A kind of synthetic method of rubber antioxidant

By reusing condensed arylamine and adding modified nanotube powder during the synthesis of rubber anti-aging agents, the problem of high preparation cost of existing rubber anti-aging agents is solved, the anti-aging performance and the strength of rubber finished products are improved, and the resource efficiency is achieved use.

CN118165367BActive Publication Date: 2024-11-08JIANGSU GUOLI CHEM TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410324170.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-21
Publication Date
2024-11-08
Estimated Expiration
2044-03-21

AI Technical Summary

Technical Problem

The existing rubber anti-aging agent preparation methods are costly and do not involve resource reuse, resulting in insufficient production efficiency and economicality.

Method used

Using a synthesis method of rubber anti-aging agent, by using the condensed aromatic amine as recycled material in the condensation reaction kettle, and adding modified nanotube powder, the Elosite nanotube powder is modified by SDS surfactant to improve the The reaction grafting rate and anti-aging properties are optimized for process flow for reduced pressure distillation and granulation to ensure that the modified nanotube powder is evenly mixed with the raw materials.

Benefits of technology

It significantly improves the anti-aging performance of anti-aging agents, enhances the strength and stiffness of finished rubber products, reduces the loss of migration, frost spraying and washing, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118165367B_ABST
    Figure CN118165367B_ABST
Patent Text Reader

Abstract

The invention discloses a method for synthesizing a rubber antioxidant, and relates to the technical field of preparation of an antioxidant, and comprises the following steps: S1, mixing; S2, condensation reaction; S3, neutralization reaction; S4, distillation and dehydration; S5, granulation. The invention uses the aromatic amine obtained by condensation as a recycled material during the preparation process, optimizes and improves it, adds modified nanotube powder, and modifies the halloysite nanotube powder with an SDS surfactant, thereby increasing the hydroxyl content on the surface of the halloysite nanotube, thereby improving the anti-aging performance of the antioxidant, so that the strength and stiffness of the finished rubber product are improved when the antioxidant is finally applied thereto.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of antioxidant preparation, in particular to a method for synthesizing a rubber antioxidant. Background Art

[0002] Rubber antioxidant is a chemical added during the rubber production process that can delay rubber aging and extend the service life of rubber. As the aging process progresses and develops, the performance of rubber and its products will gradually decrease and completely lose their use value. In order to extend the service life of rubber products, it is necessary to add some substances that can inhibit the aging process into the rubber, thereby extending the storage period and service life of rubber and its products. These substances are called antioxidants. There are many types of antioxidants with different functions. According to their main functions, they can be divided into anti-thermal oxidation aging agents, anti-ozonants, harmful metal ion inhibitors, anti-fatigue agents, ultraviolet absorbers, anti-cracking agents, etc. However, since each protective function is often not dedicated to a certain antioxidant, most antioxidants can act on several aging factors, but to different degrees. The following is an introduction to the antioxidants commonly used in the wire and cable industry. It is not clearly classified, but only its main protective function is pointed out.

[0003] Paraphenylenediamine antioxidants can effectively inhibit the generation and development of cracks in rubber products under the combined effects of dynamic stress, ozone, and oxygen, and significantly improve the antioxidant, ozone resistance, and mechanical fatigue resistance of the products. Common paraphenylenediamine antioxidants on the market include antioxidant DBPD, antioxidant 4010, antioxidant 4010NA, antioxidant 4020, antioxidant 4030, antioxidant H, antioxidant DNP, etc. Paraphenylenediamine antioxidants can effectively improve the aging resistance of products in the production of recycled rubber products, especially antioxidant and ozone resistance. Different types of paraphenylenediamine antioxidants have different dosages in recycled rubber products, and the same type of paraphenylenediamine antioxidants have different usage and dosage in different types of recycled rubber products.

[0004] Patent CN109956875A discloses a p-phenylenediamine rubber antioxidant and a preparation method thereof. The rubber antioxidant is prepared by condensation reaction with p-phenylenediamine and p-cumylphenol as raw materials and ferric chloride as catalyst. The rubber antioxidant of the present invention has excellent anti-aging performance, good compatibility with rubber materials, and can significantly reduce the problems of migration, blooming, discoloration and water washing loss of the p-phenylenediamine antioxidant. However, the method does not involve resource recycling in the preparation process, and the cost is relatively high. Summary of the invention

[0005] In view of the above problems, the present invention provides a method for synthesizing a rubber antioxidant.

[0006] The technical solution of the present invention is:

[0007] A method for synthesizing a rubber antioxidant comprises the following steps:

[0008] S1, mixing: by weight, take 150-170 parts of o-toluidine and 130-150 parts of aniline to mix to obtain a primary mixed material, take 2 / 3 of the total amount of the primary mixed material into a condensation reactor, and store the remaining 1 / 3 of the primary mixed material for standby use, add 160-180 parts of hydroquinone and 2-3 parts of a catalyst from the feeding port of the condensation reactor, and stir and mix evenly;

[0009] S2, condensation reaction: connect the condenser cooling water to the condensation reactor, heat it to 200°C for condensation reaction, and pass the obtained product mixed amine and water into the water separator. The upper mixed amine in the water separator flows back into the condensation reactor, and the lower water in the water separator is discharged into the receiving tank and sent to the wastewater treatment station. When the temperature is continuously raised to 245°C, the remaining 1 / 3 of the initial mixed material is added to the condensation reactor, and 12 to 16 parts of recycled materials are added. The temperature is continued to rise to 255 to 260°C for reaction for 3 to 4 hours. After the condensation reaction is completed, the materials in the condensation reactor are transferred to the neutralization reactor by a vacuum system and cooled naturally;

[0010] S3, neutralization reaction: when the internal temperature of the neutralization reaction kettle drops to 110°C, keep it warm, take 2-4 parts of trisodium phosphate and put it into the neutralization reaction kettle, stir and carry out neutralization reaction for 2-3 hours, stop stirring after the neutralization reaction is completed, vacuum pump the materials inside the neutralization reaction kettle into a distillation kettle, and distill and dehydrate;

[0011] S4, distillation and dehydration: heating the material inside the still kettle and performing vacuum distillation, controlling the internal temperature of the still kettle to 270-290° C., reducing the pressure to -0.12--0.09 MPa, transferring the material inside the still kettle to the intermediate tank after the distillation is completed, and condensing and recovering the aromatic amine as the raw material of the reused material in step S2;

[0012] S5. Granulation: After the material in the intermediate tank is naturally cooled, it is introduced into a granulator for granulation to obtain a finished antioxidant with uniform particles.

[0013] Furthermore, the catalyst in step S1 is ferric oxide hexahydrate.

[0014] Note: By preferably using hexahydrate iron trioxide as a catalyst, the subsequent neutralization reaction can be stably carried out.

[0015] Furthermore, in step S1, the stirring speed is 200-300 rpm, and the stirring time is 10-30 min.

[0016] Furthermore, in step S2, the heating rate is 0.4-0.8°C / min.

[0017] Note: By controlling the heating rate, the condensation reaction time is controlled so that the condensation reaction proceeds stably and completely.

[0018] Furthermore, in step S4, the decompression equipment uses a mechanical vacuum pump, and the condensation adopts a first-stage water cooling and a first-stage freezing condensation in series, the temperature of the first-stage water cooling is 18 to 35°C, and the temperature of the first-stage freezing is -10 to -5°C.

[0019] Description: Promote the recovery of aromatic amines and the generation of recycled materials by optimizing condensation.

[0020] Furthermore, the recycled materials in step S2 include, by weight, 9 to 11 parts of aromatic amine recovered by condensation in step S4, 2 to 3 parts of modified nanotube powder, and 1 to 2 parts of deionized water.

[0021] Furthermore, the preparation method of the modified nanotube powder is:

[0022] S6-1: taking halloysite nanotube powder and adding ethanol solution at a solid-liquid ratio of 1g:3mL, stirring for 1h, drying at 75-80°C, grinding to obtain pure halloysite nanotube powder, mixing the pure halloysite nanotube powder with deionized water to obtain a pure halloysite nanotube solution with a mass concentration of 20%, adding a 2% sodium hexametaphosphate aqueous solution with a mass concentration of 10% of the total volume of the pure halloysite nanotube solution, stirring for 1h, precipitating to remove impurities, taking the upper suspension, centrifuging the suspension at a centrifugal speed of 3000-4000rpm, taking the solid, drying at 75-80°C, and grinding to obtain purified halloysite nanotube powder;

[0023] S6-2: Add SDS surfactant to deionized water at a solid-liquid ratio of 1g:5mL and mix, add 40% of the total volume of SDS surfactant purified halloysite nanotube powder, ultrasonically disperse for 10 to 15 minutes to obtain a modified nanotube solution, dry the modified nanotube solution at 85 to 90°C, and grind to obtain modified nanotube powder.

[0024] Description: By modifying the halloysite nanotube powder with SDS surfactant, the hydroxyl content on the surface of the halloysite nanotube is increased to increase the reaction grafting rate with the raw materials of the p-phenylenediamine rubber antioxidant, thereby improving the anti-aging performance of the antioxidant.

[0025] Preferably, the method for recycling the recycled material is:

[0026] Take 9-11 parts of the aromatic amine condensed and recovered in step S4, 2-3 parts of the modified nanotube powder, and 1-2 parts of deionized water, mix them, and then disperse them ultrasonically for 10-15 minutes, and then reflux them into the condensation reactor at 80°C.

[0027] Description: By optimizing the ratio of aromatic amine recovered by condensation in the recycled material and the modified nanotube powder and the timing of adding the modified nanotube powder, it is ensured that the modified nanotube powder and the recycled material can be evenly mixed with the raw materials to achieve the optimal reaction conditions, so that the antioxidant can be finally applied to the finished rubber product to improve its strength and stiffness.

[0028] Furthermore, during granulation in step S5, the temperature of the granulator head is raised to 140° C., the cooling water of the steel belt is turned on, the steel belt is started to rotate, and the pump is started to send the material in the intermediate tank into the granulator head for granulation to obtain a finished antioxidant with uniform particles.

[0029] The beneficial effects of the present invention are:

[0030] The synthetic method of a rubber antioxidant of the present invention uses aromatic amine obtained by condensation as recycled material during the preparation process, optimizes and improves the aromatic amine, adds modified nanotube powder, and modifies the halloysite nanotube powder with an SDS surfactant to increase the hydroxyl content on the surface of the halloysite nanotube, thereby increasing the reaction grafting rate with the raw materials of the p-phenylenediamine rubber antioxidant, thereby improving the anti-aging performance of the antioxidant; and optimizes the ratio of aromatic amine recovered by condensation in the recycled material to the modified nanotube powder and the timing of adding the modified nanotube powder, thereby ensuring that the modified nanotube powder and the recycled material can be uniformly mixed with the raw materials, achieving the optimal reaction conditions, and finally applying the antioxidant to the finished rubber product to improve the strength and stiffness. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 is a rubber stress-strain test diagram prepared in each case of Experimental Example 1 of the present invention;

[0032] Figure 2 This is a graph showing the change in tensile strength of the rubber prepared in each case of Experimental Example 2 of the present invention during thermal oxidation aging. DETAILED DESCRIPTION

[0033] Example 1

[0034] A method for synthesizing a rubber antioxidant comprises the following steps:

[0035] S1, mixing: by weight, take 160 parts of o-toluidine and 140 parts of aniline to mix to obtain a primary mixed material, take 2 / 3 of the total amount of the primary mixed material into a condensation reactor, and store the remaining 1 / 3 of the primary mixed material for standby use, add 170 parts of hydroquinone and 2.5 parts of a catalyst from the feeding port of the condensation reactor, the catalyst is ferric oxide hexahydrate, stir and mix evenly, the stirring speed is 250 rpm, and the stirring time is 20 min;

[0036] S2, condensation reaction: connect the condenser cooling water to the condensation reactor, heat it to 200°C for condensation reaction, and pass the obtained product mixed amine and water into the water separator. The upper mixed amine in the water separator flows back into the condensation reactor, and the lower water in the water separator is discharged into the receiving tank and sent to the wastewater treatment station. When the temperature is continuously raised to 245°C, the heating rate is 0.6°C / min, and the remaining 1 / 3 of the initial mixed material is added to the condensation reactor, and 14 parts of the recycled material are added. The temperature is continued to rise to 258°C for reaction for 3.5h. After the condensation reaction is completed, the materials in the condensation reactor are transferred to the neutralization reactor by a vacuum system and cooled naturally;

[0037] S3, neutralization reaction: when the internal temperature of the neutralization reaction kettle drops to 110°C, keep it warm, take 3 parts of trisodium phosphate and put it into the neutralization reaction kettle, stir and carry out neutralization reaction for 2.5 hours, stop stirring after the neutralization reaction is completed, vacuum pump the materials inside the neutralization reaction kettle into a distillation kettle, and distill and dehydrate;

[0038] S4, distillation and dehydration: heating the material inside the still kettle and performing vacuum distillation, controlling the internal temperature of the still kettle to 280°C, reducing the pressure to -0.1MPa, transferring the material inside the still kettle to the intermediate tank after the distillation is completed, and condensing the recovered aromatic amine as the raw material of the reused material in step S2, the vacuum equipment uses a mechanical vacuum pump, and the condensation adopts a first-stage water cooling in series with a first-stage freezing condensation, the temperature of the first-stage water cooling is 25°C, and the temperature of the first-stage freezing is -8°C;

[0039] S5, granulation: After the material in the intermediate tank is naturally cooled, it is introduced into the granulator for granulation to obtain a finished antioxidant with uniform particles. During granulation, the head of the granulator is heated to 140°C, the cooling water of the steel belt is turned on, the steel belt is started to rotate, and the pump is started to send the material in the intermediate tank into the head of the granulator for granulation to obtain a finished antioxidant with uniform particles;

[0040] The preparation method of modified nanotube powder is:

[0041] S6-1: Take the halloysite nanotube powder and add the ethanol solution at a solid-liquid ratio of 1g:3mL, stir for 1h, dry at 77°C, grind to obtain pure halloysite nanotube powder, mix the pure halloysite nanotube powder with deionized water to obtain a pure halloysite nanotube solution with a mass concentration of 20%, add 10% of the total volume of the pure halloysite nanotube solution and a 2% sodium hexametaphosphate aqueous solution, stir and mix for 1h, precipitate to remove impurities, take the upper suspension, centrifuge the suspension at a centrifugal speed of 3500rpm, take the solid, dry at 77°C, and grind to obtain purified halloysite nanotube powder;

[0042] S6-2: SDS surfactant was added to deionized water at a solid-liquid ratio of 1 g: 5 mL, and the mixture was mixed. Purified halloysite nanotube powder was added at a total volume of 40% of the SDS surfactant, and ultrasonic dispersion was performed for 12 minutes to obtain a modified nanotube solution. The modified nanotube solution was dried at 88° C. and ground to obtain a modified nanotube powder.

[0043] The recycling method of the recycled material is:

[0044] Take 10 parts of the aromatic amine condensed and recovered in step S4, 2.5 parts of the modified nanotube powder, and 1.5 parts of deionized water, mix them, and then disperse them by ultrasonic for 12 minutes, and then reflux them into the condensation reactor at 80°C.

[0045] Example 2

[0046] The difference between this embodiment and embodiment 1 is that the parameters of the recycling method of the recycled material are different.

[0047] The recycling methods of recycled materials are:

[0048] 9 parts of the aromatic amine recovered by condensation in step S4, 2 parts of the modified nanotube powder, and 1 part of deionized water were mixed and ultrasonically dispersed for 10 minutes, and then refluxed into the condensation reactor at 80°C.

[0049] Example 3

[0050] The difference between this embodiment and embodiment 1 is that the parameters of the recycling method of the recycled material are different.

[0051] The recycling methods of recycled materials are:

[0052] 11 parts of aromatic amine recovered by condensation in step S4, 3 parts of modified nanotube powder, and 2 parts of deionized water were mixed and ultrasonically dispersed for 15 minutes, and then refluxed into the condensation reactor at 80°C.

[0053] Example 4

[0054] The difference between this embodiment and Embodiment 1 is that the specific parameters in each step are different.

[0055] A method for synthesizing a rubber antioxidant comprises the following steps:

[0056] S1, mixing: by weight, take 150 parts of o-toluidine and 130 parts of aniline to mix to obtain a primary mixed material, take 2 / 3 of the total amount of the primary mixed material into a condensation reactor, and store the remaining 1 / 3 of the primary mixed material for standby use, add 160 parts of hydroquinone and 2 parts of a catalyst from the feeding port of the condensation reactor, the catalyst is ferric oxide hexahydrate, stir and mix evenly, the stirring speed is 200 rpm, and the stirring time is 10 min;

[0057] S2, condensation reaction: connect the condenser cooling water to the condensation reactor, heat it to 200°C for condensation reaction, and pass the obtained product mixed amine and water into the water separator, the upper mixed amine in the water separator flows back into the condensation reactor, and the lower water in the water separator is discharged into the receiving tank and sent to the wastewater treatment station. When the temperature is continuously raised to 245°C, the heating rate is 0.4°C / min, and the remaining 1 / 3 of the initial mixed material is added to the condensation reactor, and 12 parts of the recycled material are added, and the temperature is continued to rise to 255°C for reaction for 3h. After the condensation reaction is completed, the materials in the condensation reactor are transferred to the neutralization reactor by a vacuum system, and the temperature is naturally cooled;

[0058] S3, neutralization reaction: when the internal temperature of the neutralization reaction kettle drops to 110°C, keep it warm, take 2 parts of trisodium phosphate and put it into the neutralization reaction kettle, stir and carry out neutralization reaction for 2 hours, stop stirring after the neutralization reaction is completed, vacuum pump the materials inside the neutralization reaction kettle into a distillation kettle, and distill and dehydrate;

[0059] S4, distillation and dehydration: heat the internal material of the still kettle and perform vacuum distillation, control the internal temperature of the still kettle to 270°C, reduce the pressure to -0.12MPa, transfer the internal material of the still kettle to the intermediate tank after the distillation, and condense the recovered aromatic amine as the raw material of the reused material in step S2, the vacuum equipment uses a mechanical vacuum pump, and the condensation adopts a first-stage water cooling in series with a first-stage freezing condensation, the temperature of the first-stage water cooling is 18°C, and the temperature of the first-stage freezing is -5°C.

[0060] Example 5

[0061] The difference between this embodiment and Embodiment 1 is that the specific parameters in each step are different.

[0062] A method for synthesizing a rubber antioxidant comprises the following steps:

[0063] S1, mixing: by weight, take 170 parts of o-toluidine and 150 parts of aniline to mix to obtain a primary mixed material, take 2 / 3 of the total amount of the primary mixed material into a condensation reactor, and store the remaining 1 / 3 of the primary mixed material for standby use, add 180 parts of hydroquinone and 3 parts of a catalyst from the feeding port of the condensation reactor, the catalyst is ferric oxide hexahydrate, stir and mix evenly, the stirring speed is 300 rpm, and the stirring time is 30 min;

[0064] S2, condensation reaction: connect the condenser cooling water to the condensation reactor, heat it to 200°C for condensation reaction, and pass the obtained product mixed amine and water into the water separator, the upper mixed amine in the water separator flows back into the condensation reactor, and the lower water in the water separator is discharged into the receiving tank and sent to the wastewater treatment station. When the temperature is continuously raised to 245°C, the heating rate is 0.8°C / min, and the remaining 1 / 3 of the initial mixed material is added to the condensation reactor, and 16 parts of recycled materials are added. The temperature is continued to rise to 260°C for reaction for 4 hours. After the condensation reaction is completed, the materials in the condensation reactor are transferred to the neutralization reactor by a vacuum system and cooled naturally;

[0065] S3, neutralization reaction: when the internal temperature of the neutralization reaction kettle drops to 110°C, keep it warm, take 4 parts of trisodium phosphate and put it into the neutralization reaction kettle, stir and carry out neutralization reaction for 3 hours, stop stirring after the neutralization reaction is completed, vacuum pump the materials inside the neutralization reaction kettle into a distillation kettle, and distill and dehydrate;

[0066] S4, distillation and dehydration: heat the internal material of the still kettle and perform vacuum distillation, control the internal temperature of the still kettle to 290°C, reduce the pressure to -0.09MPa, transfer the internal material of the still kettle to the intermediate tank after the distillation, and condense the recovered aromatic amine as the raw material of the reused material in step S2, the vacuum equipment uses a mechanical vacuum pump, and the condensation adopts a first-stage water cooling in series with a first-stage freezing condensation, the temperature of the first-stage water cooling is 35°C, and the temperature of the first-stage freezing is -10°C.

[0067] Example 6

[0068] The difference between this embodiment and embodiment 1 is that the parameters of the preparation method of the modified nanotube powder are different.

[0069] The preparation method of modified nanotube powder is:

[0070] S6-1: Take the halloysite nanotube powder and add the ethanol solution at a solid-liquid ratio of 1g:3mL, stir for 1h, dry at 75°C, grind to obtain pure halloysite nanotube powder, mix the pure halloysite nanotube powder with deionized water to obtain a pure halloysite nanotube solution with a mass concentration of 20%, add 10% of the total volume of the pure halloysite nanotube solution and a 2% sodium hexametaphosphate aqueous solution, stir and mix for 1h, precipitate to remove impurities, take the upper suspension, centrifuge the suspension at a centrifugal speed of 3000rpm, take the solid, dry at 75°C, grind to obtain purified halloysite nanotube powder;

[0071] S6-2: Add SDS surfactant to deionized water at a solid-liquid ratio of 1g:5mL and mix, add 40% of the total volume of SDS surfactant purified halloysite nanotube powder, ultrasonically disperse for 10 minutes to obtain a modified nanotube solution, dry the modified nanotube solution at 85°C, and grind to obtain modified nanotube powder.

[0072] Example 7

[0073] The difference between this embodiment and embodiment 1 is that the parameters of the preparation method of the modified nanotube powder are different.

[0074] The preparation method of modified nanotube powder is:

[0075] S6-1: Take the halloysite nanotube powder and add the ethanol solution at a solid-liquid ratio of 1g:3mL, stir for 1h, dry at 80°C, grind to obtain pure halloysite nanotube powder, mix the pure halloysite nanotube powder with deionized water to obtain a pure halloysite nanotube solution with a mass concentration of 20%, add 10% of the total volume of the pure halloysite nanotube solution and a 2% sodium hexametaphosphate aqueous solution, stir for 1h, precipitate to remove impurities, take the upper suspension, centrifuge the suspension at 4000rpm, take the solid, dry at 80°C, grind to obtain purified halloysite nanotube powder;

[0076] S6-2: Add SDS surfactant to deionized water at a solid-liquid ratio of 1g:5mL and mix, add 40% of the total volume of SDS surfactant purified halloysite nanotube powder, ultrasonically disperse for 15 minutes to obtain a modified nanotube solution, dry the modified nanotube solution at 90°C, and grind to obtain modified nanotube powder.

[0077] Experimental Example 1

[0078] The performance of the antioxidant prepared by the present invention is tested below. The rubber products prepared by three different antioxidants in Examples 1 to 3 are subjected to stress-strain tests and compared with the comparative examples. In Comparative Example 1, no recycled material is added, and the other method parameters are the same as those in Example 1. In Comparative Example 2, no modified nanotube powder is added to the recycled material, and the other method parameters are the same as those in Example 1. The test results are shown in FIG. Figure 1 As shown;

[0079] It can be seen that the rubber products prepared in Examples 1 to 3 have a relatively high tensile strength, reaching about 22 to 23 MPa. This is because the modified nanotube powder in the added recycled material is evenly dispersed, which improves the bonding strength between the modified nanotube powder and the various substances in the antioxidant raw materials, thereby reducing the mobility of its molecular chain, improving the stiffness and strength of the rubber product, and reducing the elongation at break. In contrast, in Comparative Examples 1 and 2, no recycled material is added or the modified nanotube powder is not added to the recycled material, and the rubber products prepared by the antioxidant have lower stiffness and strength.

[0080] Experimental Example 2

[0081] The performance of the antioxidant prepared by the present invention is tested below. Rubber products prepared with three different antioxidants in Examples 1, 6 and 7 are taken out for accelerated aging after being stretched and hung, and then placed in an air hot oxygen aging oven at 100°C. The rubber products are taken out for tensile testing after aging for 1, 3 and 7 days, respectively. The results are as follows: Figure 2 As shown;

[0082] It can be seen that the tensile strength of the rubber products prepared with different antioxidants in the three groups of embodiments and the two groups of comparative examples slightly decreases after one day of thermal oxidative aging. As the thermal oxidative aging time increases, the tensile strength of the rubber products prepared with antioxidants in comparative examples 1 and 2 decreases significantly, especially on the 7th day, it has decreased by nearly 50%. The rubber products prepared with three different antioxidants in Examples 1, 6 and 7 have a stable decreasing trend in tensile strength during the thermal oxidative aging process from the 3rd day to the 7th day. This is because in the initial stage, the tensile strength decreases due to the consumption of antioxidants in the rubber with thermal oxidative aging, and subsequently, as the thermal oxidative aging continues, the antioxidant of the halloysite nanotube grafted antioxidant in the rubber is gradually released from the matrix and exerts its effect, thereby stabilizing the decreasing trend of the tensile strength.

Claims

1. A method for synthesizing a rubber antioxidant, characterized in that: The following steps are involved: S1, mixing: by weight, take 150-170 parts of o-toluidine and 130-150 parts of aniline to mix to obtain a primary mixed material, take 2 / 3 of the total amount of the primary mixed material into a condensation reactor, and store the remaining 1 / 3 of the primary mixed material for standby use, add 160-180 parts of hydroquinone and 2-3 parts of a catalyst from the feeding port of the condensation reactor, and stir and mix evenly; S2, condensation reaction: connect the condenser cooling water to the condensation reactor, heat it to 200°C for condensation reaction, and pass the obtained product mixed amine and water into the water separator. The upper mixed amine in the water separator flows back into the condensation reactor, and the lower water in the water separator is discharged into the receiving tank and sent to the wastewater treatment station. When the temperature is continuously raised to 245°C, the remaining 1 / 3 of the initial mixed material is added to the condensation reactor, and 12 to 16 parts of recycled materials are added. The temperature is continued to rise to 255 to 260°C for reaction for 3 to 4 hours. After the condensation reaction is completed, the materials in the condensation reactor are transferred to the neutralization reactor by a vacuum system and cooled naturally; The recycled materials in step S2 include, by weight, 9 to 11 parts of the aromatic amine recovered by condensation in step S4, 2 to 3 parts of modified nanotube powder, and 1 to 2 parts of deionized water; The preparation method of the modified nanotube powder is: S6-1: taking halloysite nanotube powder and adding ethanol solution at a solid-liquid ratio of 1g:3mL, stirring for 1h, drying at 75-80°C, grinding to obtain pure halloysite nanotube powder, mixing the pure halloysite nanotube powder with deionized water to obtain a pure halloysite nanotube solution with a mass concentration of 20%, adding a 2% sodium hexametaphosphate aqueous solution with a mass concentration of 10% of the total volume of the pure halloysite nanotube solution, stirring for 1h, precipitating to remove impurities, taking the upper suspension, centrifuging the suspension at a centrifugal speed of 3000-4000rpm, taking the solid, drying at 75-80°C, and grinding to obtain purified halloysite nanotube powder; S6-2: SDS surfactant was added to deionized water at a solid-liquid ratio of 1 g: 5 mL, and the mixture was mixed. Purified halloysite nanotube powder was added at a total volume of 40% of the SDS surfactant, and ultrasonic dispersion was performed for 10 to 15 minutes to obtain a modified nanotube solution. The modified nanotube solution was dried at 85 to 90° C., and ground to obtain a modified nanotube powder. S3, neutralization reaction: when the internal temperature of the neutralization reaction kettle drops to 110°C, keep it warm, take 2-4 parts of trisodium phosphate and put it into the neutralization reaction kettle, stir and carry out neutralization reaction for 2-3 hours, stop stirring after the neutralization reaction is completed, vacuum pump the materials inside the neutralization reaction kettle into a distillation kettle, and distill and dehydrate; S4, distillation and dehydration: heating the material inside the still kettle and performing vacuum distillation, controlling the internal temperature of the still kettle to 270-290° C., reducing the pressure to -0.12--0.09 MPa, transferring the material inside the still kettle to the intermediate tank after the distillation is completed, and condensing and recovering the aromatic amine as the raw material of the reused material in step S2; S5. Granulation: After the material in the intermediate tank is naturally cooled, it is introduced into a granulator for granulation to obtain a finished antioxidant with uniform particles.

2. The method for synthesizing a rubber antioxidant according to claim 1, characterized in that: The catalyst in step S1 is ferric oxide hexahydrate.

3. The method for synthesizing a rubber antioxidant according to claim 1, characterized in that: In step S1, the stirring speed is 200-300 rpm, and the stirring time is 10-30 min.

4. The method for synthesizing a rubber antioxidant according to claim 1, characterized in that: The heating rate in step S2 is 0.4-0.8°C / min.

5. The method for synthesizing a rubber antioxidant according to claim 1, characterized in that: In step S4, the decompression device uses a mechanical vacuum pump, and the condensation adopts a first-stage water cooling in series with a first-stage freezing condensation, the temperature of the first-stage water cooling is 18 to 35° C., and the temperature of the first-stage freezing is -10 to -5° C.

6. The method for synthesizing a rubber antioxidant according to claim 1, characterized in that: The recycling method of the recycled material is: Take 9-11 parts of the aromatic amine condensed and recovered in step S4, 2-3 parts of the modified nanotube powder, and 1-2 parts of deionized water, mix them, and then disperse them ultrasonically for 10-15 minutes, and then reflux them into the condensation reactor at 80°C.

7. The method for synthesizing a rubber antioxidant according to claim 1, characterized in that: During granulation in step S5, the temperature of the granulator head is raised to 140° C., the cooling water of the steel belt is turned on, the steel belt is started to rotate, and the pump is started to send the material in the intermediate tank into the granulator head for granulation to obtain a finished antioxidant with uniform particles.