A method for rolling fine-grained, high-strength nickel-based alloys
By employing a fine-grained, high-strength rolling method for nickel-based alloys, and through homogenization heat treatment and two-stage rolling, controlling the heating temperature and compression ratio, the problem of nickel-based alloy plates failing to achieve high strength levels in existing technologies has been solved, thus realizing high-strength and fine-grained plate performance.
Patent Information
- Application Number
- CN202410291965.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-14
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-03-14
AI Technical Summary
Existing technologies cannot reliably achieve the high yield strength, tensile strength, and elongation requirements for large-diameter, long-distance oil pipelines through conventional rolling and heat treatment processes, and are prone to mixed crystal and coarse crystal phenomena.
A fine-grained, high-strength rolling method for nickel-based alloys is adopted, including homogenization heat treatment, two-stage rolling, and annealing. By controlling parameters such as heating temperature, compression ratio, and final rolling temperature, fine grains and high strength of nickel-based alloy plates are achieved.
It achieves a grain size of ≥7 for nickel-based alloy plates, meeting the performance requirements of high-strength grades such as yield strength ≥414MPa, tensile strength ≥827MPa, and elongation ≥30%, while avoiding mixed grain and coarse grain problems.
Smart Images

Figure CN118166299B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for rolling fine-grained, high-strength nickel-based alloys, specifically how to achieve fine-grained, high-strength nickel-based alloy sheets through rolling and other control methods. Background Technology
[0002] Nickel-based alloys, due to their excellent high-temperature mechanical properties and corrosion resistance, are widely used in petrochemicals, key equipment, and other fields, making them an indispensable and extremely important material for economic construction and national defense. The performance requirements for nickel-based alloy plates vary depending on the application. For example, for N06625 nickel-based alloy, Grade 1 is a high-strength grade, primarily aiming for high strength and high fatigue performance, requiring a yield strength ≥379MPa, tensile strength ≥758MPa, and elongation ≥30%; Grade 2 is a low-strength grade, primarily aiming for high creep and endurance performance, requiring a yield strength ≥276MPa, tensile strength ≥690MPa, and elongation ≥30%. However, for large-diameter, long-distance oil pipelines, to ensure pipeline dimensional stability and overhead rigidity, even higher requirements are placed on the mechanical properties of the medium-strength plate (requiring a yield strength ≥414MPa, tensile strength ≥827MPa, and elongation ≥30%). Since N06625 is a solid solution strengthened nickel-based alloy, it is difficult to stably achieve the above-mentioned high strength level using conventional rolling and heat treatment processes. After heat treatment, phenomena such as mixed grains and coarse grains often occur. Summary of the Invention
[0003] The purpose of this invention is to address the shortcomings of existing technologies by providing a method for fine-grained, high-strength rolling of nickel-based alloys.
[0004] Specifically, the nickel-based alloy fine-grained high-strength rolling method provided by the present invention includes:
[0005] (1) Homogenize the slab material with heat treatment;
[0006] (2) The billet is subjected to a first rolling process to obtain an intermediate billet;
[0007] The thickness of the intermediate billet is determined based on the thickness of the finished plate to ensure that the compression ratio of the second rolling is ≥5.
[0008] (3) The intermediate billet is subjected to a second rolling process to obtain the finished plate;
[0009] Among them, the heating temperature of the second rolling process increases with the increase of the compression ratio;
[0010] (4) Annealing of finished boards.
[0011] In the above-mentioned fine-grained high-strength rolling method for nickel-based alloys, the slab is smelted in a vacuum induction furnace or electric furnace, and then obtained by continuous casting or ingot casting.
[0012] In the above-mentioned method for rolling fine-grained, high-strength nickel-based alloys, the homogenization heat treatment temperature is 1200-1250℃, and the heating time is 48-72h.
[0013] In the above-mentioned fine-grained high-strength rolling method for nickel-based alloys, the heating temperature of the billet in the first rolling is 1180-1220℃, the total heating time is 1-1.5min / mm thickness, the initial rolling temperature of the plate is ≥1080℃, the final rolling temperature is ≥850℃, and the plate is air-cooled after rolling.
[0014] In the above-mentioned nickel-based alloy fine-grained high-strength rolling method, in step (3), when 5 ≤ compression ratio < 7, the heating temperature of the intermediate billet is 1130-1150℃; when 7 ≤ compression ratio < 9, the heating temperature of the intermediate billet is 1160-1180℃; when the compression ratio ≥ 9, the heating temperature of the intermediate billet is 1200-1230℃.
[0015] In the above-mentioned fine-grained high-strength rolling method for nickel-based alloys, the total heating time for the second rolling process is 1-1.5 min / mm.
[0016] In the above-mentioned fine-grained high-strength rolling method for nickel-based alloys, the final rolling temperature of the second heat rolling is ≥850℃.
[0017] In the above-mentioned fine-grained high-strength rolling method for nickel-based alloys, the annealing temperature of the finished plate is 950-990℃, and the holding time is 2-5 min / mm thickness.
[0018] On the other hand, the present invention provides a nickel-based alloy sheet, which is rolled using the above-mentioned nickel-based alloy fine-grained high-strength rolling method.
[0019] The aforementioned nickel-based alloy sheet includes N06625 alloy, N10276, or N07718.
[0020] The technical solution of the present invention has the following beneficial effects:
[0021] (1) The nickel-based alloy fine-grained high-strength rolling method of the present invention provides different original billet microstructure states according to different compression ratios. The rolling process can make the finished plate microstructure undergo sufficient dynamic recrystallization, resulting in fine and uniform grains, which provides good microstructure conditions for subsequent plate annealing heat treatment.
[0022] (2) The nickel-based alloy is rolled according to the rolling method of the present invention, and the grain size of the plate after annealing is ≥7. Figure 1 ), to achieve high enhancement. Attached Figure Description
[0023] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the invention.
[0024] Figure 1 The finished product after annealing has a fine and uniform grain structure (grain size 7-8). Detailed Implementation
[0025] To fully understand the purpose, features, and effects of this invention, the following detailed embodiments are provided. Except as described below, the process methods of this invention employ conventional methods or apparatus in the art. Unless otherwise specified, the terms and expressions used below have the meanings commonly understood by those skilled in the art.
[0026] The terms “first,” “second,” etc., used herein do not indicate any order or importance, but are used to distinguish one element from another. The terms “the,” “the,” “an,” and “a” do not indicate a limitation of quantity, but rather indicate the presence of at least one of the mentioned objects. The terms “preferred,” “more preferred,” etc., refer to embodiments of the invention that, in certain circumstances, provide certain beneficial effects. However, other embodiments may also be preferred in the same or other circumstances. Furthermore, the description of one or more embodiments does not imply that other embodiments are unavailable, nor is it intended to exclude other embodiments from the scope of the invention.
[0027] Specifically, the nickel-based alloy fine-grained high-strength rolling method provided by the present invention includes:
[0028] Preparation of slabs
[0029] The alloy is smelted in a vacuum induction furnace or electric furnace, and then slabs are obtained by continuous casting or ingot casting.
[0030] Optionally, the slab material is N06625, and the standard composition control range is (wt%):
[0031]
[0032] The ingredient control standards refer to ASME SB-443 or ASME SB-446.
[0033] Homogenization heat treatment
[0034] By homogenizing the billet through heat treatment, defects such as element segregation can be effectively eliminated.
[0035] Preferably, the homogenization heat treatment is performed at a temperature of 1200-1250℃ for a holding time of 48-72 hours.
[0036] Preferably, the homogenization heat treatment is performed using a gas-fired furnace or an electric furnace.
[0037] First rolling
[0038] The billet is subjected to a first rolling process to obtain an intermediate billet.
[0039] The billet heating temperature is 1180-1220℃, and the total heating time is considered based on a billet thickness of 1-1.5 min / mm. The initial rolling temperature of the plate is ≥1080℃, the final rolling temperature is ≥850℃, and it is air-cooled after rolling.
[0040] The principle for determining the thickness of the billet in the first rolling mill is as follows: Based on the thickness of the finished plate, the size of the intermediate billet is reasonably designed to ensure that the compression ratio of the finished product in the second rolling mill is ≥5.
[0041] The first rolling process transforms the coarse cast structure in the slab into a rolled structure, significantly improving the plasticity of the billet.
[0042] After the first rolling, the surface of the billet is ground to ensure that there are no cracks or defects before the second rolling of the finished plate can be carried out.
[0043] Second rolling
[0044] Because cast nickel-based alloy billets have a coarse microstructure and low thermoplasticity, they cannot be rolled into sheets in a single operation. Therefore, a two-stage rolling process is required to produce the finished product.
[0045] In particular, the heating temperature of the second rolling process increases with the increase of the compression ratio.
[0046] Since the grain size of the finished plate is closely related to the rolling compression ratio and the billet heating temperature, the billet heating temperature is determined according to the following principles: when 5 ≤ compression ratio < 7, the heating temperature of the intermediate billet is 1130-1150℃; when 7 ≤ compression ratio < 9, the heating temperature of the intermediate billet is 1160-1180℃; when the compression ratio ≥ 9, the heating temperature of the intermediate billet is 1200-1230℃.
[0047] Preferably, the total heating time for the second rolling is 1.0-1.5 min / mm, and the final rolling temperature is ≥850℃.
[0048] The billet heating temperature and compression ratio have a significant impact on grain size. When the compression ratio is relatively low, the billet should be heated at a low temperature to prevent the grain structure from becoming too coarse before rolling. This would prevent the grain refinement from being fully achieved through dynamic recrystallization due to the compression ratio limitation. When the compression ratio is high, the billet rolling time is long and there are many rolling passes. If low-temperature heating is still used, the temperature drop during rolling will prevent effective rolling to the final product dimensions. Therefore, high-temperature heating is necessary. Although the billet structure is relatively coarse before high-temperature heating, the high compression ratio allows for complete dynamic recrystallization to refine the grains.
[0049] Based on the above control principles, different original billet microstructures are provided according to different compression ratios. The rolling process allows for full dynamic recrystallization of the finished plate microstructure, resulting in fine and uniform grains, which provides good microstructure conditions for subsequent plate annealing heat treatment.
[0050] Finished board annealing
[0051] Preferably, the annealing temperature of the finished plate is 950-990℃, and the holding time is 2-5 min / mm thickness.
[0052] On the other hand, the present invention also provides a nickel-based alloy sheet, which is rolled using the above-mentioned nickel-based alloy fine-grained high-strength rolling method.
[0053] The nickel-based alloy plates are N06625 alloy, N10276, N07718, etc.
[0054] In practice, nickel-based alloy plates prepared according to the method of this invention have a grain size ≥ 7 after annealing, achieving high strength.
[0055] Example
[0056] The present invention is further illustrated below by way of embodiments, but the invention is not limited to the scope of the embodiments described herein. Experimental methods in the following embodiments, unless otherwise specified, are performed according to conventional methods and conditions.
[0057] The alloy used in Examples 1-3 and Comparative Examples 1-3 was N06625, and the controlled composition content was as follows (wt%).
[0058]
[0059]
[0060] Example 1
[0061] N06625 alloy was smelted using a vacuum induction furnace. The composition is shown in the table above. Homogenization temperature was 1230℃, and holding time was 58 hours to obtain slabs with a thickness of 250mm. The finished slab thickness was 10mm. The first rolling process involved heating at 1200℃ for 250 minutes, followed by further rolling after removal from the furnace. The initial rolling temperature was 1100℃, and the final rolling temperature was 890℃, resulting in an intermediate slab thickness of 68mm. The second rolling process involved a compression ratio of 6.8, with the billet heating temperature at 1150℃ for 102 minutes and a final rolling temperature of 880℃. The final finished slab dimensions were 10*1500*6000mm. The annealing temperature was 980℃, holding time was 30 minutes, and the slab was water-cooled.
[0062] The measured grain size of the sheet is 7.5, the yield strength Rp0.2 = 480 MPa, the tensile strength Rm = 880 MPa, and the elongation is 55%.
[0063] Example 2
[0064] N06625 alloy was smelted using an electric furnace, with the composition shown in the table above. Homogenization was carried out at 1230℃ for 50 hours to obtain slabs with a thickness of 180mm. The finished slab thickness was 15mm. The first rolling process involved heating at 1200℃ for 180 minutes, followed by further rolling at 1090℃ and 880℃, resulting in an intermediate slab thickness of 120mm. The second rolling process involved a compression ratio of 8, with the billet heating at 1180℃ for 180 minutes and a final rolling temperature of 890℃, producing a final slab size of 15*1600*6000mm. The annealing temperature was 990℃ for 45 minutes, followed by water cooling.
[0065] The measured grain size of the sheet is grade 8, the yield strength Rp0.2 = 506 MPa, the tensile strength Rm = 914 MPa, and the elongation is 53%.
[0066] Example 3
[0067] N06625 alloy was smelted using an electric furnace, with the composition shown in the table above. Homogenization was carried out at 1230℃ for 50 hours to obtain slabs with a thickness of 180mm. The finished slab thickness was 12mm. The first rolling process involved heating at 1200℃ for 180 minutes, followed by further rolling after exiting the furnace. The initial rolling temperature was 1090℃, and the final rolling temperature was 880℃, resulting in an intermediate slab thickness of 120mm. The second rolling process involved a compression ratio of 10, with the billet heating temperature at 1220℃ for 180 minutes and a final rolling temperature of 870℃. The final finished slab dimensions were 12*1500*8000mm. The annealing temperature was 980℃, the holding time was 36 minutes, and the slab was water-cooled.
[0068] The measured grain size of the sheet is grade 9, the yield strength Rp0.2 = 531 MPa, the tensile strength Rm = 937 MPa, and the elongation is 49%.
[0069] Comparative Example 1
[0070] N06625 alloy was smelted using a vacuum induction furnace, with the composition shown in the table above. Homogenization was carried out at 1230℃ for 58 hours to obtain slabs with a thickness of 250mm. The finished slab thickness was 10mm. The first rolling process involved heating at 1200℃ for 250 minutes, followed by further rolling after removal from the furnace. The initial rolling temperature was 1100℃, and the final rolling temperature was 890℃, resulting in an intermediate slab thickness of 68mm. The second rolling process involved heating the slab at 1200℃ for 102 minutes, with a final rolling temperature of 890℃. The final finished slab dimensions were 10*1500*6000mm. The annealing temperature was 980℃, holding time was 30 minutes, and the slab was water-cooled.
[0071] The measured grain size of the sheet is 5.5, the yield strength Rp0.2 = 380 MPa, the tensile strength Rm = 810 MPa, and the elongation is 54%.
[0072] Comparative Example 2
[0073] N06625 alloy was smelted using an electric furnace, with the composition shown in the table above. Homogenization was carried out at 1230℃ for 50 hours to obtain slabs with a thickness of 180mm. The finished slab thickness was 15mm. The first rolling process involved heating at 1200℃ for 180 minutes, followed by further rolling after exiting the furnace. The initial rolling temperature was 1090℃, and the final rolling temperature was 880℃, resulting in an intermediate slab thickness of 120mm. The second rolling process involved heating the slab at 1130℃ for 180 minutes, followed by a final rolling temperature of 840℃, producing a final slab size of 15*1600*6000mm. The annealing temperature was 990℃, with a holding time of 45 minutes, followed by water cooling.
[0074] The measured grain size of the sheet is grade 3-7 (some mixed crystals), yield strength Rp0.2 = 410 MPa; tensile strength Rm = 807 MPa, elongation 46%.
[0075] Comparative Example 3
[0076] N06625 alloy was smelted using an electric furnace, with the composition shown in the table above. Homogenization was carried out at 1230℃ for 50 hours to obtain slabs with a thickness of 180mm. The finished slab thickness was 12mm. The first rolling process involved heating at 1200℃ for 180 minutes, followed by further rolling after exiting the furnace. The initial rolling temperature was 1090℃, and the final rolling temperature was 880℃, resulting in an intermediate slab thickness of 120mm. The second rolling process involved heating the slab at 1140℃ for 180 minutes. Due to excessive temperature drop, the target thickness was not achieved, and the final finished slab dimensions were 16*1500*8000mm. The annealing temperature was 980℃, the holding time was 53 minutes, and water cooling was performed.
[0077] The measured grain size of the sheet is grade 5, the yield strength Rp0.2 = 369 MPa, the tensile strength Rm = 798 MPa, and the elongation is 42%.
[0078] The present invention has been disclosed above with reference to preferred embodiments. However, those skilled in the art should understand that these embodiments are merely illustrative of the invention and should not be construed as limiting its scope. It should be noted that any variations and substitutions equivalent to these embodiments should be considered to be covered within the scope of the claims. Therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.
Claims
1. A fine-grained high-strength rolling method for a nickel-based alloy, characterized by, include: (1) Homogenize the slab material with heat treatment; (2) The slab is subjected to a first rolling process to obtain an intermediate slab; The thickness of the intermediate billet is determined based on the thickness of the finished plate to ensure that the compression ratio of the second rolling is ≥5. (3) The intermediate billet is subjected to a second rolling process to obtain the finished plate; Wherein, when 5 ≤ compression ratio < 7, the heating temperature of the intermediate billet is 1130-1150℃; when 7 ≤ compression ratio < 9, the heating temperature of the intermediate billet is 1160-1180℃; when the compression ratio ≥ 9, the heating temperature of the intermediate billet is 1200-1230℃. (4) Annealing of finished boards; The nickel-based alloy is N06625 alloy.
2. The fine-grained high-strength rolling method of a nickel-based alloy according to claim 1, characterized by, The slab material is smelted in a vacuum induction furnace or electric furnace, and then obtained by continuous casting or ingot casting.
3. The fine-grained high-strength rolling method of a nickel-based alloy according to claim 1, characterized by, The homogenization heat treatment is performed at a temperature of 1200-1250℃ for a heating time of 48-72 hours.
4. The fine-grained high-strength rolling method of a nickel-based alloy according to claim 1, characterized by, The heating temperature of the slab in the first rolling is 1180-1220℃, the total heating time is 1-1.5min / mm thickness, the initial rolling temperature of the slab is ≥1080℃, the final rolling temperature is ≥850℃, and it is air-cooled after rolling.
5. The fine-grained high-strength rolling process for a nickel-based alloy according to claim 1, characterized in that, The total heating time for the second rolling process is 1-1.5 min / mm thickness.
6. The fine-grained high-strengthened rolling method of a nickel-based alloy according to claim 1 or 5, characterized in that, The final rolling temperature of the second rolling process is ≥850℃.
7. The fine-grained high-strength rolling method of a nickel-based alloy according to claim 1, characterized by, The annealing temperature of the finished plate is 950-990℃, and the holding time is 2-5 min / mm thickness.
8. A nickel-base alloy plate, characterized by, The nickel-based alloy fine-grained high-strength rolling method according to any one of claims 1-7 is used for rolling.
Citation Information
Patent Citations
Nickel-based alloy plate rolling method
CN112496037A