A high-strength PVC and preparation method thereof, and a cable protection tube

Through the blending of high-strength PVC materials and additives to improve compatibility, the brittleness problem of double-wall corrugated pipes in low-temperature environments is solved, and the efficient use of cable protection pipes in cold areas and the improvement of ring rigidity is achieved.

CN118165434BActive Publication Date: 2024-11-15HENAN EPRI GAOKE GROUP CO LTD +2
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410286174.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-13
Publication Date
2024-11-15
Estimated Expiration
2044-03-13

AI Technical Summary

Technical Problem

The brittleness problem of existing double-wall corrugated pipes in low temperature environments, especially the use of composite reinforced HMPVC in cold areas, and the low elastic modulus of PE and PP and poor heat resistance of PVC limits its application range.

Method used

High-strength PVC material is made of PVC, silicone rubber, compatibility agent, ACR resin, chlorinated polyethylene, filler, heat stabilizer and polyethylene wax, etc., to improve compatibility through blending and additives, improve low-temperature toughness and The ring is rigid, and the cable protection tube is prepared.

Benefits of technology

It significantly improves the low-temperature toughness and ring rigidity of the cable protection tube, making it excellent performance in the temperature range of -60℃ to +250℃, suitable for use in cold areas, and extends its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004739208120000121
    Figure BDA0004739208120000121
  • Figure BDA0004739208120000131
    Figure BDA0004739208120000131
Patent Text Reader

Abstract

The present invention relates to the field of cable protection tubes, and specifically discloses a high-strength PVC and a preparation method, and a cable protection tube. The high-strength PVC is made of the following raw materials in parts by weight: 60-80 parts of PVC; 15-20 parts of silicone rubber; 4-6 parts of compatibilizer; 2.5-3.5 parts of ACR resin; 5-7 parts of chlorinated polyethylene; 10-15 parts of filler; 3-5 parts of heat stabilizer; 0.8-1.5 parts of polyethylene wax; 1-2 parts of stearic acid. The present invention uses PVC and silicone rubber blended as the main materials of the cable protection tube, and uses a compatibilizer to improve the compatibility of the two, adds a variety of additives, improves the overall performance, and makes the cable protection tube have excellent low-temperature toughness and high ring rigidity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of cable protection tubes, and more specifically, to a high-strength PVC and a preparation method thereof, and a cable protection tube. Background Art

[0002] Double-wall corrugated pipe refers to a new type of pipe with an annular outer wall and a smooth inner wall. It has the advantages of light weight, fast construction and easy installation. It is widely used in municipal engineering, industry, railways and other industries. In municipal engineering, it can be used as drainage and sewage pipes, and in railways, it can be used as a protective pipe for communication cables and optical cables.

[0003] The mainstream materials of double-wall corrugated pipes include PE, PP and PVC. Among them, PE and PP have low elastic modulus and poor ring stiffness, and PVC is brittle and has poor heat resistance, all of which have application limitations.

[0004] Composite reinforced HMPVC refers to high-strength polyvinyl chloride made by compounding PVC with other polymers. It has good mechanical properties, but it is still very brittle in low temperature environments and is not suitable for use in cold areas. Summary of the invention

[0005] In order to improve the low-temperature toughness of PVC, the present invention provides a high-strength PVC and a preparation method thereof, and a cable protection tube.

[0006] In the first aspect, the present invention provides a high-strength PVC, which adopts the following technical solution:

[0007] A high-strength PVC is made from the following raw materials in parts by weight:

[0008] PVC 60-80 parts;

[0009] Silicone rubber 15-20 parts;

[0010] 4-6 parts of compatibilizer;

[0011] ACR resin 2.5-3.5 parts;

[0012] Chlorinated polyethylene 5-7 parts;

[0013] 10-15 parts of filler;

[0014] 3-5 parts of heat stabilizer;

[0015] Polyethylene wax 0.8-1.5 parts;

[0016] 1-2 parts of stearic acid.

[0017] By adopting the above technical solution, PVC and silicone rubber are blended as the main materials of the cable protection tube, and a compatibilizer is used to improve the compatibility of the two, and a variety of additives are added to improve the overall performance, so that the cable protection tube has excellent low-temperature toughness and high ring rigidity.

[0018] Among them, silicone rubber is a polymer compound with excellent heat resistance, cold resistance, dielectric properties, ozone resistance and atmospheric aging resistance. Its outstanding performance is a wide range of operating temperatures. It can be used for a long time at -60°C to +250°C, making it very suitable as a material for cable protection tubes. However, silicone rubber is a non-polar rubber, and the Si-O bond in its molecular structure has high polarity, but silicone rubber as a whole is still a non-polar substance, while PVC has polar chlorine atoms and exhibits a certain polarity in its molecular structure. Therefore, the compatibility of PVC and silicone rubber is not good. Based on the physical and chemical properties of silicone rubber and PVC, the present invention makes a self-made compatibilizer so that they can be blended and used, thereby improving the low-temperature toughness of PVC corrugated pipes.

[0019] ACR resin is an acrylic copolymer with a core-shell structure. It is usually used as an impact modifier and processing modifier for PVC. It can not only improve the impact resistance of PVC materials, but also improve the plasticization properties of PVC resin, reduce the processing temperature and pressure of PVC, make it easier to process and shape, shorten the processing cycle, and improve production efficiency. ACR resin also has good weather resistance, which can enhance the UV resistance and aging resistance of PVC materials and extend its service life. In addition, ACR resin can synergize with compatibilizers in the blending system of PVC and silicone rubber, and improve the compatibility of PVC and silicone rubber.

[0020] Chlorinated polyethylene (CPE) is mainly used as a plasticizer and modifier in PVC materials, and its functions are as follows: 1. Plasticizing effect: As a plasticizer, it can reduce the processing temperature of PVC, improve processing performance, and make PVC easier to plasticize and flow; 2. Impact resistance: Improve the impact resistance of PVC materials, improve its toughness and strength, make the cable protection tube less likely to break, and improve its durability; 3. Weather resistance: Improve the UV resistance and aging resistance of PVC materials, so that the cable protection tube has a longer service life when used outdoors; 4. Chemical corrosion resistance: Improve chemical corrosion resistance, so that the cable protection tube is not easily corroded by acid, alkali, salt and other chemical substances. In addition, chlorinated polyethylene can work synergistically with a compatibilizer in the blending system of PVC and silicone rubber, and has an improving effect on the compatibility of PVC and silicone rubber.

[0021] Fillers play a role in reinforcement and filling. Heat stabilizers play a stabilizing role to prevent PVC from thermal decomposition during processing. Polyethylene wax has excellent cold resistance, heat resistance, chemical resistance and wear resistance, which can improve the processing performance of PVC and improve the dispersibility of fillers. Stearic acid plays a role in promoting processing performance, improving physical properties, adjusting hardness, lubrication, and thermal stability.

[0022] Optionally, the preparation process of the compatibilizer is as follows:

[0023] By weight, 30-40 parts of terminal hydroxyl nitrile rubber and 5-7 parts of diphenylmethane diisocyanate are mixed evenly, nitrogen is passed through for protection, the temperature is raised to 80-85°C, the reaction is carried out for 2-3 hours, 1-2 parts of chain extender are added, the reaction is continued for 30-50 minutes, and then 80-100 parts of tetrahydrofuran are added. After mixing evenly, the mixture is allowed to stand at room temperature for 12-18 hours, and then dried at 50-60°C for 6-8 hours, and finally cured at 100-110°C for 10-12 hours to obtain a compatibilizer.

[0024] By adopting the above technical solution, the polymer obtained after the grafting reaction of the terminal hydroxyl nitrile rubber and phenylmethane diisocyanate can be used as a compatibilizer between PVC and silicone rubber, which can significantly improve the compatibility between the two.

[0025] Optionally, the chain extender is diethylene glycol.

[0026] By adopting the above technical solution, the chain extender is preferably selected to improve the effect of the compatibilizer.

[0027] Optionally, the added amount of the PVC is 60 parts, and the added amount of the silicone rubber is 20 parts.

[0028] By adopting the above technical solution, when the compatibility between PVC and silicone rubber is improved, the low-temperature toughness of the cable protection tube can be further improved by increasing the content ratio of silicone rubber.

[0029] Optionally, 2-3 parts by weight of fluorinated phosphazene rubber are also included.

[0030] By adopting the above technical solution, fluorinated phosphazene rubber refers to an elastomer composed of alternating phosphorus atoms and nitrogen atoms, with fluoroalkoxy groups on the phosphorus atoms. It has excellent heat aging resistance, low temperature resistance, flame retardancy and electrical properties. Its brittle temperature is -68°C, and it can be used in most cold areas. Fluorinated phosphazene rubber is suitable for the blending system of PVC and silicone rubber and has good compatibility.

[0031] Optionally, the filler comprises sepiolite and camphor wood powder in a mass ratio of (2-5):1.

[0032] By adopting the above technical scheme, the crystals of sepiolite are in a layered chain structure, orthorhombic or monoclinic, and are generally in block, earthy or fibrous aggregates. Sepiolite also has the properties of decolorization, heat insulation, insulation, corrosion resistance, radiation resistance and thermal stability. Camphorwood powder is a powdery substance processed from camphorwood, which has a natural fragrance and the functions of anti-insect, moisture-proof and anti-corrosion. The composite filler of the two can improve the toughness of PVC corrugated pipes to a certain extent.

[0033] Optionally, the mass ratio of the sepiolite to the camphor wood powder is 3:1.

[0034] Optionally, the heat stabilizer is a calcium-zinc composite stabilizer.

[0035] By adopting the above technical solution, the calcium-zinc composite stabilizer is a non-toxic stabilizer which is synthesized by a special composite process with calcium salt, zinc salt, lubricant, antioxidant and the like as main components and can replace toxic stabilizers such as lead-cadmium salts and organic tin. It not only has good thermal stability, light stability, transparency and tinting power, but also has excellent processing performance in PVC resin products.

[0036] In a second aspect, the present invention provides a method for preparing a cable protection tube, which adopts the following technical solution:

[0037] A method for preparing a cable protection tube comprises the following steps:

[0038] S1 Mixing: according to the required weight parts of the formula, PVC, silicone rubber, compatibilizer, ACR resin, chlorinated polyethylene, filler, heat stabilizer, polyethylene wax and stearic acid are put into a high-speed kneading machine, kneaded at a speed of 1000-1200r / min for 10-15min, and discharged at a temperature of 120-130℃ to obtain a hot mix;

[0039] S2 stirring and cooling: put the hot mixed material into a low-speed mixer, mix it at a speed of 80-100 r / min for 5-7 minutes, and discharge it at a temperature of 50-55°C to obtain a cold mixed material;

[0040] S3 extrusion molding: put the above cold mixed material into a twin-screw extruder with a die head temperature of 180-210℃, and mold the outer wall and inner wall at one time, and then use a compression molding machine to shape and pull to make the outer wall corrugated, and finally cut it with a cutting machine, and then use a expanding machine to expand it to obtain a cable protection tube.

[0041] In a third aspect, the present invention provides a cable protection tube produced by the above-mentioned preparation method.

[0042] In summary, the present invention has the following beneficial effects:

[0043] The PVC and silicone rubber are blended as the main materials of the cable protection tube, and the polymer obtained by grafting reaction of terminal hydroxyl nitrile rubber and phenylmethane diisocyanate is used as a compatibilizer between PVC and silicone rubber, which can significantly improve the compatibility of the blending system. A variety of additives are added to improve the overall performance, so that the cable protection tube has excellent low-temperature toughness and high ring rigidity. DETAILED DESCRIPTION

[0044] The present invention is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the reactions are carried out according to conventional conditions or conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.

[0045] The embodiments of the present invention adopt the following raw materials:

[0046] The model of PVC is GM-R3X, purchased from Guangdong Guangsu Technology Co., Ltd.; the model of silicone rubber is MY2056HTV-1, purchased from Anhui Mingyi Silicon Industry Co., Ltd.; ACR resin, calcium zinc composite stabilizer, and chlorinated polyethylene are all purchased from Shandong Bangtai Petrochemical (Group) Co., Ltd., the model of ACR resin is BLD-81, and the model of chlorinated polyethylene is 135B; the average particle size of sepiolite is 500 mesh, and the average particle size of camphor wood powder is 300 mesh; the model of terminal hydroxyl nitrile rubber is 1300X8, purchased from Huntsman.

[0047] Preparation Example 1:

[0048] The preparation process of the compatibilizer is as follows:

[0049] By weight, 30 parts of terminal hydroxyl nitrile rubber and 5 parts of diphenylmethane diisocyanate were mixed evenly, nitrogen was passed through, the temperature was raised to 80°C, and the reaction was carried out for 2 hours. Then 1 part of 1,4-butanediol was added and the reaction was continued for 30 minutes. Then 80 parts of tetrahydrofuran were added, mixed evenly, and allowed to stand at room temperature for 12 hours, then dried at 50°C for 6 hours, and finally cured at 100°C for 10 hours to obtain a compatibilizer.

[0050] Preparation Example 2:

[0051] The preparation process of the compatibilizer is as follows:

[0052] By weight, 40 parts of terminal hydroxyl nitrile rubber and 7 parts of diphenylmethane diisocyanate were mixed evenly, nitrogen was passed through, the temperature was raised to 85°C, and the reaction was carried out for 3 hours. Then 2 parts of 1,4-butanediol were added and the reaction was continued for 50 minutes. Then 100 parts of tetrahydrofuran were added, mixed evenly, and allowed to stand at room temperature for 18 hours, and then dried at 60°C for 8 hours, and finally cured at 110°C for 12 hours to obtain a compatibilizer.

[0053] Preparation Example 3:

[0054] The preparation process of the compatibilizer is as follows:

[0055] By weight, 35 parts of terminal hydroxyl nitrile rubber and 6 parts of diphenylmethane diisocyanate were mixed evenly, nitrogen was passed through, the temperature was raised to 82°C, the reaction was carried out for 2.5 hours, and then 1.5 parts of 1,4-butanediol were added, and the reaction was continued for 40 minutes. Then 90 parts of tetrahydrofuran were added, and after mixing evenly, the mixture was allowed to stand at room temperature for 15 hours, and then dried at 55°C for 7 hours, and finally cured at 105°C for 11 hours to obtain a compatibilizer.

[0056] Preparation Example 4:

[0057] The preparation process of the compatibilizer is as follows:

[0058] By weight, 35 parts of terminal hydroxyl nitrile rubber and 6 parts of diphenylmethane diisocyanate were mixed evenly, nitrogen was passed through, the temperature was raised to 82°C, the reaction was carried out for 2.5 hours, 1.5 parts of diethylene glycol were added, the reaction was continued for 40 minutes, and then 90 parts of tetrahydrofuran were added. After mixing evenly, the mixture was allowed to stand at room temperature for 15 hours, and then dried at 55°C for 7 hours, and finally cured at 105°C for 11 hours to obtain a compatibilizer.

[0059] Embodiment 1:

[0060] A cable protection tube is made of high-strength PVC. The high-strength PVC is made of raw materials containing the following parts by weight:

[0061] PVC 60 parts;

[0062] Silicone rubber 15 parts;

[0063] 4 parts of compatibilizer, prepared in Preparation Example 1;

[0064] 2.5 parts of ACR resin;

[0065] 5 parts of chlorinated polyethylene;

[0066] 10 parts of calcium carbonate;

[0067] 3 parts of calcium zinc composite stabilizer;

[0068] 0.8 parts of polyethylene wax;

[0069] 1 part of stearic acid.

[0070] A method for preparing a cable protection tube comprises the following steps:

[0071] S1 Mixing: according to the required weight parts of the formula, PVC, silicone rubber, compatibilizer, ACR resin, chlorinated polyethylene, calcium carbonate, calcium zinc composite stabilizer, polyethylene wax and stearic acid are put into a high-speed kneading machine, kneaded at a speed of 1000r / min for 10min, and discharged at a temperature of 120°C to obtain a hot mix;

[0072] S2 stirring and cooling: put the hot mixture into a low-speed mixer, mix at a speed of 80r / min for 5min, discharge at a temperature of 50°C to obtain a cold mixture;

[0073] S3 extrusion molding: put the above cold mixed material into a twin-screw extruder with a die head temperature of 180°C, and mold the outer wall and inner wall at one time, and then use a compression molding machine to shape and pull to make the outer wall corrugated, and finally cut it with a cutting machine, and then use a expanding machine to expand it to obtain a cable protection tube.

[0074] Embodiment 2:

[0075] A cable protection tube is made of high-strength PVC. The high-strength PVC is made of raw materials containing the following parts by weight:

[0076] PVC 80 parts;

[0077] Silicone rubber 20 parts;

[0078] 6 parts of compatibilizer, prepared in Preparation Example 2;

[0079] 3.5 parts of ACR resin;

[0080] Chlorinated polyethylene 7 parts;

[0081] 15 parts of calcium carbonate;

[0082] 5 parts of calcium zinc composite stabilizer;

[0083] 1.5 parts of polyethylene wax;

[0084] 2 parts of stearic acid.

[0085] A method for preparing a cable protection tube comprises the following steps:

[0086] S1 Mixing: according to the required weight parts of the formula, PVC, silicone rubber, compatibilizer, ACR resin, chlorinated polyethylene, calcium carbonate, calcium zinc composite stabilizer, polyethylene wax and stearic acid are put into a high-speed kneading machine, kneaded at a speed of 1200r / min for 15min, and discharged at a temperature of 130°C to obtain a hot mix;

[0087] S2 stirring and cooling: put the hot mixture into a low-speed mixer, mix at a speed of 100 r / min for 7 minutes, and discharge the mixture at a temperature of 55°C to obtain a cold mixture;

[0088] S3 extrusion molding: put the above cold mixed material into a twin-screw extruder with a die head temperature of 210°C, and mold the outer wall and inner wall at one time, and then use a compression molding machine to shape and pull to make the outer wall corrugated, and finally cut it with a cutting machine, and then use a expanding machine to expand it to obtain a cable protection tube.

[0089] Embodiment 3:

[0090] A cable protection tube is made of high-strength PVC. The high-strength PVC is made of raw materials containing the following parts by weight:

[0091] PVC 70 parts;

[0092] Silicone rubber 18 parts;

[0093] 5 parts of compatibilizer, prepared in Preparation Example 3;

[0094] 3 parts of ACR resin;

[0095] 6 parts of chlorinated polyethylene;

[0096] 12 parts of calcium carbonate;

[0097] 4 parts of calcium zinc composite stabilizer;

[0098] 1.2 parts of polyethylene wax;

[0099] 1.5 parts of stearic acid.

[0100] A method for preparing a cable protection tube comprises the following steps:

[0101] S1 Mixing: according to the required weight parts of the formula, PVC, silicone rubber, compatibilizer, ACR resin, chlorinated polyethylene, calcium carbonate, calcium zinc composite stabilizer, polyethylene wax and stearic acid are put into a high-speed kneading machine, kneaded at a speed of 1100r / min for 12min, and discharged at a temperature of 125°C to obtain a hot mix;

[0102] S2 stirring and cooling: put the hot mixture into a low-speed mixer, mix at a speed of 90r / min for 6min, and discharge at a temperature of 52°C to obtain a cold mixture;

[0103] S3 extrusion molding: put the above cold mixed material into a twin-screw extruder with a die head temperature of 190°C, and mold the outer wall and inner wall at one time, and then use a compression molding machine to shape and pull to make the outer wall corrugated, and finally cut it with a cutting machine, and then use a expanding machine to expand it to obtain a cable protection tube.

[0104] Embodiment 4:

[0105] A cable protection tube is made of high-strength PVC. The high-strength PVC is made of raw materials containing the following parts by weight:

[0106] PVC 70 parts;

[0107] Silicone rubber 18 parts;

[0108] 5 parts of compatibilizer, prepared in Preparation Example 4;

[0109] 3 parts of ACR resin;

[0110] 6 parts of chlorinated polyethylene;

[0111] 12 parts of calcium carbonate;

[0112] 4 parts of calcium zinc composite stabilizer;

[0113] 1.2 parts of polyethylene wax;

[0114] 1.5 parts of stearic acid.

[0115] A method for preparing a cable protection tube comprises the following steps:

[0116] S1 Mixing: according to the required weight parts of the formula, PVC, silicone rubber, compatibilizer, ACR resin, chlorinated polyethylene, calcium carbonate, calcium zinc composite stabilizer, polyethylene wax and stearic acid are put into a high-speed kneading machine, kneaded at a speed of 1100r / min for 12min, and discharged at a temperature of 125°C to obtain a hot mix;

[0117] S2 stirring and cooling: put the hot mixture into a low-speed mixer, mix at a speed of 90r / min for 6min, and discharge at a temperature of 52°C to obtain a cold mixture;

[0118] S3 extrusion molding: put the above cold mixed material into a twin-screw extruder with a die head temperature of 190°C, and mold the outer wall and inner wall at one time, and then use a compression molding machine to shape and pull to make the outer wall corrugated, and finally cut it with a cutting machine, and then use a expanding machine to expand it to obtain a cable protection tube.

[0119] Embodiment 5:

[0120] The only difference from Example 4 is that the added amount of PVC is 60 parts and the added amount of silicone rubber is 20 parts.

[0121] Embodiment 6:

[0122] The only difference from Example 5 is that the high-strength PVC also contains 2 parts of fluorinated phosphazene rubber, which is added to the S1 mixture.

[0123] Embodiment 7:

[0124] The only difference from Example 5 is that the high-strength PVC also contains 3 parts of fluorinated phosphazene rubber, which is added to the S1 mixture.

[0125] Embodiment 8:

[0126] The only difference from Example 7 is that the filler is replaced by sepiolite and camphor wood powder in a ratio of 5:1.

[0127] Embodiment 9:

[0128] The only difference from Example 7 is that the filler is replaced by sepiolite and camphor wood powder in a ratio of 2:1.

[0129] Embodiment 10:

[0130] The only difference from Example 7 is that the filler is replaced by sepiolite and camphor wood powder in a ratio of 3:1.

[0131] Comparative Example 1:

[0132] The only difference from Example 3 is that the high-strength PVC does not contain silicone rubber and compatibilizer.

[0133] Comparative Example 2:

[0134] The only difference from Example 3 is that the high-strength PVC does not contain ACR resin.

[0135] Comparative Example 3:

[0136] The only difference from Example 3 is that the high-strength PVC does not contain chlorinated polyethylene.

[0137] Performance Testing:

[0138] With reference to the method described in GB / T 18477.1-2007 "Uniform polyvinyl chloride (PVC-U) structural wall pipe system for buried drainage Part 1: Double-wall corrugated pipe", the cable protection pipes of Examples 1-10 and Comparative Examples 1-3 were tested for performance, and the ring stiffness, room temperature impact performance and low temperature impact performance were tested. The results are shown in Table 1.

[0139] Among them, low-temperature impact performance means that the cable protection tube sample is placed in an environment of -35°C for 24 hours before testing, and then the impact performance test is carried out.

[0140] The greater the ring stiffness, the stronger the cable protection tube's ability to resist external pressure load. The indicator of impact performance is the true impact rate, which is the total number of impact damages divided by the total number of impacts when the entire batch of products is tested, expressed as a percentage. The lower the true impact rate, the better the impact toughness of the cable protection tube.

[0141] Table 1 Cable protection tube performance test results record

[0142]

[0143]

[0144] It can be seen from Table 1 that:

[0145] 1. Combining the test results of Examples 1-3 and Comparative Example 1, it can be seen that the addition of silicone rubber and compatibilizer is beneficial to significantly improve the low-temperature toughness of the cable protection tube, while still maintaining appropriate ring stiffness to meet the use requirements;

[0146] 2. Combining the test results of Example 3 and Comparative Examples 2 and 3, it can be seen that the addition of ACR resin and chlorinated polyethylene has an impact on the ring stiffness and impact performance of the cable protection tube, especially the low-temperature impact performance;

[0147] 3. Combining the test results of Example 3 and Example 4, it can be seen that the use of diethylene glycol as a chain extender is beneficial to improving the effect of the compatibilizer, thereby improving the comprehensive performance of the cable protection tube;

[0148] 4. Combining the test results of Example 4 and Example 5, it can be seen that the increase in the amount of silicone rubber added has a significant effect on improving the low-temperature impact performance;

[0149] 5. Combining the test results of Example 5 with those of Examples 6 and 7, it can be seen that the fluorinated phosphazene rubber has a significant effect on improving the low-temperature impact properties;

[0150] 6. Combining the test results of Example 7 and Examples 8-10, it can be seen that the filler is preferably sepiolite and camphor wood powder. Although the ring stiffness is reduced to a certain extent, the impact performance is significantly improved, meeting the use requirements.

[0151] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.

Claims

1. A high-strength PVC, characterized in that: Made from the following raw materials in parts by weight: PVC 60-80 parts; Silicone rubber 15-20 parts; 4-6 parts of compatibilizer; ACR resin 2.5-3.5 parts; Chlorinated polyethylene 5-7 parts; 10-15 parts of filler; 3-5 parts of heat stabilizer; Polyethylene wax 0.8-1.5 parts; 1-2 parts of stearic acid; The preparation process of the compatibilizer is as follows: By weight, 30-40 parts of terminal hydroxyl nitrile rubber and 5-7 parts of diphenylmethane diisocyanate are mixed evenly, nitrogen is passed through for protection, the temperature is raised to 80-85°C, the reaction is carried out for 2-3 hours, 1-2 parts of diethylene glycol are added, the reaction is continued for 30-50 minutes, and then 80-100 parts of tetrahydrofuran are added. After mixing evenly, the mixture is allowed to stand at room temperature for 12-18 hours, and then dried at 50-60°C for 6-8 hours, and finally cured at 100-110°C for 10-12 hours to obtain a compatibilizer.

2. The high-strength PVC according to claim 1, characterized in that: The added amount of the PVC is 60 parts, and the added amount of the silicone rubber is 20 parts.

3. The high-strength PVC according to claim 1, characterized in that: Calculated by weight, it also contains 2-3 parts of fluorinated phosphazene rubber.

4. The high-strength PVC according to claim 1, characterized in that: The filler includes sepiolite and camphor wood powder in a mass ratio of (2-5):

1.

5. The high-strength PVC according to claim 4, characterized in that: The mass ratio of the sepiolite to the camphor wood powder is 3:

1.

6. The high-strength PVC according to claim 1, characterized in that: The heat stabilizer is a calcium-zinc composite stabilizer.

7. A method for preparing a cable protection tube, characterized in that: The steps include: S1 Mixing: according to the high-strength PVC ratio described in any one of claims 1 to 6, PVC, silicone rubber, compatibilizer, ACR resin, chlorinated polyethylene, filler, heat stabilizer, polyethylene wax and stearic acid are put into a high-speed kneading machine, kneaded at a speed of 1000-1200r / min for 10-15min, and discharged at a temperature of 120-130°C to obtain a hot mix; S2 stirring and cooling: put the hot mixed material into a low-speed mixer, mix it at a speed of 80-100 r / min for 5-7 minutes, and discharge it at a temperature of 50-55°C to obtain a cold mixed material; S3 extrusion molding: put the above cold mixed material into a twin-screw extruder with a die head temperature of 180-210℃, and mold the outer wall and inner wall at one time, and then use a compression molding machine to shape and pull to make the outer wall corrugated, and finally cut it with a cutting machine, and then use a expanding machine to expand it to obtain a cable protection tube.

8. A cable protection tube obtained by the preparation method according to claim 7.

Citation Information

Cited By

  • High-performance low-cost PVC (polyvinyl chloride) composite material and application thereof in cable protection pipe