymethyl)aminomethane, the concentration of tris(hydroxymethyl)aminomethane is 7g / L, the solid-liquid mass ratio of the dried solid phase added to the aqueous solution of tris(hydroxymethyl)aminomethane is the dried solid phase: aqueous solution of tris(hydroxymethyl)aminomethane=1:50, the solution is stirred, and then tannic acid and copper chloride are added to the solution under stirring, and the mass ratio of tannic acid and copper chloride added to the solution to the aqueous solution of tris(hydroxymethyl)aminomethane is tannic acid: copper chloride: aqueous solution of tris(hydroxymethyl)aminomethane=0.02:0.01:50; after the addition is completed, the solution is continued to be stirred for 1h, and then the solid-liquid is separated, the solid phase is washed with deionized water, and dried at 60°C for 80min to obtain the filler described in this comparative example.
[0045] Comparative Example 2
[0046] A comparative filler preparation method comprises the following steps:
[0047] (1) preparing an aqueous solution of ethylene glycol and an aqueous solution of palladium nitrate; in the aqueous solution of ethylene glycol, the volume percentage of ethylene glycol is 20%, and the solvent is water; in the aqueous solution of palladium nitrate, the concentration of palladium nitrate is 7 g / L, and the solvent is water; keeping the aqueous solution of ethylene glycol constant at 60±3° C. in a water bath, stirring the aqueous solution of ethylene glycol, and simultaneously adding acetylacetone and n-butyl titanate to the solution under stirring, wherein the volume ratio of acetylacetone and n-butyl titanate added to the aqueous solution of ethylene glycol is ethylene glycol aqueous solution: acetylacetone: n-butyl titanate = 50:2:3; after the addition is completed, the mixed solution is stirred at a constant temperature of 60±3°C for 5 minutes, and after the stirring is completed, the pH of the mixed solution is adjusted to 3 with a nitric acid solution, and the concentration of the solute in the nitric acid solution is 2.5 mol / L; then the mixed solution is stirred at a constant temperature of 60±3°C, and the aqueous solution of palladium nitrate is added to the mixed solution under stirring, and the added volume ratio of the aqueous solution of palladium nitrate to the added volume of n-butyl titanate is the aqueous solution of palladium nitrate: n-butyl titanate = 2:3; after the addition is completed, the mixed solution is stirred at a constant temperature of 60±3°C for 30 minutes; a mixed solution A is obtained;
[0048] (2) dissolving polyvinyl pyrrolidone in deionized water kept at 80±5°C to obtain a polyvinyl pyrrolidone solution; in the polyvinyl pyrrolidone solution, the concentration of polyvinyl pyrrolidone is 0.7 g / L; adding a silver nitrate solution to the polyvinyl pyrrolidone solution under the condition of keeping at 80±5°C, wherein the concentration of silver nitrate in the silver nitrate solution is 12 g / L, and the solvent is water; after the addition is completed, the solution is kept at 80±5°C and stirred for 10 minutes, and then a sodium borohydride solution is added to the solution under stirring, wherein the concentration of sodium borohydride in the sodium borohydride solution is 3 g / L, and the solvent is water; after the addition is completed, the solution is kept at 80±5°C and stirred for 90 minutes, and the volume ratio of the silver nitrate solution, the sodium borohydride solution and the polyvinyl pyrrolidone solution is polyvinyl pyrrolidone solution: silver nitrate solution: sodium borohydride solution = 100:8:21; solid-liquid separation, the solid phase is washed with deionized water, and dried at 80°C for 30 minutes to obtain the nano silver powder of this comparative example;
[0049] (3) adding the nano silver powder to an ethanol solution of polyvinyl pyrrolidone to form a suspension; the solid-liquid mass ratio of the nano silver powder to the ethanol solution of polyvinyl pyrrolidone is nano silver powder: ethanol solution of polyvinyl pyrrolidone = 1:200; wherein the concentration of polyvinyl pyrrolidone in the ethanol solution of polyvinyl pyrrolidone is 2 g / L, the suspension is kept at a constant temperature of 70±5° C. in a water bath, the suspension is stirred, and then the mixed solution A is added to the suspension under stirring; and the suspension is added The volume ratio of the mixed liquid A is suspension: mixed liquid A=1:1; after the addition is completed, the mixture is stirred at a constant temperature of 70±5°C for 20 minutes; then, an aqueous solution of hydrazine hydrate is added under stirring, and the mass percentage of hydrazine hydrate in the aqueous solution of hydrazine hydrate is 30%; the volume ratio of the added volume of the aqueous solution of hydrazine hydrate to the suspension is suspension: aqueous solution of hydrazine hydrate=10:7; after the addition is completed, the mixture is stirred at a constant temperature of 70±5°C for 2 hours, and then the solid-liquid is separated, and the solid phase is calcined at 300°C in an argon atmosphere for 4 hours to obtain a solid phase B;
[0050] (4) preparing an aqueous solution of cysteamine hydrochloride; in the aqueous solution of cysteamine hydrochloride, the concentration of cysteamine hydrochloride is 10 g / L, and the solvent is water; adding the solid phase B into deionized water to form an aqueous suspension; the solid-liquid ratio of the solid phase B added into deionized water to form an aqueous suspension is solid phase B: deionized water = 1 g: 50 mL, stirring the aqueous suspension, and then adding the aqueous solution of cysteamine hydrochloride to the aqueous suspension under stirring; the volume ratio of the aqueous solution of cysteamine hydrochloride added into the aqueous suspension is aqueous suspension: aqueous solution of cysteamine hydrochloride = 10:1; stirring is continued for 3 hours after the addition is completed, and then solid-liquid separation is performed, the solid phase is dried at 60° C. for 40 minutes, and the dried solid phase is added to an aqueous solution of tris(hydroxymethyl)aminomethane. In the aqueous solution of tris(hydroxymethyl)aminomethane, the concentration of tris(hydroxymethyl)aminomethane is 7g / L, the solid-liquid mass ratio of the dried solid phase added to the aqueous solution of tris(hydroxymethyl)aminomethane is the dried solid phase: aqueous solution of tris(hydroxymethyl)aminomethane=1:50, the solution is stirred, and then tannic acid and copper chloride are added to the solution under stirring, and the mass ratio of tannic acid and copper chloride added to the solution to the aqueous solution of tris(hydroxymethyl)aminomethane is tannic acid: copper chloride: aqueous solution of tris(hydroxymethyl)aminomethane=0.02:0.01:50; after the addition is completed, the solution is continued to be stirred for 1h, and then the solid-liquid is separated, the solid phase is washed with deionized water, and dried at 60°C for 80min to obtain the filler described in this comparative example.
[0051] Comparative Example 3
[0052] A comparative filler preparation method comprises the following steps:
[0053] (1) preparing an aqueous solution of ethylene glycol and an aqueous solution of palladium nitrate; in the aqueous solution of ethylene glycol, the volume percentage of ethylene glycol is 20%, and the solvent is water; in the aqueous solution of palladium nitrate, the concentration of palladium nitrate is 7 g / L, and the solvent is water; keeping the aqueous solution of ethylene glycol constant at 60±3° C. in a water bath, stirring the aqueous solution of ethylene glycol, and simultaneously adding acetylacetone and n-butyl titanate to the solution under stirring, wherein the volume ratio of acetylacetone and n-butyl titanate added to the aqueous solution of ethylene glycol is ethylene glycol aqueous solution: acetylacetone: n-butyl titanate = 50:2:3; after the addition is completed, the mixed solution is stirred at a constant temperature of 60±3°C for 5 minutes, and after the stirring is completed, the pH of the mixed solution is adjusted to 3 with a nitric acid solution, and the concentration of the solute in the nitric acid solution is 2.5 mol / L; then the mixed solution is stirred at a constant temperature of 60±3°C, and the aqueous solution of palladium nitrate is added to the mixed solution under stirring, and the added volume ratio of the aqueous solution of palladium nitrate to the added volume of n-butyl titanate is the aqueous solution of palladium nitrate: n-butyl titanate = 2:3; after the addition is completed, the mixed solution is stirred at a constant temperature of 60±3°C for 30 minutes; a mixed solution A is obtained;
[0054] (2) dissolving polyvinyl pyrrolidone in deionized water kept at 80±5° C. to obtain a polyvinyl pyrrolidone solution; in the polyvinyl pyrrolidone solution, the concentration of polyvinyl pyrrolidone is 0.7 g / L; adding a silver nitrate solution to the polyvinyl pyrrolidone solution under the condition of keeping warm at 80±5° C., wherein the concentration of silver nitrate in the silver nitrate solution is 12 g / L, and the solvent is water; after the addition is completed, the solution is kept warm at 80±5° C. and stirred for 10 minutes, and then a sodium borohydride solution is added to the solution under stirring, wherein the concentration of sodium borohydride in the sodium borohydride solution is 3 g / L, and the solvent is water; after the addition is completed, The solution was stirred at 80±5°C for 10 minutes, and then a sodium sulfide solution was added to the solution under stirring, wherein the concentration of sodium sulfide in the sodium sulfide solution was 54 g / L, and the solvent was water; the volume ratio of the silver nitrate solution, the sodium borohydride solution, the sodium sulfide solution and the polyvinyl pyrrolidone solution was polyvinyl pyrrolidone solution: silver nitrate solution: sodium borohydride solution: sodium sulfide solution = 100:8:21:0.03; after the addition was completed, the solution was stirred at 80±5°C for 80 minutes, and then the solid-liquid separation was carried out, the solid phase was washed with deionized water, and dried at 80°C for 30 minutes to obtain sulfide nano silver powder;
[0055] (3) adding the sulfide nano-silver powder to an ethanol solution of polyvinyl pyrrolidone to form a suspension; the solid-liquid mass ratio of the sulfide nano-silver powder to the ethanol solution of polyvinyl pyrrolidone is sulfide nano-silver powder: ethanol solution of polyvinyl pyrrolidone = 1:200; wherein the concentration of polyvinyl pyrrolidone in the ethanol solution of polyvinyl pyrrolidone is 2 g / L, the suspension is kept at a constant temperature of 70±5° C. in a water bath, the suspension is stirred, and then the mixed solution A is added to the suspension under stirring; and the suspension is added to the mixed solution. The volume ratio of the mixed liquid A added to the suspension is suspension: mixed liquid A = 1:1; after the addition is completed, the mixture is stirred at a constant temperature of 70±5°C for 20 minutes; then an aqueous solution of hydrazine hydrate is added under stirring, wherein the mass percentage of hydrazine hydrate in the aqueous solution of hydrazine hydrate is 30%; the volume ratio of the added volume of the aqueous solution of hydrazine hydrate to the suspension is suspension: aqueous solution of hydrazine hydrate = 10:7; after the addition is completed, the mixture is stirred at a constant temperature of 70±5°C for 2 hours, and then the solid-liquid is separated, and the solid phase is calcined at 300°C in an argon atmosphere for 4 hours to obtain a solid phase B;
[0056] (4) preparing an aqueous solution of cysteamine hydrochloride; in the aqueous solution of cysteamine hydrochloride, the concentration of cysteamine hydrochloride is 10 g / L, and the solvent is water; adding the solid phase B to deionized water to form an aqueous suspension; the solid-liquid ratio of the solid phase B added to deionized water to form an aqueous suspension is solid phase B: deionized water = 1 g: 50 mL, stirring the aqueous suspension, and then adding the aqueous solution of cysteamine hydrochloride to the aqueous suspension under stirring; adding the aqueous solution of cysteamine hydrochloride to the aqueous suspension in a volume ratio of aqueous suspension: aqueous solution of cysteamine hydrochloride = 10:1; after the addition is completed, stirring is continued for 3 hours, and then the solid and liquid are separated, the solid phase is washed with deionized water, and dried at 60° C. for 80 minutes to obtain the filler described in this comparative example.
[0057] Example 5
[0058] The test glue was prepared by using the fillers prepared by the methods described in the above embodiments and comparative examples. The preparation method of the test glue is as follows: bisphenol F170 epoxy resin, dicyandiamide curing agent, organic urea curing accelerator, KH560 coupling agent, and adipic acid are mixed evenly to form a resin matrix, and the raw materials of the resin matrix are calculated by weight as 100 parts of bisphenol F170 epoxy resin, 6 parts of dicyandiamide curing agent, 0.3 parts of organic urea curing accelerator, 1.2 parts of KH560 coupling agent, and 3 parts of adipic acid. Then the filler is added to the resin matrix and mixed evenly, and the mixing mass ratio is filler: resin matrix = 7.5:2.5; after mixing, degassing treatment is performed, and then injected into a cylinder, cured at 150°C for 2h, and after cooling, it is polished into a disc sample with a thickness of 3mm and a diameter of 60mm. The thermal conductivity of the disc sample in the thickness direction is tested, and the results are shown in Table 1.
[0059] Table 1
[0060]
[0061]
[0062] As can be seen from Table 1, after the filler prepared by the method of the present invention is added to the resin matrix, a glue material with good thermal conductivity and high thermal conductivity can be obtained. This is mainly because on the one hand, the thermal resistance of the filler is reduced by improving the process of the filler itself and reducing the amount of silver in the filler. On the other hand, the interface bonding between the filler and the resin matrix is promoted, the contact thermal resistance between the filler and the resin is reduced, and the thermal conductivity of the material is improved as a whole.
[0063] The technical solution provided by the present invention is introduced in detail above. For those skilled in the art, according to the concept of the embodiments of the present invention, there may be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for preparing a high thermal conductivity metal filler, characterized in that the steps include: (1) preparing an aqueous solution of ethylene glycol and an aqueous solution of palladium nitrate; keeping the aqueous solution of ethylene glycol constant at 60±3° C. in a water bath, stirring the aqueous solution of ethylene glycol, adding acetylacetone and n-butyl titanate to the solution while stirring, stirring the mixed solution at 60±3° C. for 5 to 8 minutes after the addition is completed, adjusting the pH of the mixed solution to 3 with a nitric acid solution after the stirring is completed; then stirring the mixed solution at 60±3° C., adding the aqueous solution of palladium nitrate to the mixed solution while stirring, and continuing to stir the mixed solution at 60±3° C. for 20 to 30 minutes after the addition is completed; obtaining a mixed solution A; (2) dissolving polyvinyl pyrrolidone in deionized water kept at 80±5° C. to obtain a polyvinyl pyrrolidone solution; adding a silver nitrate solution to the polyvinyl pyrrolidone solution under a heat preservation condition of 80±5° C., and stirring the solution at 80±5° C. for 10 to 15 minutes after the addition is completed, and then adding a sodium borohydride solution to the solution under stirring, and stirring the solution at 80±5° C. for 10 minutes after the addition is completed, and then adding a sodium sulfide solution to the solution under stirring, and stirring the solution at 80±5° C. for 80 to 100 minutes after the addition is completed, and then separating the solid and liquid, washing the solid phase with deionized water, and drying at 80° C. for more than 30 minutes to obtain sulfide nano silver powder; (3) adding the sulfide nanosilver powder to an ethanol solution of polyvinyl pyrrolidone to form a suspension; keeping the suspension constant temperature at 70±5° C. in a water bath, stirring the suspension, and then adding the mixed solution A to the suspension under stirring; continuing to stir at 70±5° C. for 10 to 20 min after the addition is completed; then adding an aqueous solution of hydrazine hydrate under stirring, stirring at 70±5° C. for more than 2 h after the addition is completed, then separating the solid from the liquid, and calcining the solid phase at 300° C. in an argon atmosphere for 4 h to obtain a solid phase B; (4) preparing an aqueous solution of cysteamine hydrochloride; adding the solid phase B to deionized water to form an aqueous suspension; stirring the aqueous suspension, and then adding the aqueous solution of cysteamine hydrochloride to the aqueous suspension under stirring; continuing to stir for more than 3 hours after the addition is completed, and then separating the solid and liquid, drying the solid phase at 60° C. for more than 40 minutes, adding the dried solid phase to an aqueous solution of tris(hydroxymethyl)aminomethane, stirring the solution, and then adding tannic acid and copper chloride to the solution under stirring, continuing to stir the solution for more than 1 hour after the addition is completed, and then separating the solid and liquid, washing the solid phase with deionized water, and drying at 60° C. for more than 80 minutes to obtain the high thermal conductivity metal filler.
2. The method for preparing a high thermal conductivity metal filler according to claim 1, characterized in that: In the step (1), in the aqueous solution of ethylene glycol, the volume percentage of ethylene glycol is 20% to 30%, and the solvent is water; in the aqueous solution of palladium nitrate, the concentration of palladium nitrate is 7 to 8 g / L, and the solvent is water; acetylacetone and n-butyl titanate are added to the aqueous solution of ethylene glycol at the same time in a volume ratio of ethylene glycol aqueous solution: acetylacetone: n-butyl titanate = 50:2:3 to 4; the concentration of the solute in the nitric acid solution is 2.5 mol / L; the ratio of the added volume of the aqueous solution of palladium nitrate to the added volume of n-butyl titanate is palladium nitrate aqueous solution: n-butyl titanate = 1 to 4:3 to 4.
3. The method for preparing a high thermal conductivity metal filler according to claim 1, characterized in that: In the step (2), in the polyvinyl pyrrolidone solution, the concentration of polyvinyl pyrrolidone is 0.6-0.8 g / L, in the silver nitrate solution, the concentration of silver nitrate is 10-15 g / L, and the solvent is water; in the sodium borohydride solution, the concentration of sodium borohydride is 3-4 g / L, and the solvent is water; in the sodium sulfide solution, the concentration of sodium sulfide is 50-60 g / L, and the solvent is water; the volume ratio of the silver nitrate solution, the sodium borohydride solution, the sodium sulfide solution and the polyvinyl pyrrolidone solution is polyvinyl pyrrolidone solution: silver nitrate solution: sodium borohydride solution: sodium sulfide solution = 100:6-10:20-22:0.03-0.
04.
4. The method for preparing a high thermal conductivity metal filler according to claim 1, characterized in that: In the step (3), the solid-liquid mass ratio of the sulfide nano-silver powder added to the ethanol solution of polyvinyl pyrrolidone is sulfide nano-silver powder: ethanol solution of polyvinyl pyrrolidone = 1:200; the concentration of polyvinyl pyrrolidone in the ethanol solution of polyvinyl pyrrolidone is 2 g / L, the volume ratio of the mixed solution A added to the suspension is suspension: mixed solution A = 1:1; the mass percentage of hydrazine hydrate in the aqueous solution of hydrazine hydrate is 30%; the volume ratio of the added volume of the aqueous solution of hydrazine hydrate to the suspension is suspension: aqueous solution of hydrazine hydrate = 10:6-8.
5. The method for preparing a high thermal conductivity metal filler according to claim 1, characterized in that: In the step (4), the concentration of cysteamine hydrochloride in the aqueous solution of cysteamine hydrochloride is 10 g / L, and the solvent is water; the solid-liquid ratio of the solid phase B added to deionized water to form an aqueous suspension is solid phase B: deionized water = 1 g: 50 mL, and the volume ratio of the aqueous solution of cysteamine hydrochloride added to the aqueous suspension is aqueous suspension: aqueous solution of cysteamine hydrochloride = 10:
1.
6. The method for preparing a high thermal conductivity metal filler according to claim 1, characterized in that: In the step (4), the concentration of tris(hydroxymethyl)aminomethane in the aqueous solution of tris(hydroxymethyl)aminomethane is 6-8 g / L, the solid-liquid mass ratio of the dried solid phase added to the aqueous solution of tris(hydroxymethyl)aminomethane is the dried solid phase: aqueous solution of tris(hydroxymethyl)aminomethane = 1:50, and the mass ratio of tannic acid and cupric chloride added to the solution to the aqueous solution of tris(hydroxymethyl)aminomethane is tannic acid: cupric chloride: aqueous solution of tris(hydroxymethyl)aminomethane = 0.02-0.03:0.01:50.