A Y element improves Cu-Ti 2 Preparation method and application of SnC composite material interface and performance
By adding Y elements to the Cu-Ti2SnC composite material, and using wet dispersion and plasma sintering processes, the YSn3 and CuY mesophases are generated, which solves the problem of poor decomposition and wettability of Ti2SnC, which significantly improves the wear resistance and mechanical properties of the material. , meet the performance requirements of electrical contact materials in high-tech fields.
Patent Information
- Application Number
- CN202410157041.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-04
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-02-04
AI Technical Summary
The Cu-Ti2SnC composite material is easy to decompose during high-temperature sintering, resulting in reduced conductivity and mechanical properties. The low sintering temperature is insufficient density and poor wettability, making it difficult to meet the reliability and performance requirements of electrical contact materials in the high-tech field.
The preparation method of Y element to improve Cu-Ti2SnC composite material is used to improve the preparation method, and through wet dispersion, drying, ball milling, stress removal annealing and discharge plasma sintering processes, the YSn3 and CuY mesophases are generated, the interface and performance are improved, the decomposition of Ti2SnC is suppressed, and the resistance is improved. Abrasive and mechanical properties.
It significantly improves the strength, hardness, wetting and oxidation resistance of Cu-Ti2SnC composite materials, maintains excellent conductivity, meets the needs of high-frequency and high-current circuits, and is also used in applications such as resistance welding electrodes, motor rectifiers, and relays. Show good service status.
Smart Images

Figure CN118147483B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of copper-based wear-resistant materials, and specifically relates to a preparation method and application of Y element to improve the interface and performance of Cu-Ti2SnC composite material. Background Art
[0002] Electrical contact materials are key functional materials in electrical appliances that are responsible for connecting, disconnecting, carrying and isolating currents. They are widely used in many fields, mainly including electrical components, electronic components, power equipment, etc. These materials are mainly used to manufacture switches, relays, circuit breakers, motor commutators and other electrical appliances and power equipment. The performance of these materials directly affects the safety, reliability and life of the operation of electrical appliances. In recent years, high-tech fields such as energy, rail transit, aerospace, etc. have developed rapidly. In the automotive industry, with the development of electric vehicles and intelligent networked vehicles, electrical contact materials are widely used in the manufacture of contacts and connections of automotive electronic components such as automobile starters, generators, regulators, etc., and the demand for electrical components and power equipment has increased significantly; in energy and power systems, electrical contact materials are widely used in power generation, transmission and distribution systems, such as electrical contact materials used in contacts and connections of key equipment such as high-voltage switchgear and transformers; in the field of rail transit, electrical contact materials are used to manufacture key components such as pantographs and electrical connectors of rail transit vehicles such as subways, light rails and high-speed railways; in the field of industrial automation, electrical contact materials can be used to manufacture joint sensors and controllers of robots to improve the movement accuracy and stability of robots; in the field of aerospace, for example, in the control systems and communication systems of aircraft and satellites, electrical contact materials are used to manufacture various sensors, controllers and actuators and other components; the development of the above rail transit, aerospace, industrial automation and other fields has put forward higher requirements on the reliability, conductivity and mechanical properties of electrical contact materials.
[0003] MAX phase is a new type of ternary layered ceramic material with the chemical formula M n + 1 AX n,n = 1, 2, 3, MAX phase materials combine the advantages of metals and ceramics, and have good thermal conductivity, electrical conductivity and thermal shock resistance. It can maintain plasticity at high temperatures and can be processed like metals and graphite. In addition, it also has high yield strength, high melting point, high thermal stability and excellent oxidation resistance and corrosion resistance. In particular, MAX phase materials also have excellent wear resistance and self-lubrication. Ti2SnC is one of the most outstanding materials in the MAX phase. It has a high melting point, hardness, excellent electrical conductivity and thermal conductivity, as well as excellent corrosion resistance and high temperature stability in high temperature and corrosive environments. It can be used to manufacture electronic devices, heat sink materials, high temperature structural materials, corrosion-resistant materials, wear-resistant materials and other electrical contact materials. It is an advanced material with broad application prospects, and its preparation and application research are of great significance. The process of preparing copper-based composites by adding Ti2SnC reinforcement phase to Cu matrix still faces some difficulties. On the one hand, when the composite powder is sintered at 800 ℃ and above, Ti2SnC will decompose, and Cu and Ti2SnC will diffuse with each other at the interface, which will lead to problems such as reduced conductivity and mechanical properties. On the other hand, lower sintering temperature will lead to problems such as reduced density of the material, insufficient mechanical properties, and poor wettability of Cu and Ti2SnC. Therefore, it is of great significance to explore a Cu-Ti2SnC composite material with trace elements to improve the interface and performance and its application. Summary of the invention
[0004] The purpose of the present invention is to provide a preparation method and application of Y element to improve the interface and performance of Cu-Ti2SnC composite material in view of the shortcomings of existing process technology. The mechanical properties of the prepared Cu-Ti2SnC-Y electrical contact material are significantly improved, the interface wettability and wear resistance are improved, and the service condition is excellent.
[0005] In order to achieve the above purpose, the present invention adopts the following technical solutions:
[0006] A preparation method for improving the interface and performance of a Cu-Ti2SnC composite material by Y element, specifically comprising the following steps:
[0007] Cu powder, Ti2SnC powder and Y powder are sequentially loaded into a beaker containing an appropriate amount of anhydrous ethanol, and the beaker is then placed in a magnetic stirrer for heating and stirring. After the mixed powder is evenly stirred, the beaker is placed in a drying oven and taken out for grinding after being completely air-dried; the ground powder is loaded into a ball mill under an argon atmosphere and ball-milled; the ball-milled powder is placed in a tubular furnace and stress-relief annealed under a hydrogen atmosphere to obtain a Cu-Ti2SnC-Y composite powder after grinding; finally, the obtained Cu-Ti2SnC-Y composite powder is loaded into a graphite mold for spark plasma sintering to obtain a Cu-Ti2SnC composite material modified with the Y element.
[0008] Preferably, the Cu powder is high-purity electrolytic Cu powder, in the shape of grape bunches, with a purity of 99.999% and a particle size of 1 to 3 microns; the Ti2SnC powder is a high-purity multilayer flaky ceramic powder with a particle size of 600 to 800 meshes; the Y powder has a purity of 99.99% and a particle size of 0.5 to 2 microns;
[0009] Preferably, the addition amounts of the Cu powder, Ti2SnC powder and Y powder are calculated according to mass fraction, wherein the addition amount of the Ti2SnC powder is 0.9-1.2 wt%, the addition amount of the Y powder is 0-0.3 wt%, and the balance is Cu powder.
[0010] Preferably, the stirring temperature of the magnetic stirrer is set at 25-35° C., the stirring time is set at 6-8 hours, and in addition to an appropriate amount of anhydrous ethanol, sodium dodecylbenzoate is added to the beaker as a dispersant to promote more uniform dispersion of the powder.
[0011] Preferably, the amount of anhydrous ethanol added to the beaker is determined according to the amounts of Cu powder, Ti2SnC powder and Y powder added, and the amount of dispersant sodium dodecylbenzoate added is determined according to the dispersion of the mixed powder.
[0012] Preferably, after the mixed powder is stirred evenly, it is repeatedly rinsed with anhydrous ethanol, and after being rinsed clean, it is placed in a blast drying oven for drying, and the temperature of the blast drying oven is set at 20-30°C.
[0013] Preferably, the ground powder is sieved through a 800-1000 mesh sieve and then placed in a ball mill in a vacuum glove box under an argon atmosphere at a ball milling speed of 400-450 r / min for 16-18 hours.
[0014] Preferably, the amount of hydrogen introduced into the tube furnace is 300-350 ml / min, the temperature for stress relief annealing is 300-400° C., and the time for stress relief annealing is 1-3 hours.
[0015] Preferably, the ball-milled powder is subjected to stress relief annealing and grinding and then sieved through a 800-1000 mesh sieve to obtain a Cu-Ti2SnC-Y composite powder.
[0016] Preferably, the graphite mold has an inner diameter of ∅20 mm, an outer diameter of ∅60 mm, and a height of 70 mm.
[0017] Preferably, the spark plasma sintering process is to first increase the temperature from room temperature to 500-600 ° C and keep it for 5-10 minutes, then continue to increase the temperature to 850-950 ° C, keep it for 10-15 minutes, the heating rate is 80-100 ° C / min, the pre-pressing pressure is 30 MPa, and the pressure is increased to 50 MPa during the second heating process. Finally, after cooling with the furnace, a Cu-Ti2SnC composite material with improved performance of the Y element is obtained.
[0018] Preferably, the Cu-Ti2SnC-Y electrical contact material prepared according to a preparation method for improving the interface and performance of a Cu-Ti2SnC composite material with a Y element is used in resistance welding electrodes, motor commutators, relays, and vacuum switch electrical contacts.
[0019] The innovation of the present invention is embodied in:
[0020] Material design: Through the specific proportion design of the three components of Cu powder, Ti2SnC reinforcement phase and Y powder, the excellent self-lubrication, electrical conductivity and thermal conductivity of the Ti2SnC reinforcement phase, as well as the excellent corrosion resistance and high temperature stability under high temperature and corrosive environment, and the improvement of the Cu-Ti2SnC interface and performance by the Y element, the characteristics of high conductivity, high wear resistance and excellent mechanical properties are achieved.
[0021] Preparation method: The preparation method of the present invention is composed of wet dispersion, drying, ball milling, stress relief annealing and spark plasma sintering processes, so that the material has a specific crystal structure and phase composition, thereby improving the performance of the material. The preparation method provides the possibility for large-scale production of this high-performance electrical contact material.
[0022] Performance optimization: The Cu-Ti2SnC composite material is improved by adding Y element, which further improves the strength, wear resistance and oxidation resistance, maintains excellent conductivity, effectively inhibits the decomposition of Ti2SnC, improves stability, and exhibits excellent overall performance.
[0023] Compared with the existing process technology, the preparation method of the Y element for improving the interface and performance of the Cu-Ti2SnC composite material and the prepared Cu-Ti2SnC-Y electrical contact material of the present invention have at least the following beneficial effects:
[0024] The preparation method of improving the interface and performance of Cu-Ti2SnC composite material by Y element of the present invention is composed of wet dispersion, drying, ball milling, stress relief annealing and discharge plasma sintering process. The addition of trace Y element not only improves the interface of Cu-Ti2SnC, generates YSn3 and CuY intermediate phase at the interface, significantly improves the strength, hardness, wettability and oxidation resistance of the material, and effectively inhibits the decomposition of Ti2SnC, maintains the self-lubricating structure of Ti2SnC, improves the wear resistance and mechanical properties of the material, and maintains excellent conductivity, which can meet the needs of high-frequency and high-current circuits. The Cu-Ti2SnC-Y electrical contact material prepared by the present invention has good processing performance and plasticity, and the production process is simple and efficient. It is not only in good service condition in resistance welding electrodes, motor commutators, relays, vacuum switch electrical contacts, but also can be used in emerging fields such as renewable energy systems and electric vehicles, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 SEM image of Cu-1.0 wt.%Ti2SnC-0.2 wt.%Y composite powder;
[0026] Figure 2 It is a low-magnification SEM image of Cu-1.0 wt.%Ti2SnC-0.2 wt.%Y composite material;
[0027] Figure 3 High magnification SEM image of Cu-1.0 wt.%Ti2SnC-0.2 wt.%Y composite material;
[0028] Figure 4 This is a high-magnification SEM image of the interface of Cu-1.0 wt.%Ti2SnC-0.2 wt.%Y composite material;
[0029] Figure 5 EDS image of Ti2SnC at the interface of Cu-1.0 wt.%Ti2SnC-0.2 wt.%Y composite material;
[0030] Figure 6 This is the EDS image of the Cu matrix at the interface of Cu-1.0 wt.%Ti2SnC-0.2 wt.%Y composite material. DETAILED DESCRIPTION
[0031] The present invention is further described below in conjunction with specific embodiments.
[0032] The invention discloses a preparation method and application of Y element to improve the interface and performance of Cu-Ti2SnC composite material, belonging to the technical field of copper-based wear-resistant materials. Cu powder, Ti2SnC powder and Y powder are uniformly dispersed by wet stirring, and then Cu-Ti2SnC-Y composite powder is obtained by ball milling and stress relief annealing; the Cu-Ti2SnC-Y composite powder is subjected to spark plasma sintering to obtain Cu-Ti2SnC composite material modified by Y element; the excellent self-lubricating property of Ti2SnC gives the composite material extraordinary wear resistance and self-lubricating property; the addition of trace Y element not only improves the interface of Cu-Ti2SnC, generates YSn3 and CuY intermediate phases at the interface, and significantly improves the strength, hardness, wettability and oxidation resistance of the material; and effectively inhibits the decomposition of Ti2SnC, maintains the self-lubricating structure of Ti2SnC, and improves the wear resistance and mechanical properties of the material. The Cu-Ti2SnC composite material with improved interface and performance by Y element in the present invention has excellent service condition in resistance welding electrodes, motor commutators, relays and vacuum switch electric contacts and has broad application prospects.
[0033] The preparation method of the Cu-Ti2SnC composite material with improved interface and performance by Y element of the present invention specifically comprises the following steps:
[0034] (1) Cu powder, Ti2SnC powder and Y powder are sequentially placed in a beaker containing an appropriate amount of anhydrous ethanol and sodium dodecylbenzoate, and then the beaker is placed in a magnetic stirrer for heating and stirring. After repeated rinsing with anhydrous ethanol, the powder is dried in a drying oven until it is completely air-dried and then taken out for grinding;
[0035] Cu powder is high-purity electrolytic Cu powder, in the shape of grape bunches, with a purity of 99.999% and a particle size of 1~3 microns; Ti2SnC powder is high-purity multi-layer flaky ceramic powder with a particle size of 600~800 mesh; Y powder has a purity of 99.99% and a particle size of 0.5~2 microns;
[0036] The addition amount of Cu powder, Ti2SnC powder and Y powder is calculated according to the mass fraction, wherein the addition amount of Ti2SnC powder is 0.9~1.2 wt%, the addition amount of Y powder is 0~0.3 wt%, and the balance is Cu powder;
[0037] (2) The ground powder was sieved through a 800-1000 mesh sieve and placed in a ball mill under an argon atmosphere for ball milling at a speed of 400-450 r / min for 16-18 hours;
[0038] (3) placing the ball-milled powder in a tube furnace and performing stress relief annealing in a hydrogen atmosphere at a temperature of 300-400 °C for 1-3 hours to obtain a Cu-Ti2SnC-Y composite powder after grinding;
[0039] (4) Finally, the obtained Cu-Ti2SnC-Y composite powder is loaded into a graphite mold for spark plasma sintering. The spark plasma sintering process is to first increase the temperature from room temperature to 500-600 °C and keep it for 5-10 min, then continue to increase the temperature to 850-950 °C and keep it for 10-15 min. The heating rate is 80-100 °C / min, the pre-compression pressure is 30 MPa, and the pressure is increased to 50 MPa during the second heating process. Finally, after cooling in the furnace, the Cu-Ti2SnC electrical contact material with improved performance of the Y element is obtained.
[0040] The Cu-Ti2SnC composite material with improved interface and performance by Y element in the present invention has excellent service condition in resistance welding electrodes, motor commutators, relays and vacuum switch electric contacts and has broad application prospects.
[0041] Example 1 (Resistance welding electrode)
[0042] (1) The addition amounts of Cu powder, Ti2SnC powder and Y powder were calculated according to the mass fraction, where the addition amount of Ti2SnC powder was 1.2 wt%, the addition amount of Y powder was 0 wt%, and the rest was Cu powder. They were sequentially placed in a beaker containing an appropriate amount of anhydrous ethanol and sodium dodecylbenzoate, and then the beaker was placed in a magnetic stirrer and heated and stirred at 25 °C for 6 hours. After repeated rinsing with anhydrous ethanol, the beaker was placed in a constant temperature drying oven at 20 °C until it was completely air-dried and then taken out for grinding;
[0043] (2) The ground powder was sieved through a 800-1000 mesh sieve and placed in a ball mill under an argon atmosphere for ball milling at a speed of 400 r / min for 16 h.
[0044] (3) placing the ball-milled powder in a tube furnace and performing stress relief annealing in a hydrogen atmosphere at a temperature of 300 °C for 1 hour to obtain a Cu-Ti2SnC-Y composite powder after grinding;
[0045] (4) Finally, the obtained Cu-Ti2SnC-Y composite powder was loaded into a graphite mold for spark plasma sintering. The spark plasma sintering process was as follows: first, the temperature was raised from room temperature to 500 °C and kept at that temperature for 5 min, then the temperature was further raised to 850 °C and kept at that temperature for 10 min. The heating rate was 80 °C / min, the pre-compression pressure was 30 MPa, and the pressure was raised to 50 MPa during the second heating process. Finally, after cooling in the furnace, a Cu-Ti2SnC electrical contact material with improved interface and performance by Y element was obtained.
[0046] Example 2 (motor commutator)
[0047] (1) The addition amounts of Cu powder, Ti2SnC powder and Y powder were calculated according to the mass fraction, where the addition amount of Ti2SnC powder was 1.1 wt%, the addition amount of Y powder was 0.1 wt%, and the rest was Cu powder. They were sequentially placed in a beaker containing an appropriate amount of anhydrous ethanol and sodium dodecylbenzoate, and then the beaker was placed in a magnetic stirrer and heated and stirred at 30 °C for 7 hours. After repeated rinsing with anhydrous ethanol, the beaker was placed in a constant temperature drying oven at 25 °C until it was completely air-dried and then taken out for grinding;
[0048] (2) The ground powder was sieved through a 800-1000 mesh sieve and placed in a ball mill under an argon atmosphere for ball milling at a speed of 425 r / min for 16 h.
[0049] (3) placing the ball-milled powder in a tube furnace and performing stress relief annealing in a hydrogen atmosphere at a temperature of 350 °C for 2 hours to obtain a Cu-Ti2SnC-Y composite powder after grinding;
[0050] (4) Finally, the obtained Cu-Ti2SnC-Y composite powder was loaded into a graphite mold for spark plasma sintering. The spark plasma sintering process was as follows: first, the temperature was raised from room temperature to 550 °C and kept at that temperature for 5 min, then the temperature was further raised to 900 °C and kept at that temperature for 12 min. The heating rate was 90 °C / min, the pre-compression pressure was 30 MPa, and the pressure was raised to 50 MPa during the second heating process. Finally, after cooling in the furnace, a Cu-Ti2SnC electrical contact material with improved interface and performance by Y element was obtained.
[0051] Example 3 (Relay)
[0052] (1) The addition amounts of Cu powder, Ti2SnC powder and Y powder were calculated according to the mass fraction, where the addition amount of Ti2SnC powder was 1.0 wt%, the addition amount of Y powder was 0.2 wt%, and the rest was Cu powder. They were sequentially placed in a beaker containing an appropriate amount of anhydrous ethanol and sodium dodecylbenzoate, and then the beaker was placed in a magnetic stirrer and heated and stirred at 30 °C for 7 hours. After repeated rinsing with anhydrous ethanol, the beaker was placed in a constant temperature drying oven at 25 °C until it was completely air-dried and then taken out for grinding;
[0053] (2) The ground powder was sieved through a 800-1000 mesh sieve and placed in a ball mill under an argon atmosphere at a ball mill speed of 450 r / min for 18 h.
[0054] (3) placing the ball-milled powder in a tube furnace and performing stress relief annealing in a hydrogen atmosphere at a temperature of 350 °C for 2 hours to obtain a Cu-Ti2SnC-Y composite powder after grinding;
[0055] (4) Finally, the obtained Cu-Ti2SnC-Y composite powder was loaded into a graphite mold for spark plasma sintering. The spark plasma sintering process was as follows: first, the temperature was raised from room temperature to 550 °C and kept at this temperature for 10 min, then the temperature was further raised to 900 °C and kept at this temperature for 12 min. The heating rate was 90 °C / min, the pre-compression pressure was 30 MPa, and the pressure was raised to 50 MPa during the second heating process. Finally, after cooling in the furnace, a Cu-Ti2SnC electrical contact material with improved interface and performance by Y element was obtained.
[0056] Embodiment 4 (Electric contact of vacuum switch)
[0057] (1) The addition amounts of Cu powder, Ti2SnC powder and Y powder were calculated according to the mass fraction, where the addition amount of Ti2SnC powder was 0.9 wt%, the addition amount of Y powder was 0.3 wt%, and the rest was Cu powder. They were sequentially placed in a beaker containing an appropriate amount of anhydrous ethanol and sodium dodecylbenzoate, and then the beaker was placed in a magnetic stirrer and heated and stirred at 35 °C for 8 hours. After repeated rinsing with anhydrous ethanol, the beaker was placed in a constant temperature drying oven at 30 °C until it was completely air-dried and then taken out for grinding;
[0058] (2) The ground powder was sieved through a 800-1000 mesh sieve and placed in a ball mill under an argon atmosphere at a ball mill speed of 450 r / min for 18 h.
[0059] (3) placing the ball-milled powder in a tube furnace and performing stress relief annealing in a hydrogen atmosphere at a temperature of 400 °C for 2 hours to obtain a Cu-Ti2SnC-Y composite powder after grinding;
[0060] (4) Finally, the obtained Cu-Ti2SnC-Y composite powder was loaded into a graphite mold for spark plasma sintering. The spark plasma sintering process was as follows: first, the temperature was raised from room temperature to 600 °C and kept at this temperature for 10 min, then the temperature was further raised to 950 °C and kept at this temperature for 15 min. The heating rate was 100 °C / min, the pre-compression pressure was 30 MPa, and the pressure was raised to 50 MPa during the second heating process. Finally, after cooling in the furnace, a Cu-Ti2SnC electrical contact material with improved interface and performance by Y element was obtained.
[0061] The conductivity and mechanical properties of the Cu-Ti2SnC composite material improved by the Y element in Examples 1 to 4 were tested, and the test results are shown in Table 1:
[0062] Table 1 The conductivity, mechanical properties and average friction coefficient of Cu-Ti2SnC composite materials improved by Y element in Examples 1 to 4
[0063] It can be seen from Table 1 that the addition of trace Y element significantly improves the strength of the composite material and reduces the average friction coefficient. When 0.2 wt.% Y element is added, the tensile strength of the composite material reaches a maximum of 370 MPa, and the average friction coefficient drops to a minimum of 0.5378, indicating that the addition of Y element improves the interface of Cu-Ti2SnC and effectively inhibits the decomposition of Ti2SnC, significantly improving the mechanical properties and wear resistance of the composite material. The composite material maintains an excellent strain of 31.8% and an excellent conductivity of 85.6% IACS, obtaining a Cu-Ti2SnC electrical contact material with excellent comprehensive performance and improved interface and performance of Y element.
[0064] Depend on Figure 1 It can be seen that the Cu-Ti2SnC-Y composite powder is in irregular flakes, which helps to improve the sintering driving force and make the composite material denser.
[0065] Depend on Figure 2 and Figure 3 It can be seen that the Ti2SnC particles are evenly distributed in the copper matrix and can play a good role in dispersion strengthening.
[0066] Depend on Figure 4 It can be seen that the phase interface between Cu and Ti2SnC is complete; Figure 5 and Figure 6 Analysis shows that no Sn, Ti and other elements were detected on the Cu-based side at the interface between Cu and Ti2SnC, proving that the addition of trace Y elements improved the Cu-Ti2SnC interface and inhibited the decomposition of Ti2SnC.
[0067] The preparation method of the Y element for improving the interface and performance of a Cu-Ti2SnC composite material of the present invention comprises wet dispersion, drying, ball milling, stress relief annealing and spark plasma sintering processes. The addition of a trace amount of Y element not only improves the interface of Cu-Ti2SnC, generates YSn3 and CuY intermediate phases at the interface, and significantly improves the strength, hardness, wettability and oxidation resistance of the material; and effectively inhibits the decomposition of Ti2SnC, maintains the self-lubricating structure of Ti2SnC, improves the wear resistance and mechanical properties of the material, and maintains excellent electrical conductivity, which can meet the needs of high-frequency and high-current circuits.
[0068] The Cu-Ti2SnC-Y electrical contact material prepared by the present invention has good processing performance and plasticity, and the production process is simple and efficient. It not only has excellent service conditions in resistance welding electrodes, motor commutators, relays, and vacuum switch electrical contacts, but can also be used in emerging fields such as renewable energy systems and electric vehicles, and has broad application prospects.
[0069] The above embodiments only illustrate specific implementations of the present disclosure, but the implementations of the present disclosure are not limited by the above contents. Any changes, modifications, substitutions, combinations, and simplifications made without substantially departing from the main idea and principle of the inventive concept of the present disclosure shall be equivalent replacement methods and shall be included in the scope of protection determined by the claims.
Claims
1. A method for preparing a Cu-Ti2SnC composite material by using Y element to improve its interface and performance, characterized in that: The specific steps include: Cu powder, Ti2SnC powder and Y powder are sequentially placed in a beaker containing anhydrous ethanol, and then the beaker is placed in a magnetic stirrer for heating and stirring. After the mixed powder is stirred evenly, the beaker is placed in a drying oven until it is completely air-dried and then taken out for grinding; the ground powder is placed in a ball mill under an argon atmosphere and ball-milled; the ball-milled powder is placed in a tube furnace and stress-relief annealed under a hydrogen atmosphere at a temperature of 300-400 °C and a time of 1-3 hours. After grinding, a Cu-Ti2SnC-Y composite powder is obtained; finally, the obtained Cu-Ti2SnC-Y composite powder is placed in a graphite mold for spark plasma sintering. The process of spark plasma sintering is firstly to rise from room temperature to 500-600 °C and keep warm for 5-10 minutes, then continue to rise to 850-950 °C, keep warm for 10-15 minutes, and the heating rate is 80-100 ℃ / min, the pre-pressing pressure is 30 MPa, and the pressure rises to 50 MPa during the second heating process. Finally, after cooling with the furnace, a Cu-Ti2SnC composite material with improved performance of the Y element is obtained. The addition amounts of the Cu powder, Ti2SnC powder and Y powder are calculated according to the mass fraction, wherein the addition amount of the Ti2SnC powder is 0.9~1.2 wt%, the addition amount of the Y powder is 0.1~0.3 wt%, and the balance is Cu powder.
2. A method for preparing a Cu-Ti2SnC composite material with Y element to improve its interface and performance as claimed in claim 1, characterized in that: The Cu powder is high-purity electrolytic Cu powder in the shape of grape bunches, with a purity of 99.999% and a particle size of 1 to 3 microns; the Ti2SnC powder is high-purity multi-layer flaky ceramic powder with a particle size of 600 to 800 meshes; the Y powder has a purity of 99.99% and a particle size of 0.5 to 2 microns.
3. A method for preparing a Cu-Ti2SnC composite material with Y element to improve its interface and performance as claimed in claim 1, characterized in that: The stirring temperature of the magnetic stirrer is set at 25-35°C, and the stirring time is set at 6-8 hours. In addition to anhydrous ethanol, sodium dodecyl benzoate is added to the beaker as a dispersant to promote more uniform dispersion of the powder. The amount of anhydrous ethanol added to the beaker is determined according to the amount of Cu powder, Ti2SnC powder and Y powder added, and the amount of dispersant sodium dodecyl benzoate added is determined according to the dispersion of the mixed powder.
4. A method for preparing a Cu-Ti2SnC composite material with Y element to improve its interface and performance as claimed in claim 1, characterized in that: After the mixed powder is stirred evenly, it is repeatedly rinsed with anhydrous ethanol, and after being rinsed clean, it is placed in a blast drying oven for drying, and the temperature of the blast drying oven is set at 20-30°C.
5. The method for preparing a Cu-Ti2SnC composite material with Y element for improving the interface and performance as claimed in claim 1, characterized in that: The ground powder was sieved through a 800-1000 mesh screen and then placed in a ball mill in a vacuum glove box under an argon atmosphere. The ball mill speed was 400-450 r / min and the ball mill time was 16-18 hours.
6. A method for preparing a Cu-Ti2SnC composite material with Y element to improve its interface and performance as claimed in claim 1, characterized in that: The amount of hydrogen introduced into the tubular furnace is 300-350 mL / min.
7. A method for preparing a Cu-Ti2SnC composite material with Y element to improve its interface and performance as claimed in claim 1, characterized in that: The ball-milled powder is subjected to stress relief annealing and grinding, and then sieved through a 800-1000 mesh sieve to obtain a Cu-Ti2SnC-Y composite powder.
8. A method for preparing a Cu-Ti2SnC composite material with Y element to improve its interface and performance as claimed in claim 1, characterized in that: The graphite mold has an inner diameter of ∅20 mm, an outer diameter of ∅60 mm, and a height of 70 mm.
9. Application of a method for preparing a Cu-Ti2SnC composite material by using Y element to improve the interface and performance, characterized in that: A method for preparing a Cu-Ti2SnC-Y electrical contact material using the Y element to improve the interface and performance of a Cu-Ti2SnC composite material as described in any one of claims 1 to 8, and its use in resistance welding electrodes, motor commutators, and vacuum switch electrical contacts.