A paeonol liposome-loaded nanofiber membrane and its preparation method and application
Through the preparation method of paeonol liposome-loaded nanofiber membrane, soybean lecithin, cholesterol and paeonol are mixed in ethanol, combined with carboxymethyl chitosan, to solve the problem of insufficient food preservation ability of existing packaging materials. , achieving efficient and safe food preservation effects.
Patent Information
- Application Number
- CN202410598054.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-15
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-05-15
AI Technical Summary
Existing sustainable packaging materials have limited ability to preserve food, and it is difficult to extend the shelf life of food. At the same time, there are safety and degradability issues.
The paeonol liposome-loaded nanofiber membrane was prepared by mixing soybean phospholipids, cholesterol and paeonol in ethanol, combined with carboxymethyl chitosan, and using microfluidic technology to package paeonol and pass it through Nanofiber membranes are prepared by electrospinning technology to form nanofiber membranes with high encapsulation efficiency, sustained release performance and thermal stability.
It achieves efficient encapsulation and sustained release of paeonol, extending the shelf life of food. It is also highly safe and biodegradable, and is suitable for the field of food preservation.
Smart Images

Figure CN118166484B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of food packaging materials, and in particular to a paeonol liposome-loaded nanofiber membrane and a preparation method and application thereof. Background Art
[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Most plastic products are not easy to degrade. Long-term accumulation in the natural environment becomes "white pollution", causing great harm to the ecosystem. Sustainable packaging materials can solve the "white pollution" problem from the source. The current sustainable packaging materials have relatively single functions and limited ability to preserve food. Therefore, how to provide a packaging material that can extend the shelf life of food and is safe and degradable is an urgent problem to be solved. Summary of the invention
[0004] In view of this, the present invention provides a paeonol liposome-loaded nanofiber membrane and a preparation method and application thereof. The provided paeonol liposome-loaded nanofiber membrane can fully exert the bioavailability of paeonol and extend the shelf life of food. At the same time, it is highly safe and biodegradable.
[0005] In a first aspect, the present invention provides a method for preparing a paeonol liposome-loaded nanofiber membrane, comprising the following steps:
[0006] Soybean lecithin, cholesterol and paeonol are mixed in ethanol as an alcohol phase; carboxymethyl chitosan is dissolved in water as an aqueous phase, and the alcohol phase and the aqueous phase are pumped into a microfluidic chip at a flow rate ratio of 1:(2-4) to mix, thereby obtaining a paeonol lipid suspension;
[0007] The paeonol liposome suspension is stirred and mixed with a mixed solution of polyvinyl alcohol, chitosan and acetic acid, and then allowed to stand after ultrasonic treatment to obtain a spinning solution;
[0008] The spinning solution is subjected to electrostatic spinning to obtain the product.
[0009] Preferably, in the alcohol phase, the concentration of soybean lecithin is 13-17 mg / mL, the mass ratio of soybean lecithin to cholesterol is (4-6):1, and the concentration of paeonol is 1-2 mg / mL; in the aqueous phase, the concentration of carboxymethyl chitosan is 5-7 mg / mL.
[0010] Furthermore, the concentration of the soybean lecithin is 15-16 mg / mL, the mass ratio of the soybean lecithin to cholesterol is (4-5):1, and the concentration of carboxymethyl chitosan is 6-7 mg / mL.
[0011] Preferably, the total flow rate of the alcohol phase and the aqueous phase is 1100-1300 μL / min; and the flow rate ratio of the alcohol phase to the aqueous phase is 1:3.
[0012] Preferably, in the mixed solution of polyvinyl alcohol, chitosan and acetic acid, the concentration of chitosan is 3-5 mg / mL, the concentration of polyvinyl alcohol is 7-10 wt %, and the concentration of acetic acid is 0.5-2 wt %.
[0013] Preferably, the volume ratio of the paeonol liposome suspension to the mixed solution of polyvinyl alcohol, chitosan and acetic acid is 1:(1-3).
[0014] Preferably, the stirring time is 5 to 10 h; the ultrasonic time is 50 to 70 min; and the standing time is 10 to 20 h.
[0015] Preferably, the electrospinning rate is 0.08-0.12 mm / min, the collection speed is 70-90 r / min, and the jet distance is 13-17 cm.
[0016] Preferably, during the electrospinning process, the temperature is 25-30° C. and the humidity is 45-55%.
[0017] In a second aspect, the present invention provides a paeonol liposome-loaded nanofiber membrane prepared by the above-mentioned preparation method.
[0018] In a third aspect, the present invention provides an application of the paeonol liposome-loaded nanofiber membrane in the field of food preservation.
[0019] Compared with the prior art, the present invention has achieved the following beneficial effects:
[0020] The preparation method of the paeonol liposome-loaded nanofiber membrane provided by the present invention is simple and easy, and can achieve a high encapsulation rate and a high utilization rate of paeonol. The prepared paeonol liposome-loaded nanofiber membrane has high safety and good sustained-release performance, thermal stability and biodegradability, and can extend the shelf life of food, thus having broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute an improper limitation of the present invention. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0022] Figure 1 The liposome encapsulation efficiency (left) and particle size (right) of Examples 1 to 3 of the present invention and Comparative Examples 2 to 3;
[0023] Figure 2 The liposome encapsulation efficiency (left) and particle size (right) of Examples 1, 4-5 and Comparative Examples 4-5 of the present invention;
[0024] Figure 3 The liposome encapsulation efficiency (left) and particle size (right) of Examples 1, 6-7 and Comparative Examples 6-7 of the present invention;
[0025] Figure 4 is the Fourier transform infrared analysis diagram of the liposomes of Example 1 of the present invention and Comparative Example 1;
[0026] Figure 5 This is a TEM measurement image of the liposomes of Example 1 of the present invention;
[0027] Figure 6 are the in vitro release curves of the PAE of the present invention, the CMCS-PAE-LPs of Example 1, and the PAE-LPs of Comparative Example 1;
[0028] Figure 7 is a particle size distribution diagram (a) and a Zeta potential diagram (b) of CMCS-PAE-LPs prepared in Example 1 of the present invention;
[0029] Figure 8 The salt stability of PAE-LPs of Comparative Example 1 of the present invention and CMCS-PAE-LPs of Example 1 is measured: the effect of ionic strength on particle size (a) and the effect of ionic strength on PDI (b); wherein the bar graphs in a and b represent NaCl solutions of different concentrations (0 mM, 200 mM, 400 mM, 600 mM and 800 mM);
[0030] Fig. 9 The salt stability determination of the PAE-LPs of Comparative Example 1 of the present invention and the CMCS-PAE-LPs of Example 1: the effect of ionic strength on Zeta potential (a) and the effect of ionic strength on appearance (b); wherein the bar graph in a represents NaCl solutions of different concentrations (0 mM, 200 mM, 400 mM, 600 mM and 800 mM);
[0031] Fig.10 The pH stability of PAE-LPs of Comparative Example 1 of the present invention and CMCS-PAE-LPs of Example 1 is measured: the effect of pH on particle size (a) and the effect of pH on PDI (b);
[0032] Fig.11 The pH stability of the PAE-LPs of Comparative Example 1 of the present invention and the CMCS-PAE-LPs of Example 1 is measured: the effect of pH on Zeta potential (a) and the effect of pH on appearance (b);
[0033] Fig.12 The thermal stability of the PAE-LPs of Comparative Example 1 of the present invention and the CMCS-PAE-LPs of Example 1 at 80°C for different time periods;
[0034] Fig.13 FTIR measurement of CMCS-PAE-LPs / PVA-CS NFs of Example 1 of the present invention and PVA-CS NFs of Comparative Example 8;
[0035] Fig.14 It is the TGA measurement of PVA-CS NFs of Comparative Example 8 of the present invention and CMCS-PAE-LPs / PVA-CS NFs of Example 1;
[0036] Fig.15 It is the DSC measurement of PVA-CS NFs of Comparative Example 8 of the present invention and CMCS-PAE-LPs / PVA-CS NFs of Example 1;
[0037] Fig.16 The surface morphology and diameter distribution of PVA-CS NFs (a) of Comparative Example 8 of the present invention and CMCS-PAE-LPs / PVA-CS NFs (b) of Example 1;
[0038] Fig.17 is the release curve of PAE of the present invention from PAE-LPs / PVA-CS NFs of Comparative Example 1 and CMCS-PAE-LPs / PVA-CS NFs of Example 1 into water;
[0039] Fig.18 is the DPPH removal rate of PVA-CS NFs of Comparative Example 8 of the present invention and CMCS-PAE-LPs / PVA-CS NFs of Example 1;
[0040] Fig.19 It is the cytotoxicity test of CMCS-PAE-LPs / PVA-CS NFs of Example 1 of the present invention;
[0041] Fig. 20is the antibacterial activity of the PVA-CS NFs of Comparative Example 8 of the present invention and the CMCS-PAE-LPs / PVA-CS NFs of Example 1;
[0042] Fig.21 It is the strawberry weight loss rate of the control group, the polyvinyl chloride (PVC) group, the PVA-CS NFs treatment group of Comparative Example 8, and the CMCS-PAE-LPs / PVA-CS NFs treatment group of Example 1 in the application examples of the present invention;
[0043] Fig. 22 This is the storage status of strawberries in the control group, polyvinyl chloride (PVC) group, PVA-CS NFs treatment group of Comparative Example 8 and CMCS-PAE-LPs / PVA-CS NFs treatment group of Example 1 within 9 days in the application examples of the present invention. DETAILED DESCRIPTION
[0044] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0045] The present invention provides a method for preparing a paeonol liposome-loaded nanofiber membrane, comprising the following steps:
[0046] Soybean lecithin, cholesterol and paeonol are mixed in ethanol as an alcohol phase; carboxymethyl chitosan is dissolved in water as an aqueous phase, and the alcohol phase and the aqueous phase are pumped into a microfluidic chip at a flow rate ratio of 1:(2-4) to mix, thereby obtaining a paeonol lipid suspension;
[0047] The paeonol liposome suspension is stirred and mixed with a mixed solution of polyvinyl alcohol, chitosan and acetic acid, and then allowed to stand after ultrasonic treatment to obtain a spinning solution;
[0048] The spinning solution is subjected to electrostatic spinning to obtain the product.
[0049] Paeonol, also known as 2-hydroxy-4-methoxyacetophenone, is a component in Chinese medicines such as white peony root and salvia miltiorrhiza. It has been widely used in the field of medicine and beauty products because of its anti-inflammatory, antioxidant, antibacterial and whitening effects. However, paeonol has low water solubility, low stability and volatility at room temperature, and these shortcomings limit the further application of paeonol. In the present invention, paeonol is encapsulated into liposomes by microfluidics technology, and the polymer chain of carboxymethyl chitosan can form a protective film on the surface of paeonol liposomes, which prevents direct contact and aggregation between liposomes as a physical barrier. This physical isolation effect helps to maintain the dispersed state of paeonol liposomes and has good stability. Therefore, the stability of paeonol is enhanced and its encapsulation efficiency is improved by carboxymethyl chitosan. The nanofiber membrane prepared by electrostatic spinning of paeonol liposomes and polyvinyl alcohol / chitosan not only has good biodegradability, but also can stably load paeonol and has a good paeonol sustained-release effect.
[0050] In the present invention, in the alcohol phase, the concentration of soybean lecithin is 13-17 mg / mL, the mass ratio of soybean lecithin to cholesterol is (4-6):1, and the concentration of paeonol is 1-2 mg / mL; in the aqueous phase, the concentration of carboxymethyl chitosan is 5-7 mg / mL. The concentrations of soybean lecithin, cholesterol and carboxymethyl chitosan will affect the encapsulation efficiency of paeonol to a certain extent. Under the above conditions, the encapsulation efficiency of paeonol is more than 70%. More preferably, the concentration of soybean lecithin is 15-16 mg / mL, the mass ratio of soybean lecithin to cholesterol is (4-5):1, and the concentration of carboxymethyl chitosan is 6-7 mg / mL.
[0051] In the present invention, the total flow rate of the alcohol phase and the aqueous phase is 1100-1300 μL / min; the flow rate ratio of the alcohol phase to the aqueous phase is 1:3.
[0052] In the present invention, in the mixed solution of polyvinyl alcohol, chitosan and acetic acid, the concentration of chitosan is 3~5mg / mL, the concentration of polyvinyl alcohol is 7~10wt%, and the concentration of acetic acid is 0.5~2wt%. The addition of acetic acid can promote the dissolution of chitosan, and chitosan provides a positive potential, so that the liposome suspension and the polyvinyl alcohol / chitosan solution are stably combined through electrostatic interaction, and polyvinyl alcohol is the main membrane material of the nanofiber membrane. The present invention does not impose any special restrictions on the preparation method of the mixed solution of polyvinyl alcohol, chitosan and acetic acid. The present invention preferably adds chitosan to the mixed aqueous solution of polyvinyl alcohol and acetic acid, and stirs at 80~95°C for 1~4 h to ensure that the chitosan is fully dissolved.
[0053] In the present invention, the volume ratio of the paeonol liposome suspension to the mixed solution of polyvinyl alcohol, chitosan and acetic acid is 1:(1-3), preferably 1:2.
[0054] In the present invention, in order to make the paeonol liposome suspension and the mixed solution of polyvinyl alcohol, chitosan and acetic acid better mixed, the stirring time is 5 to 10 hours. In order to remove bubbles in the spinning solution and avoid introducing defects in the nanofiber membrane, the present invention performs ultrasonic treatment after mixing, and the ultrasonic time is 50 to 70 minutes. Standing after ultrasound is to dissipate the bubbles, and the standing time is 10 to 20 hours.
[0055] In the present invention, the electrospinning rate is 0.08-0.12 mm / min, the collection speed is 70-90 r / min, and the jet distance is 13-17 cm. During the electrospinning process, the temperature is 25-30°C and the humidity is 45-55%. Keeping the parameters stable during the electrospinning process is conducive to preparing a nanofiber membrane with stable and uniform performance.
[0056] The present invention also provides a paeonol liposome-loaded nanofiber membrane prepared by the above-mentioned preparation method, which has high safety, good sustained-release performance, stability and biodegradability.
[0057] The present invention also provides an application of the paeonol liposome-loaded nanofiber membrane in the field of food preservation. For example, the paeonol liposome-loaded nanofiber membrane can be made into a food preservation bag or a preservation film. The present invention does not impose any special restrictions on this specific application form. The paeonol liposome-loaded nanofiber membrane can significantly extend the shelf life of food and has a good application effect.
[0058] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0059] Example 1
[0060] This embodiment provides a method for preparing a paeonol liposome-loaded nanofiber membrane.
[0061] (1) Dissolve 225 mg soybean lecithin (i.e., concentration of 15 mg / mL), 45 mg cholesterol (i.e., the mass ratio of soybean lecithin to cholesterol is 5:1), and 22.5 mg paeonol (PAE) in 15 mL of ethanol to obtain an alcohol phase; dissolve 90 mg carboxymethyl chitosan (CMCS) in 15 mL of water (i.e., concentration of 6 mg / mL) to obtain an aqueous phase; the alcohol phase and the aqueous phase are pumped into a microfluidic chip at a flow rate ratio of 1:3 and a total flow rate of 1200 μL / min for mixing to prepare paeonol liposome suspension CMCS-PAE-LPs.
[0062] (2) 0.04 g of chitosan (CS) was added to 10 mL of a mixed aqueous solution of 8 wt % polyvinyl alcohol (PVA) and 1 wt % acetic acid, followed by magnetic stirring at 90 °C for 2 h to obtain a PVA-CS mixed solution.
[0063] (3) Mix 5 mL of paeonol liposome suspension CMCS-PAE-LPs and 10 mL of PVA-CS mixed solution evenly, stir continuously for 8 h, ultrasonically treat for 60 min to remove bubbles, and let stand for 12 h to obtain a spinning solution.
[0064] (4) The spinning solution of step (3) was poured into a 10 ml syringe with a 22-gauge needle for electrospinning. During the entire spinning process, the ambient temperature was controlled at 27 ± 2 °C and the relative humidity was maintained at 50 ± 5%. Paeonol liposome-loaded nanofiber membranes (CMCS-PAE-LPs / PVA-CS NFs) were successfully prepared under the conditions of a spinning rate of 0.1 mm / min, a collection speed of 80 r / min, and a spray distance of 15 cm.
[0065] Example 2
[0066] The difference between this embodiment and embodiment 1 is that the added amount of soybean lecithin in this embodiment is 195 mg (ie, the concentration is 13 mg / mL).
[0067] Example 3
[0068] The difference between this embodiment and embodiment 1 is that the added amount of soybean lecithin in this embodiment is 255 mg (ie, the concentration is 17 mg / mL).
[0069] Example 4
[0070] The difference between this embodiment and embodiment 1 is that the added amount of cholesterol in this embodiment is 56.3 mg (ie, the mass ratio of soybean lecithin to cholesterol is 4:1).
[0071] Example 5
[0072] The difference between this embodiment and embodiment 1 is that the added amount of cholesterol in this embodiment is 37.5 mg (ie, the mass ratio of soybean lecithin to cholesterol is 6:1).
[0073] Example 6
[0074] The difference between this embodiment and embodiment 1 is that the added amount of carboxymethyl chitosan in this embodiment is 75 mg (ie, the concentration is 5 mg / mL).
[0075] Example 7
[0076] The difference between this embodiment and embodiment 1 is that the added amount of carboxymethyl chitosan in this embodiment is 105 mg (ie, the concentration is 7 mg / mL).
[0077] Comparative Example 1
[0078] The difference between this comparative example and Example 1 is that this comparative example does not contain carboxymethyl chitosan, and finally obtains paeonol liposome suspension (denoted as PAE-LPs) and paeonol liposome loaded nanofiber membrane, denoted as PAE-LPs / PVA-CSNFs.
[0079] Comparative Example 2
[0080] The difference between this comparative example and Example 1 is that the added amount of soybean lecithin in this comparative example is 195 mg (ie, the concentration is 11 mg / mL).
[0081] Comparative Example 3
[0082] The difference between this comparative example and Example 1 is that the added amount of soybean lecithin in this comparative example is 255 mg (ie, the concentration is 19 mg / mL).
[0083] Comparative Example 4
[0084] The difference between this comparative example and Example 1 is that the added amount of cholesterol in this comparative example is 75 mg (ie, the mass ratio of soybean lecithin to cholesterol is 3:1).
[0085] Comparative Example 5
[0086] The difference between this comparative example and Example 1 is that the added amount of cholesterol in this comparative example is 37.5 mg (ie, the mass ratio of soybean lecithin to cholesterol is 7:1).
[0087] Comparative Example 6
[0088] The difference between this comparative example and Example 1 is that the added amount of carboxymethyl chitosan in this comparative example is 60 mg (ie, the concentration is 4 mg / mL).
[0089] Comparative Example 7
[0090] The difference between this comparative example and Example 1 is that the added amount of carboxymethyl chitosan in this comparative example is 120 mg (ie, the concentration is 8 mg / mL).
[0091] Comparative Example 8
[0092] Compared with Example 1, this comparative example is different in that this comparative example does not contain the preparation of paeonol liposome suspension (CMCS-PAE-LPs), and the specific steps are as follows:
[0093] (1) 0.04 g of chitosan was added to 10 mL of 8 wt % PVA and acetic acid mixed solution, followed by magnetic stirring at 90 °C for 2 h to obtain a PVA-CS mixed solution.
[0094] (2) Ultrasonic treatment was performed for 60 min to remove bubbles, and the solution was allowed to stand for 12 h to obtain a spinning solution.
[0095] (3) The spinning solution of step (2) was poured into a 10 ml syringe with a 22-gauge needle for electrospinning. During the entire spinning process, the ambient temperature was controlled at 27 ± 2 °C and the relative humidity was maintained at 50 ± 5%. Polyvinyl alcohol / chitosan nanofiber membranes (PVA-CS NFs) were successfully prepared under the conditions of a spinning rate of 0.1 mm / min, a collection speed of 80 r / min, and a spray distance of 15 cm.
[0096] Test example
[0097] 1. Determination of paeonol encapsulation efficiency and liposome particle size
[0098] The encapsulation efficiency (EE) of the liposome suspensions of Examples 1 to 7 and Comparative Examples 1 to 7 was measured using the following test method:
[0099] Mix 1 mL of liposome suspension, 3 mL of methanol and 6 mL of ultrapure water, sonicate for 30 min, and centrifuge for 15 min at 22°C and 10,000 r / min. Collect the supernatant and measure it using an ultraviolet spectrophotometer (UV-1900). Place 5 mL of liposome suspension in a pre-activated dialysis bag and dialyze for 12 h. Repeat the above procedure and measure the absorbance of the dialyzed solution. Calculate the total drug and free drug content using the absorbance standard curve. The values are calculated according to the following equations.
[0100]
[0101] Where: C total is the total amount of drug, mg / mL; C free is the amount of free drug, mg / mL.
[0102] The particle size and PDI of liposomes were tested using dynamic light scattering (DLS) technology and Zetasizer Nano ZS90 instrument. The specific operation includes: measuring the particle size and PDI of liposome suspension diluted 10 times with ultrapure water at 25°C and 90° light scattering angle. The test results are as follows: Figure 1 , Figure 2 and Figure 3 shown.
[0103] from Figure 1 It can be seen that as the phospholipid concentration increases from 11 mg / mL to 19 mg / mL, the particle size of CMCS-PAE-LPs continues to increase from 110.81 nm to 159.44 nm. The encapsulation efficiency initially increased from 65.59% to 86.78%, and then decreased to 59.22% as the phospholipid concentration further increased. This is attributed to the fact that when the phospholipid concentration increases, the interaction between liposomes is strengthened, which leads to an increase in particle size and an initial increase in encapsulation efficiency. However, once the concentration exceeds a certain critical point, the excessive accumulation of phospholipid molecules in the liposomes and the formation of micelle structures and the restrictions they bring begin to have an adverse effect on the encapsulation efficiency, causing it to decrease. When the phospholipid concentration is 13~17 mg / mL, the encapsulation efficiency can reach more than 70%.
[0104] from Figure 2 As can be seen, the ratio of phospholipids to cholesterol increases from 3:1 to 7:1 ( w : w ), because we reduced the change in ratio, the particle size of CMCS-PAE-LPs did not change much, only increasing from 165.82 nm to 187.31 nm. The encapsulation efficiency of CMCS-PAE-LPs initially increased from 66.19% to 85.68%, but then decreased to 73.8% as the ratio of phospholipid to cholesterol further increased. This is because cholesterol makes the phospholipid molecules compact and improves the orderliness of the liposomes. When the ratio of phospholipid to cholesterol is 4-6:1, the encapsulation efficiency can reach more than 70%.
[0105] from Figure 3 It can be seen that as the CMCS concentration increases from 4 mg / mL to 8 mg / mL, the particle size of CMCS-PAE-LPs changes significantly, from 114.72 nm to 198.37 nm, and the encapsulation efficiency increases from 63.48% to 86.56%. However, as the concentration increases further, the encapsulation efficiency decreases to 70.38%. The increase in particle size reflects the natural result of CMCS forming a larger complex structure on the surface of liposomes. The initial increase in encapsulation efficiency is due to the fact that CMCS enhances the affinity between liposomes and drugs, while the subsequent decrease is due to excessive accumulation of CMCS, which interferes with the further encapsulation process of paeonol. When the CMCS concentration is 5-7 mg / mL, the encapsulation efficiency can reach more than 70%.
[0106] 2. Liposome Fourier Transform Infrared Analysis (FTIR)
[0107] Paeonol (PAE), empty liposomes without PAE encapsulation (BL-LPs), empty liposomes modified with CMCS but without PAE encapsulation (CMCS-BL-LPs), PAE-LPs of Comparative Example 1, and CMCS-PAE-LPs of Example 1 were analyzed by FT-IR. Figure 4 The FTIR spectrum of PAE mainly includes its special absorption peak at 1915.65 cm -1 and 1620.98 cm -1 , which originates from the carbonyl conjugated system in the molecular structure of paeonol, which is similar to previous reports. The FT-IR spectrum of PAE-LPs is almost the same as that of BL-LPs, and the characteristic -OH stretching (3430.31 cm -1 )、CH absorption peak(2926.41 cm -1 )、ester functional group -COOR(1736 cm -1 ), the characteristic peak of PAE disappeared, proving that PAE has been encapsulated inside the liposomes. The FT-IR spectrum of CMCS-PAE-LPs is almost the same as that of CMCS-BL-LPs, with a peak at 1596.38 cm -1 and 1067.52 cm -1 New characteristic peaks are generated at 1605.44 cm-1, which is related to the asymmetric stretching of -NH2 and -COO-. The peaks of amino and carboxyl groups shift to 1605.44 cm-1, respectively. -1 and 1423.20cm -1 , and its strength was significantly reduced after coating, which may be due to the hydrogen bonding between CMCS and the bilayer. In summary, PAE has been encapsulated by liposomes and CMCS has been deposited on the surface of PAE-LPs, proving that Example 1 has successfully prepared CMCS-PAE-LPs.
[0108] 3. Liposome TEM (transmission electron microscopy) determination
[0109] Figure 5 The TEM observation results revealed that the CMCS-PAE-LPs of Example 1 had a spherical or nearly spherical vesicle morphology. These nanoparticles had a smooth surface, and the overall structure showed good stability, with no damage observed. The particles were of uniform size, approximately 150 nm, evenly distributed, and regular in shape. CMCS-PAE-LPs formed a unique core-shell structure through polysaccharide modification. The TEM results further confirmed the FT-IR results, and CMCS had been deposited on the surface of PAE-LPs.
[0110] 4. In vitro release study of paeonol in liposomes
[0111] The in vitro release of PAE, CMCS-PAE-LPs of Example 1 and PAE-LPs of Comparative Example 1 was measured by dialysis. Accurately take 5 mL of sample and place it in a dialysis bag, immerse the dialysis bag in 50 mL of ultrapure water, and place it on a magnetic stirrer and stir it in a constant temperature dark environment at 25°C. At the set time point, 1 mL of release medium was extracted for measurement and immediately supplemented with 1 mL of ultrapure water to ensure that the total volume of the system remained unchanged. The concentration of the drug in the release medium was determined by a UV spectrophotometer, and the percentage of drug release within a predetermined time period was calculated based on this, and the formula is as follows.
[0112]
[0113] In vitro release curves of PAE-LPs and CMCS-PAE-LPs Figure 6 The results show that the release rate of CMCS-PAE-LPs is significantly slower than that of PAE monomers and PAE-LPs. This phenomenon may contribute to the sustained release of drugs in the target area, thereby improving their target effect. Specifically, in the first 4 h, the release rates of PAE-LPs and CMCS-PAE-LPs were similar, and the release rate of PAE was higher, indicating that under the influence of the lipid membrane, the liposomes had a certain sustained release effect; after 4 h, the release rate of CMCS-PAE-LPs modified with CMCS was significantly lower than that of PAE-LPs; after 48 h of release experiment, only about 69.32% of PAE was released in CMCS-PAE-LPs, while in contrast, the release amount of PAE monomers was about 95.48% and the release amount of PAE-LPs was about 75.36%. This result shows that by encapsulating PAE in liposomes, not only its solubility in aqueous environment is significantly improved, but also the effective control of drug release rate is successfully achieved, thereby prolonging the sustained release time of the drug. This sustained-release effect is mainly due to the physical barrier formed by the phospholipid bilayer of the liposome, which effectively delays the direct interaction between the drug molecules and the external environment and prolongs the release period. In addition, the modification of carboxymethyl chitosan further enhances this sustained-release property, and adds an additional barrier effect through the hydration layer formed on the surface of the liposome, further slowing down the release of the drug.
[0114] 5. Liposome stability determination
[0115] (1) System stability
[0116] After appropriately diluting the CMCS-PAE-LPs prepared in Example 1, we used a laser particle size analyzer to measure its particle size, PDI and Zeta potential, and repeated the measurement three times to ensure the accuracy of the results. Figure 7As shown, the average particle size of the obtained CMCS-PAE-LPs is 123.83±1.514nm (n=3), the PDI value is 0.093±0.013 (n=3), and the Zeta potential is -28.13±1.059mV (n=3). The measurement of Zeta potential reveals the interaction strength between CMCS-PAE-LPs, where a higher Zeta potential indicates their stronger stability in solution. Generally, when the absolute value of the Zeta potential of liposomes exceeds 20 mV, they are considered to be in a stable state. The results of this experiment show that these liposomes exhibit a uniform particle size distribution and obvious electronegativity, which proves the high stability of the system.
[0117] (2) Salt stability
[0118] The ionic stability of the liposome samples was tested in aqueous NaCl solutions of different concentrations (0-800 mM) (25°C, 2 h). The particle size, PDI and Zeta potential of the samples were then measured.
[0119] When NaCl solutions of different concentrations (0-800 mM) were mixed with PAE-LPs of Comparative Example 1 and CMCS-PAE-LPs of Example 1 in equal volumes and left at room temperature for 2 h, Figure 8 As shown in a in Figure 1, it was found that the average particle size of both PAE-LPs and CMCS-PAE-LPs decreased with the increase of NaCl concentration. The particle size of PAE-LPs decreased from 140.51 nm to 98.62 nm, while the particle size of CMCS-PAE-LPs decreased from 165.34 nm to 122.49 nm. This decrease can be explained as the result of osmotic pressure, that is, as salt ions penetrate the phospholipid layer of liposomes, partial loss of internal water is triggered. At the same time, Figure 8 As shown in (b), with the increase of NaCl concentration, the PDI of PAE-LPs and CMCS-PAE-LPs increased. Specifically, the PDI of PAE-LPs increased from 0.152 to 0.252, and that of CMCS-PAE-LPs increased from 0.151 to 0.167. The increase in PDI is attributed to the fact that the ions in NaCl shielded the charges on the surface of the liposomes, thereby reducing the electrostatic repulsion between them. At the same time, the PDI of CMCS-PAE-LPs increased less, indicating that the modification of CMCS enhanced the stability of liposomes in a high salt environment, limited aggregation, and maintained a high uniformity in the particle size distribution. Fig. 9As depicted in a in the figure, with the increase of NaCl concentration, the Zeta potential of PAE-LPs and CMCS-PAE-LPs also changed, from -10.31 mV to -3.18 mV for PAE-LPs and from -31.25 mV to -19.93 mV for CMCS-PAE-LPs. These changes are caused by the interaction between ions and the charged groups on the outer layer of liposomes. As the ion concentration in the solution increases, the charge balance on the surface of the liposomes is affected, thereby changing the Zeta potential of the liposomes. Compared with PAE-LPs, CMCS-PAE-LPs exhibit stronger charge shielding, maintaining the repulsion between liposomes, thereby improving the stability of the system. In appearance, as shown in Figure 2, the Zeta potential of PAE-LPs and CMCS-PAE-LPs is higher than that of PAE-LPs, which can effectively prevent the liposomes from being damaged. Fig. 9 As shown in (b), even at an ionic strength of 800 mM, the CMCS-PAE-LPs solution remained optically transparent without precipitation.
[0120] (3) pH stability
[0121] The effects of different pH conditions on the liposome systems of Comparative Example 1 and Example 1 are shown in Fig.10 a, b and Fig.11 As shown in a and b in the figure. The results show that for PAE-LPs, the particle size is relatively stable in the range of pH 5 to 8, with a small fluctuation between 138.24 nm and 140.51 nm, while the large increase in the PDI value indicates that the particles are aggregated. The Zeta potential gradually decreases from -2.39 mV (pH=5) to -11.52 mV (pH=8), reflecting that the negative value of the liposome surface charge increases with the increase in pH value, which is related to the deprotonation of the functional groups on the liposome surface.
[0122] In contrast, CMCS-PAE-LPs showed a significant increase in particle size under acidic conditions. At a pH of 5, the liposome particle size increased significantly to 212.81 nm, while in an environment of pH 6-8, the particle size changed very little. This is because CMCS is more easily protonated under acidic conditions, which increases the repulsive force between molecules and causes the liposomes to swell. Similar to PAE-LPs, its PDI value varies very little over the entire pH range. Compared with PAE-LPs, the Zeta potential of CMCS-PAE-LPs also shows that the liposomes have a higher negative charge over the entire pH range, which further emphasizes the potential role of the stable negative charge provided by the CMCS modification in maintaining particle stability and preventing aggregation. Appearance Fig.11 As shown in b, the CMCS-PAE-LPs solution remained optically transparent in the pH range of 5-8, and no precipitation was observed.
[0123] (4) Thermal stability
[0124] To evaluate the stability of liposomes at higher temperatures, which is critical for determining their suitability during storage and transportation, thermal stability tests were performed ( Fig.12 , 80°C). The PAE-LPs of Comparative Example 1 and the CMCS-PAE-LPs of Example 1 were kept at 80°C for 60 min. The PAE-LPs monomers leaked rapidly from the dialysis bag, and only 41.25% remained after 60 min. In contrast, the retention rate of PAE in CMCS-PAE-LPs reached 74.76%, indicating that the encapsulation in polysaccharide-modified liposomes effectively maintained its stability under thermal conditions and slowed down the heat-induced drug release.
[0125] 6. FTIR determination of nanofiber membrane
[0126] The FTIR measurements of the CMCS-PAE-LPs / PVA-CS NFs of Example 1 and the polyvinyl alcohol / chitosan nanofiber membrane (PVA-CS NFs) of Comparative Example 8 without CMCS-PAE-LPs are as follows: Fig.13 As shown. At approximately 3328.8 cm -1 At 2940.5 cm, both samples showed a broad -OH band, which is a typical characteristic absorption of hydroxyl groups. -1 and 2912.3 cm -1 We noticed that CMCS-PAE-LPs / PVA-CS NFs showed an enhanced and broader absorption peak compared to PVA-CS NFs without CMCS-PAE-LPs loading. This indicates that although CMCS-PAE-LPs are encapsulated in PVA-CS NFs, their composition still affects the infrared absorption properties of the PVA-CS matrix.
[0127] In addition, the absorption enhancement of the amide I band appears at 1731.6 cm -1 and 1712.3 cm -1 This may be due to the phospholipid components of the liposomes forming a new chemical environment or interaction in the nanofiber matrix. -1 The enhanced absorption at 1325.8 cm indicates that the POC ether bond of phospholipids does exist in CMCS-PAE-LPs / PVA-CS NFs and has an impact on the chemical properties of the matrix. -1 A series of absorption peaks displayed nearby are the symmetric stretching vibration peaks of carboxyl groups, proving that CMCS-PAE-LPs have been combined with PVA-CS NFs.
[0128] Although the nanofiber wrapping may limit the direct detection of specific functional groups of CMCS-PAE-LPs, we are still able to observe obvious changes introduced by CMCS-PAE-LPs from the overall features of the IR spectra, demonstrating the successful loading of CMCS-PAE-LPs in PVA-CS NFs and indicating that their distribution in PVA-CS NFs may have a significant impact on the chemical properties of the nanofibrous membranes.
[0129] 7. TGA determination of nanofiber membrane
[0130] In the TGA test of the PVA-CS NFs of Comparative Example 8 and the CMCS-PAE-LPs / PVA-CS NFs composite material of Example 1 ( Fig.14 ), we found that PVA-CS NFs began to decompose at nearly 280°C. The low residue content of PVA-CS NFs indicated that its carbon layer was insufficiently formed and failed to effectively inhibit further pyrolysis. At the same time, CMCS-PAE-LPs / PVA-CS NFs showed obvious double degradation peaks. After the introduction of CMCS-PAE-LPs, the residual carbon content of the composite material at 600°C was significantly increased to 15.01%, which was higher than that of the sample containing only PVA-CS NFs. This is because of the high carbon content of CMCS-PAE-LPs and the dense carbon layer formed during the pyrolysis process, which effectively blocked the heat transfer. In addition, the addition of CMCS further optimized the thermal stability. Its unique chemical structure promoted the formation of more carbon layers during decomposition, enhancing the material's resistance to high temperatures. Therefore, the combination of PAE-LPs and CMCS significantly enhanced the thermal stability of PVA-CS NFs, providing important performance support for its application in high temperature environments.
[0131] 8. DSC determination of nanofiber membrane
[0132] like Fig.15 As shown in the figure, the CMCS-PAE-LPs / PVA-CS NFs (red curve) of Example 1 exhibited obvious thermal decomposition characteristics at nearly 600°C, and the heat flow dropped to a lower level. In contrast, the heat flow of the PVA-CS NFs of Comparative Example 8 decreased more slowly and stabilized around 700°C, indicating that it had good thermal stability in the same temperature range. This reflects the unique thermal behavior of CMCS-PAE-LPs / PVA-CS NFs during heat treatment, providing important thermal analysis data for material design and high-temperature applications.
[0133] 9. SEM observation of nanofiber membrane
[0134] Fig.16 a in Fig.16The surface morphology and diameter distribution of PVA-CS NFs of Comparative Example 8 and CMCS-PAE-LPs / PVA-CS NFs of Example 1 are presented in b, respectively. PVA-CS NFs exhibit a highly smooth surface and a relatively uniform diameter range, concentrated between 150 and 250 nm. After the introduction of CMCS-PAE-LPs and co-spinning with the PVA-CS NFs matrix, CMCS-PAE-LPs / PVA-CS NFs still maintain a smooth surface and a highly uniform diameter range, and its diameter is mainly distributed in the range of 150-300 nm, which is slightly larger than that of PVA-CS NFs. This increase is partly due to the plasticity and flexibility of CMCS-PAE-LPs at the nanoscale, which enables it to be effectively cross-linked with the PVA-CS NFs matrix and integrated into the fiber. This increase in fiber diameter is not only beneficial for enhancing the mechanical strength of the fibers, but also, considering the application prospects of nanofibers in food packaging, the embedding of CMCS-PAE-LPs will help improve the barrier properties and functionality of packaging materials, such as increasing antibacterial and antioxidant properties and extending the shelf life of food, thereby providing an additional layer of protection for food safety.
[0135] 10. Release behavior analysis of nanofiber membrane
[0136] Fig.17Figure 1 is the release curve of PAE from PAE-LPs / PVA-CS NFs of Comparative Example 1 and CMCS-PAE-LPs / PVA-CSNFs of Example 1 into water. The cumulative release percentage of PAE from PAE-LPs / PVA-CS NFs and CMCS-PAE-LPs / PVA-CS NFs into water increases with time. In the initial 2 h, the drug release rates of the two samples were similar, but as time went on, the release rate of CMCS-PAE-LPs / PVA-CS NFs was relatively slow. Specifically, in the first 8 h, the cumulative release rates of the two samples increased rapidly, and then the growth rate slowed down. The release amount of PAE-LPs / PVA-CS NFs at 8 h reached 54.66%, while the release rate of CMCS-PAE-LPs / PVA-CS NFs at the same time point decreased, releasing only 49.98% at 12 h. At 24 h, the release of PAE-LPs / PVA-CS NFs reached 65.82%, while the release of CMCS-PAE-LPs / PVA-CSNFs was about 58.44%. At 48 h, the release of PAE-LPs / PVA-CS NFs increased slightly and stabilized at about 70.91%, while the release of CMCS-PAE-LPs / PVA-CS NFs was slower, increasing to about 60.74%. The modification of CMCS did increase the barrier properties of the nanofiber membrane and reduce the diffusion rate of PAE, thereby prolonging the release time of the drug. This sustained-release property is very beneficial for systems that want to prolong the duration of drug release.
[0137] 11. DPPH free radical scavenging activity of nanofiber membranes
[0138] The antioxidant properties of PVA-CS NFs of Comparative Example 8 and CMCS-PAE-LPs / PVA-CS NFs of Example 1 were evaluated by the DPPH radical scavenging method. CMCS-PAE-LPs / PVA-CS NFs and PVA-CS NFs were dried and mixed with 5 mL of distilled water. Taking the CS concentration as the standard, the final concentrations of CMCS-PAE-LPs / PVA-CS NFs and PVA-CS NFs after dissolution were 0.2, 0.4, 0.6, 0.8 and 1 mg / mL, respectively. After incubation for 24 h, centrifugation was performed, and the supernatant was then used for free radical scavenging experiments. The experimental steps include mixing 20 μL of the supernatant with 5 mL of DPPH solution dissolved in 95% ethanol, reacting for 30 min at 25°C in the dark, and calculating the scavenging rate of DPPH radicals by measuring the absorbance of the reaction mixture at 517 nm. The formula for calculating the scavenging rate of DPPH radicals is as follows:
[0139]
[0140] Where: A 0——absorbance of control group, L / (g·cm);
[0141] A ——Absorbance of the experimental group, L / (g·cm).
[0142] Results Fig.18 At a concentration of 1 mg / mL, the DPPH scavenging rates of PVA-CS NFs and CMCS-PAE-LPs / PVA-CS NFs were 31.42% and 51.22%, respectively, proving that the latter has better antioxidant properties. This result shows that CMCS-PAE-LPs / PVA-CS NFs, as a food packaging material, can effectively improve the shelf life of food and maintain its freshness.
[0143] 12. Cytotoxicity analysis of nanofiber membranes
[0144] In order to explore the effect of CMCS-PAE-LPs / PVA-CS NFs on cytotoxicity, this study used the MTT assay (3-(4,5-dimethylthiazol-2-yl)-2,5-diphenyltetrazolium bromide method) to evaluate the activity of cells. The specific experimental steps are as follows: First, HFF-1 fibroblasts were cultured at 1.0 × 10 5 cells / mL, 100 μL was injected into each well and seeded in a 96-well plate. Incubate for 18 h to promote cell attachment. Next, the cells were treated with CMCS-PAE-LPs / PVA-CS NFs powder, and the final concentration of the drug was set at 2, 4, 6, 8 and 10 mg / mL, and incubated for 24 h. After incubation, 10 μL of MTT solution (concentration of 5 mg / mL) was added to each well and incubated for another 4 h at 37°C. After removing the MTT solution, 150 μL of DMSO was added to dissolve the purple formazan crystals formed. The absorbance was measured at a wavelength of 490 nm using a microplate reader, and the cell activity was evaluated by comparing the absorbance ratio of each sample with the blank control.
[0145] like Fig.19As shown in the cytotoxicity test conducted in this study, the survival rate of the untreated control group cells was 45.98%, indicating that these cells showed a certain survival ability without drug intervention. In contrast, as the concentration of PAE increased, the cell survival rate was slightly affected. Despite this, the test samples still showed high biocompatibility; even when the PAE concentration was increased to 10 mg / mL, the cell survival rate was still 44.93%. These comparative results emphasize the low toxicity characteristics of CMCS-PAE-LPs / PVA-CS NFs within the tested concentration range, further confirming the safety of CMCS-PAE-LPs / PVA-CS NFs as food packaging materials.
[0146] 13. Antibacterial activity of nanofiber membrane
[0147] The antibacterial activities of the PVA-CS NFs of Comparative Example 8 and the CMCS-PAE-LPs / PVA-CS NFs of Example 1 are shown in Table 1. Fig. 20 As shown in the figure, after 48 h incubation, PVA-CS NFs showed an inhibition zone of 0.25 ± 0.027 mm against E. coli and 0.21 ± 0.028 mm against S. aureus, which is the weak antibacterial activity of chitosan (CS) at a lower concentration. CMCS itself lacks antibacterial activity, and CMCS-PAE-LPs / PVA-CS NFs showed significant inhibition zones of 1.26 ± 0.028 mm and 1.37 ± 0.029 mm against E. coli and S. aureus, respectively, due to the addition of CMCS-PAE-LPs, indicating that PVA-CS NFs, as a carrier of CMCS-PAE-LPs, contributes to the stable release of PAE and enhances the antibacterial activity.
[0148] Application Examples
[0149] In order to evaluate the effect of CMCS-PAE-LPs / PVA-CS NFs of Example 1 on the preservation of strawberries, Dandong 99 strawberries were purchased from Ginza Supermarket, and samples with consistent appearance, the same maturity, and no obvious physical damage and fungal invasion were strictly selected for the experiment.
[0150] The strawberries were randomly assigned to four different experimental groups: a control group, a polyvinyl chloride (PVC) group, a PVA-CS NFs treatment group of Comparative Example 8, and a CMCS-PAE-LPs / PVA-CS NFs treatment group of Example 1. Each experimental group had three replicates, and each replicate contained three strawberries. The strawberries were placed in a 100 mL beaker and subjected to the following treatments: (1) without any coating; (2) sealed with PVC plastic wrap; (3) sealed with PVA-CS NFs; (4) sealed with CMCS-PAE-LPs / PVA-CS NFs. All treated strawberries were placed at room temperature (22 ± 2°C), and the state of the strawberries during the entire shelf life was recorded by a camera, and the weight loss and appearance of the strawberries were recorded and evaluated on the 1st, 3rd, 5th, 7th, and 9th days. The weight loss rate of the strawberries was measured by weighing, and the specific weight loss rate calculation formula is as follows:
[0151]
[0152] Where: W 1——weight of strawberries before storage, g;
[0153] W 2 – Weight of berries after storage for a certain period of time, g.
[0154] like Fig.21 As shown in the figure, different active packaging films have very different effects on the weight loss rate of strawberries. Specifically, the weight loss rate of untreated strawberries is as high as 71.43% within 9 days; the weight loss rate of strawberries treated with PVC NFs reaches 35.18%; the weight loss of strawberries treated with PVA-CS NFs is less in the first 3 days, but then the weight loss rate increases sharply, reaching 67.12% on the 9th day; the strawberries treated with CMCS-PAE-LPs / PVA-CS NFs show the lowest weight loss rate, only 23.19%, indicating that the excellent air permeability and antibacterial properties of CMCS-PAE-LPs / PVA-CS NFs can be continuously released, effectively reducing the weight loss rate, proving its safety and effectiveness as a food active packaging.
[0155] Fig. 22 The image shows the state of strawberries packed with different film materials after 9 days of storage. Fig. 22As shown in the figure, although the strawberries without any membrane material packaging have good air permeability, they began to lose water and grow bacteria after 5 days, which may be caused by the rapid ripening and water loss of strawberries; the PVC group, because it is not air-permeable and water-permeable, lost water on the 3rd day, and had bacterial growth on the 7th day, losing its edible value; the PVA-CS NFs group, which has good water permeability and air permeability, did not lose water, but due to the weak antibacterial activity of low-concentration CS, bacteria grew on the 7th day, losing its edible value; the CMCS-PAE-LPs / PVA-CS NFs group, which has good water permeability and air permeability, and PAE with antibacterial activity is continuously released, did not lose water or bacteria grow on the 9th day. The results show that CMCS-PAE-LPs / PVA-CS NFs packaging can effectively inhibit the corruption of strawberries and delay the aging process, thereby significantly extending the shelf life.
[0156] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a paeonol liposome-loaded nanofiber membrane, characterized in that: The steps include: Soybean lecithin, cholesterol and paeonol are mixed in ethanol as an alcohol phase; carboxymethyl chitosan is dissolved in water as an aqueous phase, and the alcohol phase and the aqueous phase are respectively pumped into a microfluidic chip at a flow rate ratio of 1:(2-4) for mixing to obtain a paeonol liposome suspension; The paeonol liposome suspension is stirred and mixed with a mixed solution of polyvinyl alcohol, chitosan and acetic acid, and then allowed to stand after ultrasonic treatment to obtain a spinning solution; The spinning solution is subjected to electrostatic spinning to obtain; In the alcohol phase, the concentration of soybean lecithin is 13-17 mg / mL, the mass ratio of soybean lecithin to cholesterol is (4-6):1, and the concentration of paeonol is 1-2 mg / mL; in the aqueous phase, the concentration of carboxymethyl chitosan is 5-7 mg / mL; the total flow rate of the alcohol phase and the aqueous phase is 1100-1300 μL / min; In the mixed solution of polyvinyl alcohol, chitosan and acetic acid, the concentration of chitosan is 3-5 mg / mL, the concentration of polyvinyl alcohol is 7-10 wt %, and the concentration of acetic acid is 0.5-2 wt %; The volume ratio of the paeonol liposome suspension to the mixed solution of polyvinyl alcohol, chitosan and acetic acid is 1:(1-3).
2. The preparation method according to claim 1, characterized in that The concentration of the soybean lecithin is 15-16 mg / mL, the mass ratio of the soybean lecithin to cholesterol is (4-5):1, the concentration of carboxymethyl chitosan is 6-7 mg / mL; and the flow rate ratio of the alcohol phase to the water phase is 1:
3.
3. The preparation method according to claim 1, characterized in that: The stirring time is 5 to 10 hours; the ultrasonic time is 50 to 70 minutes; and the standing time is 10 to 20 hours.
4. The preparation method according to claim 1, characterized in that: The electrospinning process has a spinning rate of 0.08-0.12 mm / min, a collection speed of 70-90 r / min, and a jet distance of 13-17 cm.
5. The preparation method according to claim 1, characterized in that: During the electrospinning process, the temperature is 25-30° C. and the humidity is 45-55%.
6. The paeonol liposome-loaded nanofiber membrane prepared by the preparation method according to any one of claims 1 to 5.
7. Use of the paeonol liposome-loaded nanofiber membrane as claimed in claim 6 in the field of food preservation.
Citation Information
Patent Citations
Electrostatic spinning method for preparing nanofiber membrane biosensor
CN103901088A
Micro-fluidic chip manufacturing method based on nanofiber template method
CN106925360A
Preparation method and application of dressing containing astaxanthin
CN114272149A
Methods for managing release of one or more ingredients in an edible composition
US20090175982A1
Composite woven fluidic device
US20180200714A1