A salt-alkali resistant degradable mulch film and preparation method thereof

Through the three-layer structure mulch design and automated production technology, the problem of rapid degradation rate of mulch in saline-alkali land is solved, and the long-term stability and efficient production of mulch in saline-alkali land is achieved, meeting the coating needs of saline-alkali land, and reducing pollution and energy Consumption.

CN118181919BActive Publication Date: 2024-11-05JIANGSU ACAD OF AGRI SCI +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410344576.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-25
Publication Date
2024-11-05
Estimated Expiration
2044-03-25

AI Technical Summary

Technical Problem

In the prior art, the degradation of degradation plastic films used in saline-alkali land are accelerated under high ultraviolet radiation and saline-alkali corrosion conditions, which cannot meet the coating requirements of saline-alkali land. At the same time, the twin-screw granulator is inconvenient to use and cannot effectively utilize the cooling hot air.

Method used

The design of a three-layer structure of plastic film is adopted. The inner layer uses corrosion-resistant materials to enhance the corrosion resistance of the plastic film, the middle layer uses high-barrier materials to slow down moisture evaporation, and the outer layer uses anti-UV agent to enhance the anti-UV performance, combining a twin-screw granulator and cooling and drying The device realizes the automated production of mulch film and the utilization of cooling and hot air.

Benefits of technology

The mulch can maintain an induction period of 180 days in saline-alkali land, meet the use needs of saline-alkali land, reduce pollution and energy consumption, and improve production efficiency and product performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118181919B_ABST
    Figure CN118181919B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of salt-alkali resistant mulch film, specifically a salt-alkali resistant degradable mulch film and a preparation method thereof, which comprises at least one inner layer, wherein the inner layer comprises the following components calculated by weight percentage: 5-50 parts of corrosion-resistant additives, 40-90 parts of PBAT, 0.1-10 parts of epoxy chain extender ADR4468, 0.1-10 parts of plasticizer epoxy soybean oil, 0.1-10 parts of coupling agent, 0.1-10 parts of nucleating agent, and 0.1-10 parts of anti-hydrolysis agent. The present invention uses the synergistic effect of co-extruded film to make the mulch film not only able to resist high ultraviolet radiation, but also able to withstand the erosion of salt and alkali, and the longest induction period in saline-alkali land can reach 180 days, meeting the use requirements of saline-alkali land.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of salt-alkali resistant mulch films, in particular to a salt-alkali resistant degradable mulch film and a preparation method thereof. Background Art

[0002] In the context of increasing global food demand, making full use of saline-alkali land will provide important support for my country to achieve food security and sustainable agricultural development. my country has about 500 million mu of various types of available saline-alkali land resources. How to turn these saline-alkali land resources into treasure is a huge challenge facing my country. There are many reasons for the formation of saline-alkali land, among which precipitation and ground evaporation intensity are most closely related to soil salinization. Evaporation brings up salt from groundwater and accumulates it in the surface soil. At the same time, soil salt is difficult to discharge. Long-term accumulation and concentration form salinized and alkaline soil.

[0003] At present, the main methods for improving saline-alkali land include physical tillage, chemical improvement, and cultivation of salt-alkali-tolerant crops. Although tillage and application of improvers can temporarily reduce the salinity of the surface, it requires a lot of manpower and material resources, and it only treats the symptoms and not the root cause. Cultivating salt-alkali-tolerant crops requires a long period and a lot of research and development investment, and there is currently no widely planted salt-alkali-tolerant crop that has been promoted and applied. In recent years, mulching on saline-alkali land has gradually been recognized by researchers because the mulch has the effect of retaining water and moisture, which can effectively inhibit the evaporation of water, thereby slowing down the accumulation of salt on the surface of the saline-alkali land and achieving the effect of improving the saline-alkali land. However, ordinary PE mulch is difficult to be completely decomposed when used in saline-alkali land, resulting in a significant increase in the content of microplastics in the soil, causing secondary pollution. Therefore, the use of degradable mulch has become an effective means.

[0004] However, in the prior art, there is no relevant degradable mulch that can meet the requirements of saline-alkali land. Because saline-alkali land is not only exposed to high ultraviolet radiation, but also exposed to corrosion of saline-alkali land, the degradation rate of ordinary degradable mulch is accelerated in saline-alkali land, which cannot meet the use requirements. In addition, the existing twin-screw granulator is not convenient for users to use, and the hot air generated by cooling cannot be effectively utilized during use. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a salt-alkali resistant and degradable ground film which is resistant to salt-alkali corrosion, high ultraviolet radiation, and can effectively inhibit the evaporation of water and slow down the accumulation of salt on the surface of saline-alkali land, thereby achieving the goal of improving saline-alkali land.

[0006] In order to solve the problems existing in the prior art, the present invention adopts the following technical solutions:

[0007] A salt-alkali resistant and degradable mulch film comprises at least one inner layer, wherein the inner layer comprises the following components calculated by weight percentage: 5-50 parts of a corrosion resistant additive, 40-90 parts of PBAT, 0.1-10 parts of an epoxy chain extender ADR4468, 0.1-10 parts of a plasticizer epoxy soybean oil, 0.1-10 parts of a coupling agent, 0.1-10 parts of a nucleating agent, and 0.1-10 parts of an anti-hydrolysis agent.

[0008] The above-mentioned salt-alkali resistant degradable mulch film also includes a middle layer, the weight ratio of the inner layer to the middle layer is 1-10:1-10, and the middle layer includes the following components calculated by weight percentage: 30-50 parts of PBAT, 0-30 parts of PHA, 0-30 parts of PGA, 0-30 parts of PCL, 0-30 parts of PPC, 0-80 parts of PBST, 0.1-10 parts of compatibilizer HP441, 0.1-10 parts of nucleating agent, 0.1-10 parts of epoxy chain extender ADR4468, 0.1-10 parts of plasticizer epoxy soybean oil, and 0.1-10 parts of anti-hydrolysis agent.

[0009] The above-mentioned salt-alkali resistant degradable mulch film also includes an outer layer, the weight ratio of the inner layer to the outer layer is 1-10:1-10, and the outer layer includes the following components calculated by weight percentage: 50-90 parts of PBAT, 10-30 parts of PLA, 0.1-10 parts of epoxy chain extender ADR4468, 0.1-10 parts of plasticizer epoxy soybean oil, 0.1-10 parts of coupling agent, 0.1-10 parts of nucleating agent, 0.1-10 parts of anti-hydrolysis agent, 0.1-10 parts of antioxidant, 0.1-10 parts of anti-ultraviolet agent, 10-30 parts of straw, and 1-10 parts of degradable black masterbatch.

[0010] The above-mentioned salt-alkali resistant degradable mulch film also includes a middle layer and an outer layer, the weight ratio of the inner layer, the middle layer and the outer layer is 1-10:1-10:1-10, the middle layer includes the following components calculated by weight percentage: 30-50 parts of PBAT, 0-30 parts of PHA, 0-30 parts of PGA, 0-30 parts of PCL, 0-30 parts of PPC, 0-80 parts of PBST, 0.1-10 parts of compatibilizer HP441, 0.1-10 parts of nucleating agent, 0.1-10 parts of epoxy chain extender ADR4468, 0.1-10 parts of plasticizer epoxidized soybean oil, and 0.1-10 parts of anti-hydrolysis agent; the outer layer includes the following components calculated by weight percentage: 50-90 parts of PBAT, 10-30 parts of PLA, epoxy chain extender ADR4468 0.1-10 parts, plasticizer epoxidized soybean oil 0.1-10 parts, coupling agent 0.1-10 parts, nucleating agent 0.1-10 parts, anti-hydrolysis agent 0.1-10 parts, antioxidant 0.1-10 parts, anti-ultraviolet agent 0.1-10 parts, straw 10-30 parts, degradation black masterbatch 1-10 parts.

[0011] The above-mentioned salt-alkali resistant and degradable mulch film, wherein the corrosion-resistant additive includes at least one of silicon dioxide, calcium carbonate, talcum powder, glass fiber, rice husk extract, clay, and biochar.

[0012] The above-mentioned salt-alkali resistant degradable mulch film, wherein the coupling agent is one of KH550, KH560, KH570 or titanate coupling agent.

[0013] The above-mentioned salt-alkali resistant and degradable mulch film, wherein the anti-ultraviolet agent is UV-531 or UV-327.

[0014] The above-mentioned salt-alkali resistant degradable mulch film, wherein the nucleating agent is preferably BTD-8808, the anti-hydrolysis agent is preferably BTWR-500, and the antioxidant is preferably 1010.

[0015] A method for preparing a salt-alkali resistant degradable mulch film comprises the following steps:

[0016] (1) Granulation of composite materials: Determine the raw material components of the composite materials to be processed according to the type of salt-alkali resistant degradable mulch film to be produced, weigh the corresponding raw materials according to the weight ratio of each raw material component in the corresponding formula, mix them evenly for 30-40 minutes, and put them into the twin-screw granulator for granulation to obtain different composite materials;

[0017] (2) Add different composite materials into the corresponding feed bin of the three-layer co-extrusion film blowing machine respectively;

[0018] (3) Adjust the temperature of the film blowing machine to 190-200℃ in zone 1, 170-180℃ in zone 2, 160-170℃ in zone 3, 150-160℃ in zone 4, 140-150℃ in zone 5, main machine speed to 10-30rpm, and traction speed to 10-30rpm;

[0019] (4) Start the film blowing machine, and obtain the salt-alkali resistant and degradable ground film through film blowing and winding.

[0020] The above-mentioned method for preparing a salt-alkali resistant and degradable mulch film, in which the steps described, the twin-screw granulator includes a base, a guide air plate, a cooling and drying mechanism and a power shearing mechanism, one end of the base is provided with an extrusion bin, the surface of the extrusion bin is evenly provided with a heater, two groups of spiral material columns are provided inside the extrusion bin, and both ends of the spiral material columns are connected to the extrusion bin through bearings, one end of the spiral material columns is fixedly connected to a first gear, and the first gear is located outside the extrusion bin, one end of the base is provided with a first motor, the output end of the first motor is fixedly connected to a second gear, and the second gear is meshed with the first gear, one end of the extrusion bin is provided with an extrusion nozzle, and the other end of the extrusion bin is provided with a vibrating feeder, and the control ends of the first motor and the vibrating feeder are electrically connected to an external power supply through an external switch.

[0021] The above-mentioned method for preparing a salt-alkali resistant and degradable mulch film, the cooling and drying mechanism of which includes a cooling trough, a down-pressure net, a guide positioning column, a support plate, a cooling box, a water pipe, a water pump, a heat dissipation fin, a fan, an air collecting box, a blowing plate, a first air pipe, a second air pipe and an intelligent temperature controller, a cooling trough is arranged in the middle of the top of the base, a down-pressure net is arranged inside the cooling trough, four groups of support plates are fixedly connected to the inner wall of the middle part of the cooling trough, and the top ends of the support plates are all in contact with the bottom end of the down-pressure net, ten groups of guide positioning columns are fixedly connected to the inner wall of the bottom end of the cooling trough, and the guide positioning columns are respectively located at the corners of the cooling trough, and the guide positioning columns are all slidably connected to the down-pressure net, a cooling box is arranged at the bottom end of the cooling trough, and one end of the cooling box is connected to one end of the cooling trough, and the other end of the cooling box is connected to a water pipe, and one end of the water pipe is in contact with one end of the cooling trough The heat dissipation device is a heat dissipation device, and a heat dissipation device is used to dissipate heat from the cooling element to the cooling element, and the heat is dissipated in an orderly manner. The cooling element is connected to the cooling element by the electric heat dissipation device, and the electric heat dissipation device is used to dissipate heat from the cooling element to the cooling element.

[0022] The above-mentioned method for preparing a salt-alkali resistant and degradable mulch film, wherein the power shearing mechanism includes a power frame, a power roller, a rotating part, a second motor, a belt, a pressure plate, a first movable groove, an elastic groove, a driven roller, an elastic sheet, a first movable plate, a connecting rod, an electric push rod, a receiving groove, a guide block, a first spring, a cutting plate, a second movable groove, a second movable plate, a threaded rotating rod, a pressure rod, a first clamping roller, a second clamping roller, a wide-mouth groove, a penetration groove, a slide groove, a slider, a bidirectional blade, a bracket, a reciprocating motor and a second spring, one end of the base is fixedly connected to the power frame, and the power frame is located at one end of the guide air plate, the top of the power frame is connected to two sets of power rollers through bearings, and one end of the power rollers extends to the outside of the power frame, and one end of the power rollers is fixedly connected to the rotating part , a second motor is provided at the bottom end of the power frame, a belt is provided at one end of the power frame, and the inner wall of the belt is in contact with the output end and the rotating part of the second motor, a pressing plate is provided at the top of the power frame, and first movable grooves are symmetrically provided at both ends of the pressing plate, and elastic grooves are provided in the middle of the first movable grooves, two groups of driven rollers are provided at the bottom end of the pressing plate, and both ends of the driven rollers are located inside the first movable groove, and elastic sheets are fixedly connected to the inside of the elastic grooves, and both ends of the driven rollers are fixedly connected to bearings, and the surface of the bearings is in contact with the middle of the elastic sheet, and the first movable plate is slidably connected to the middle and lower part of the power frame, and connecting rods are symmetrically slidably connected to both ends of the power frame, and both ends of the connecting rods are respectively connected to the pressing plate and the first movable The movable plate is fixedly connected, an electric push rod is provided at the bottom end of the first movable plate, and the bottom end of the electric push rod is fixedly connected to the base, the top of the power frame is evenly provided with receiving grooves, the inside of the receiving grooves are slidably connected with guide blocks, the bottom ends of the guide blocks are fixedly connected with a first spring, and the bottom ends of the first springs are fixedly connected with the inner walls of the receiving grooves, the top ends of the guide blocks are fitted with the bottom ends of the pressure plates, one end of the base is fixedly connected with a cutting plate, and the cutting plate is located on one side of the power frame, a second movable groove is provided in the middle and upper part of the cutting plate, the inside of the second movable groove is slidably connected with a second movable plate, the inside of the second movable groove is slidably connected with a pressure rod, and the pressure rod is located at the bottom end of the second movable plate, the top of the cutting plate is connected with a threaded rotating rod by a thread, and the thread The bottom end of the rotating rod is connected to the top of the second movable plate through a bearing, the bottom end of the second movable plate is evenly fixedly connected to a second spring, and the bottom ends of the second springs are fixedly connected to the top of the pressure rod, the middle part of the cutting plate is connected to two groups of first clamping rollers through bearings, the bottom end of the pressure rod is connected to two groups of second clamping rollers through bearings, the surfaces of the first clamping roller and the second clamping roller are evenly provided with corresponding wire grooves, one side of the cutting plate is evenly provided with a wide-mouth groove, and the other side of the cutting plate is evenly provided with a through groove, the central axes of the wide-mouth groove, the through groove and the wire groove on the surface of the first clamping roller coincide, one side of the cutting plate is provided with two groups of inclined sliding grooves, and the angle between the sliding groove and the vertical direction is thirty degrees, and the inside of the sliding groove is slidably connected with a slider,A bidirectional blade is provided on one side of the cutting plate, and both ends of the bidirectional blade are fixedly connected to the slider, a reciprocating motor is provided on one side of the cutting plate, a bracket is fixedly connected to the output end of the reciprocating motor, and both ends of the bracket are fixedly connected to both ends of the bidirectional blade, the bracket is located at the top of the bidirectional blade, the wide-mouth slot is trumpet-shaped, and the size of the smaller end of the wide-mouth slot is the same as the diameter of the through slot, and the second motor, the electric push rod and the control end of the reciprocating motor are all electrically connected to the external power supply through an external switch.

[0023] In the above-mentioned method for preparing a salt-alkali resistant and degradable mulch film, in the step (1), the temperature of the twin-screw granulator is 180-200°C in zone 1, 180-200°C in zone 2, 160-180°C in zone 3, 160-180°C in zone 4, and 140-160°C in zone 5; the main engine speed is 60-100rpm, and the feeding rate is 40-120rpm.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The salt-alkali resistant degradable mulch film and preparation method thereof provided by the present invention, according to different needs, uses corrosion-resistant materials / PBAT composite materials for the inner layer to enhance the corrosion resistance of the mulch film, uses high-barrier composite materials for the middle layer to enhance the water vapor barrier performance of the mulch film and slow down the evaporation of water, and uses an anti-ultraviolet formula for the outer layer to enhance the anti-ultraviolet performance of the mulch film. The three-layer film works synergistically, so that the mulch film can not only resist high ultraviolet radiation, but also withstand the erosion of salt and alkali. The longest induction period in saline-alkali land can reach 180 days, meeting the use requirements of saline-alkali land. The present invention opens up a new application field for degradable mulch films, has a certain degree of creativity, and compared with traditional PE mulch films, reduces white pollution. The developed mulch film products meet the planting needs of saline-alkali land and provide an important improvement idea for the utilization of saline-alkali land.

[0026] When the user needs to use the device of the present invention for granulation, the user controls the device to work automatically, the user adds the mixed material into the vibrating feeder, and the vibrating feeder is used for automatic feeding, the first motor drives the first gear and the spiral material column to rotate through the second gear, and at the same time the heater heats the material inside the extrusion bin, and the heated material is extruded through the extrusion nozzle through two groups of rotating spiral material columns, and the extruded material column enters the cooling tank, so that the material column is located between each group of guide positioning columns. After the material column passes through the cooling tank, the user places the lower pressure net inside the cooling tank, positions it through the guide positioning columns, and supports it through the support plate. At this time, the material column can be immersed in cooling water through the cooling tank and the lower pressure net, so as to facilitate cooling treatment of the material column. The cooling water can be internally circulated through the guide plate and the blowing plate, the water pipe and the water pump, and the circulating cooling water can be cooled through the fan and the heat dissipation fins. The heat conduction between the heat dissipation fins and the hot water is generated, and the heat at the bottom of the heat dissipation fins is blown away by the fan, so as to cool the cooling water and achieve the cooling effect. At the same time, the blown hot air is blown to the surface of the material column through the wind collecting box, the second air pipe, the first air pipe and the blowing plate, so as to dry the material column. The temperature of the hot air entering the second air pipe can be detected by the intelligent thermostat. If the temperature cannot reach the set temperature, the intelligent thermostat is used for heating to meet the drying requirements. The hot air generated by cooling and cooling can dry the material column, thereby reducing the production cost of the user. The utility model reduces energy consumption. The user controls the electric push rod to work, and the pressure plate and the driven roller can be raised through the first movable plate and the connecting rod. The user passes the material column through the power frame and the driven roller, and at the same time, the material column is located between the two sets of guide blocks, and the material column is separated by the guide blocks. The user controls the pressure plate to reset. At this time, the material column is pressed down by the driven roller, so that the elastic sheet is deformed. At the same time, the driven roller is pressed downward under the action of the elastic force of the elastic sheet itself, so that the material column is tightly located between the power roller and the driven roller. The second motor, belt, rotating part and power roller can provide power for the movement of the material column. The user passes the material column through the wide-mouth slot and the through-slot. The trumpet-shaped wide-mouth slot is convenient for the material column to penetrate. At this time, the material column is between the first clamping roller and the second The second spring is pressed against the second support member and the second support member is pressed against the second support member, and the second support member is pressed against the second support member, and the second support member is pressed against the second support member, and the second support member is pressed against the second support member, and the second support member is pressed against the second support member, and the second support member is pressed against the second support member, and the second support member is pressed against the second support member, and the second support member is pressed against the second support member, and the second support member is pressed against the second support member, and the second support member is pressed against the second support member, and the second support member is pressed against the second support member, and the second support member is pressed against the second support member, and the second support member is pressed against the second support member, and the second support member is pressed against the second support member, and the second support member is pressed against the second support member, and the second support member is pressed against the second support member, and the second support member is pressed against the second support member, and the second support memberThis device is fully automated, making it easy for users to use. It can also recycle the hot air generated by cooling, thereby reducing the user's cost. It can also automatically and quickly perform cutting work, and ensure the quality of cutting and the same cutting length. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a three-dimensional schematic diagram of the present invention;

[0028] Figure 2 It is a cross-sectional perspective schematic diagram of the present invention;

[0029] Figure 3 It is a cross-sectional stereoscopic schematic diagram of the extrusion chamber and the heater in the present invention;

[0030] Figure 4 It is a three-dimensional schematic diagram of the cooling tank and the lower pressure net in the present invention;

[0031] Figure 5 It is a cross-sectional perspective schematic diagram of the cooling box and the cooling tank in the present invention;

[0032] Figure 6 It is a cross-sectional perspective schematic diagram of the pressure plate and the power frame in the present invention;

[0033] Figure 7 It is a cross-sectional stereoscopic schematic diagram of the first movable groove and the receiving groove in the present invention;

[0034] Figure 8 is a cross-sectional perspective schematic diagram of the second movable groove and the pressure rod in the present invention;

[0035] Fig. 9 It is a cross-sectional stereoscopic schematic diagram of the slide groove and the wide-mouth groove in the present invention;

[0036] Fig.10 It is a schematic diagram for comparing the induction period in the present invention with the comparative example and Examples 1-6.

[0037] In the figure: 1. base; 2. extrusion chamber; 3. heater; 4. spiral material column; 5. first gear; 6. first motor; 7. second gear; 8. extrusion nozzle; 9. vibration feeder; 10. cooling tank; 11. lower pressure net; 12. guide positioning column; 13. support plate; 14. cooling box; 15. water pipe; 16. water pump; 17. cooling fin; 18. fan; 19. air collecting box; 20. guide air plate; 21. blowing plate; 22. first air pipe; 23. second air pipe; 24. intelligent temperature controller; 25. power frame; 26. power roller; 27. rotating part; 28. second electric machine; 29, belt; 30, pressure plate; 31, first movable groove; 32, elastic groove; 33, driven roller; 34, elastic sheet; 35, first movable plate; 36, connecting rod; 37, electric push rod; 38, receiving groove; 39, guide block; 40, first spring; 41, cutting plate; 42, second movable groove; 43, second movable plate; 44, threaded rotating rod; 45, pressure rod; 46, first clamping roller; 47, second clamping roller; 48, wide-mouth groove; 49, through groove; 50, slide groove; 51, slider; 52, two-way blade; 53, bracket; 54, reciprocating motor; 55, second spring. DETAILED DESCRIPTION

[0038] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0039] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0040] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0041] Unless otherwise specified, the raw materials used in the examples were purchased commercially.

[0042] Example 1

[0043] The present embodiment provides a salt-alkali resistant degradable ground film, comprising an inner layer, a middle layer and an outer layer, wherein the weight ratio of the inner layer, the middle layer and the outer layer is 10:3:1.

[0044] The inner layer is a corrosion-resistant silica / PBAT composite material, and its preparation steps include: 50 parts of silica, 40 parts of PBAT, 0.5 parts of epoxy chain extender ADR4468, 0.1 parts of plasticizer epoxy soybean oil, 1 part of coupling agent KH550, 0.1 parts of nucleating agent BTD-8808, and 0.3 parts of anti-hydrolysis agent BTWR-500 are uniformly mixed for half an hour, and granulated by a twin-screw strong feeding granulator, and the temperature of the twin-screw machine is adjusted to 200°C in zone one, 180°C in zone two, 180°C in zone three, 170°C in zone four, and 160°C in zone five, the main engine speed is 60rpm, and the feeding rate is 40rpm to obtain a corrosion-resistant inner layer composite material.

[0045] The middle layer is a high barrier PBAT / PLA composite material, and its preparation steps include: 50 parts of PBAT, 30 parts of PLA, 1 part of compatibilizer HP441, 0.1 part of nucleating agent BTD-8808, 10 parts of epoxy chain extender ADR4468, 0.2 parts of plasticizer epoxy soybean oil, and 0.5 parts of anti-hydrolysis agent BTWR-500 are uniformly mixed for half an hour, and granulated by a twin-screw granulator. The temperature of the twin-screw machine is adjusted to 200°C in zone one, 180°C in zone two, 180°C in zone three, 170°C in zone four, and 160°C in zone five. The main engine speed is 65rpm, and the feeding rate is 50rpm to obtain a high barrier middle layer composite material.

[0046] The outer layer is a UV-resistant PBAT composite material, and its preparation steps include: 70 parts of PBAT, 10 parts of PLA, 0.5 parts of epoxy chain extender ADR4468, 0.3 parts of plasticizer epoxy soybean oil, 10 parts of coupling agent KH550, 6 parts of nucleating agent BTD-8808, 2 parts of anti-hydrolysis agent BTWR-500, 10 parts of antioxidant 1010, 0.1 parts of anti-ultraviolet agent UV-531, 10 parts of straw, and 5 parts of degradation black masterbatch are uniformly mixed for half an hour, and granulated by a twin-screw granulator, and the temperature of the twin-screw machine is adjusted to 200°C in zone one, 180°C in zone two, 180°C in zone three, 170°C in zone four, and 160°C in zone five, the main engine speed is 70rpm, and the feeding rate is 55rpm to obtain a UV-resistant outer layer composite material.

[0047] The inner layer composite material, the middle layer composite material and the outer layer composite material are respectively added into the inner, middle and outer feed bins of the three-layer co-extrusion film blowing machine; the temperature of the film blowing machine is adjusted to 200°C for zone 1, 180°C for zone 2, 170°C for zone 3, 160°C for zone 4 and 150°C for zone 5, the main engine speed is 10rpm and the traction speed is 20rpm; the film blowing machine is started, and the salt-alkali resistant and degradable mulch film is obtained through film blowing and winding.

[0048] The film has been tested to have a tensile strength of 25MPa, an elongation at break of 510%, and a water vapor barrier of 220g / m224h. The induction period of the saline-alkali land covering experiment can reach 120 days, and the crop emergence rate reaches 95%.

[0049] Example 2

[0050] The present embodiment provides a salt-alkali resistant degradable ground film, comprising an inner layer, a middle layer and an outer layer, wherein the weight ratio of the inner layer, the middle layer and the outer layer is 3:1:10.

[0051] The inner layer is a corrosion-resistant calcium carbonate / PBAT composite material, and the preparation method includes: uniformly mixing 20 parts of calcium carbonate, 90 parts of PBAT, 10 parts of epoxy chain extender ADR4468, 0.5 parts of plasticizer epoxy soybean oil, 0.1 parts of coupling agent KH560, 85 parts of nucleating agent BTD-880, and 10 parts of anti-hydrolysis agent BTWR-500 for half an hour, and granulating through a twin-screw strong feeding granulator, adjusting the temperature of the twin-screw machine to 180°C in zone one, 200°C in zone two, 160°C in zone three, 160°C in zone four, and 140°C in zone five, the main engine speed is 80rpm, and the feeding rate is 100rpm to obtain a corrosion-resistant inner layer composite material.

[0052] The middle layer is a high barrier PBAT / PPC composite material, and its preparation steps include: 30 parts of PBAT, 30 parts of PPC, 0.1 parts of compatibilizer HP441, 0.5 parts of nucleating agent BTD-8808, 1 part of epoxy chain extender ADR4468, 0.1 parts of plasticizer epoxy soybean oil, and 10 parts of anti-hydrolysis agent BTWR-500 are uniformly mixed for half an hour, and granulated by a twin-screw granulator. The temperature of the twin-screw machine is adjusted to 180°C in zone 1, 200°C in zone 2, 160°C in zone 3, 160°C in zone 4, and 140°C in zone 5. The main engine speed is 85rpm, and the feeding rate is 90rpm to obtain a high barrier middle layer composite material.

[0053] The outer layer is a UV-resistant PBAT composite material, and its preparation steps include: 90 parts of PBAT, 30 parts of PLA, 10 parts of epoxy chain extender ADR4468, 0.1 parts of plasticizer epoxy soybean oil, 0.1 parts of coupling agent KH560, 0.1 parts of nucleating agent BTD-8808, 0.1 parts of anti-hydrolysis agent BTWR-500, 0.3 parts of antioxidant 1010, 10 parts of anti-ultraviolet agent UV-327, 20 parts of straw, and 1 part of degradation black masterbatch are uniformly mixed for 40 minutes, and granulated by a twin-screw granulator, and the temperature of the twin-screw machine is adjusted to 180°C in the first zone, 200°C in the second zone, 160°C in the third zone, 160°C in the fourth zone, and 140°C in the fifth zone, the main engine speed is 100rpm, and the feeding rate is 120rpm to obtain a UV-resistant outer layer composite material.

[0054] The inner layer composite material, the middle layer composite material and the outer layer composite material are respectively added into the inner, middle and outer feed bins of the three-layer co-extrusion film blowing machine; the temperature of the film blowing machine is adjusted to 190°C for zone 1, 170°C for zone 2, 160°C for zone 3, 150°C for zone 4 and 140°C for zone 5, the main engine speed is 30rpm and the traction speed is 30rpm; the film blowing machine is started, and the salt-alkali resistant and degradable mulch film is obtained through film blowing and winding.

[0055] The film was tested to have a tensile strength of 26.2MPa, an elongation at break of 546%, and a water vapor barrier of 253 g / m2 24h. The induction period of the film covering experiment on saline-alkali land was up to 150 days, and the crop emergence rate reached 92.6%.

[0056] Example 3

[0057] The present embodiment provides a salt-alkali resistant and degradable ground film, comprising an inner layer, a middle layer and an outer layer, wherein the weight ratio of the inner layer, the middle layer and the outer layer is 1:10:5.

[0058] The inner layer is a corrosion-resistant talcum powder / PBAT composite material, and the preparation method includes: 5 parts of talcum powder, 60 parts of PBAT, 0.1 parts of epoxy chain extender ADR4468, 10 parts of plasticizer epoxy soybean oil, 10 parts of coupling agent KH570, 10 parts of nucleating agent BTD-8808, and 0.1 parts of anti-hydrolysis agent BTWR-500 are uniformly mixed for 35 minutes, and granulated by a twin-screw strong feeding granulator, and the temperature of the twin-screw machine is adjusted to 190°C in zone one, 190°C in zone two, 170°C in zone three, 180°C in zone four, and 150°C in zone five, the main engine speed is 100rpm, and the feeding rate is 80rpm to obtain a corrosion-resistant inner layer composite material.

[0059] The middle layer is a high barrier PBAT / PBST composite material, and its preparation steps include: 40 parts of PBAT, 80 parts of PBST, 10 parts of compatibilizer HP441, 10 parts of nucleating agent BTD-8808, 0.1 parts of epoxy chain extender ADR4468, 10 parts of plasticizer epoxy soybean oil, and 0.1 parts of anti-hydrolysis agent BTWR-500 are uniformly mixed for half an hour, and granulated by a twin-screw granulator, and the temperature of the twin-screw machine is adjusted to 190°C in the first zone, 190°C in the second zone, 170°C in the third zone, 180°C in the fourth zone, and 150°C in the fifth zone. The main engine speed is 95rpm, and the feeding rate is 120rpm to obtain a high barrier middle layer composite material.

[0060] The outer layer is a UV-resistant PBAT composite material, and its preparation steps include: 50 parts of PBAT, 20 parts of PLA, 0.1 parts of epoxy chain extender ADR4468, 10 parts of plasticizer epoxy soybean oil, 8 parts of coupling agent KH570, 10 parts of nucleating agent BTD-8808, 10 parts of anti-hydrolysis agent BTWR-500, 0.1 parts of antioxidant 1010, 3 parts of anti-ultraviolet agent UV-327, 30 parts of straw, and 10 parts of degradation black masterbatch are uniformly mixed for half an hour, and granulated by a twin-screw granulator, and the temperature of the twin-screw machine is adjusted to 190°C in zone one, 190°C in zone two, 170°C in zone three, 180°C in zone four, and 150°C in zone five, the main engine speed is 80rpm, and the feeding rate is 110rpm to obtain a UV-resistant outer layer composite material.

[0061] The inner layer composite material, the middle layer composite material and the outer layer composite material are respectively added into the inner, middle and outer feed bins of the three-layer co-extrusion film blowing machine; the temperature of the film blowing machine is adjusted to 195°C for zone one, 175°C for zone two, 165°C for zone three, 155°C for zone four and 145°C for zone five, the main engine speed is 20rpm and the traction speed is 10rpm; the film blowing machine is started, and the salt-alkali resistant and degradable mulch film is obtained through film blowing and winding.

[0062] The film was tested to have a tensile strength of 22.5MPa, an elongation at break of 587%, and a water vapor barrier of 182g / m2 24h. The induction period of the film covering experiment on saline-alkali land was up to 110 days, and the crop emergence rate reached 97.5%.

[0063] Example 4

[0064] The present embodiment provides a salt-alkali resistant and degradable ground film, comprising an inner layer, a middle layer and an outer layer, wherein the weight ratio of the inner layer, the middle layer and the outer layer is 1:1:1.

[0065] The inner layer is a corrosion-resistant glass fiber / rice husk extract / PBAT composite material, and its preparation steps include: 20 parts of glass fiber, 10 parts of rice husk extract, 40 parts of PBAT, 0.5 parts of epoxy chain extender ADR4468, 0.1 parts of plasticizer epoxy soybean oil, 1 part of titanate coupling agent, 0.1 parts of nucleating agent BTD-8808, and 0.3 parts of anti-hydrolysis agent BTWR-500 are uniformly mixed for half an hour, and granulated by a twin-screw strong feeding granulator, and the temperature of the twin-screw machine is adjusted to 200°C in zone one, 180°C in zone two, 180°C in zone three, 170°C in zone four, and 160°C in zone five, the main engine speed is 60rpm, and the feeding rate is 40rpm to obtain a corrosion-resistant inner layer composite material.

[0066] The middle layer is a high barrier PBAT / PGA composite material, and its preparation steps include: 50 parts of PBAT, 30 parts of PGA, 1 part of compatibilizer HP441, 0.1 part of nucleating agent BTD-8808, 10 parts of epoxy chain extender ADR4468, 0.2 parts of plasticizer epoxy soybean oil, and 0.5 parts of anti-hydrolysis agent BTWR-500 are uniformly mixed for half an hour, and granulated by a twin-screw granulator. The temperature of the twin-screw machine is adjusted to 200°C in zone one, 180°C in zone two, 180°C in zone three, 170°C in zone four, and 160°C in zone five. The main engine speed is 65rpm, and the feeding rate is 50rpm to obtain a high barrier middle layer composite material.

[0067] The outer layer is a UV-resistant PBAT composite material, and its preparation steps include: 70 parts of PBAT, 10 parts of PLA, 0.5 parts of epoxy chain extender ADR4468, 0.3 parts of plasticizer epoxy soybean oil, 10 parts of titanate coupling agent, 6 parts of nucleating agent BTD-8808, 2 parts of anti-hydrolysis agent BTWR-500, 10 parts of antioxidant 1010, 0.1 parts of anti-ultraviolet agent UV-531, 10 parts of straw, and 5 parts of degradation black masterbatch are uniformly mixed for half an hour, and granulated by a twin-screw granulator, and the temperature of the twin-screw machine is adjusted to 200°C in zone one, 180°C in zone two, 180°C in zone three, 170°C in zone four, and 160°C in zone five, the main engine speed is 70rpm, and the feeding rate is 55rpm to obtain a UV-resistant outer layer composite material.

[0068] Add equal weights of inner layer composite material, middle layer composite material and outer layer composite material into the inner, middle and outer feed bins of the three-layer co-extrusion film blowing machine respectively; adjust the temperature of the film blowing machine to 200°C for zone 1, 180°C for zone 2, 170°C for zone 3, 160°C for zone 4 and 150°C for zone 5, the main engine speed to 10rpm and the traction speed to 20rpm; start the film blowing machine, and obtain the salt-alkali resistant and degradable mulch film by film blowing and winding.

[0069] The film was tested to have a tensile strength of 27.2MPa, an elongation at break of 550.4%, and a water vapor barrier of 205.6g / m2 24h. The induction period of the saline-alkali land covering experiment was up to 160 days, and the crop emergence rate reached 94.7%.

[0070] Example 5

[0071] The difference between this embodiment and embodiment 4 is that this embodiment provides a salt-alkali resistant degradable ground film, including an inner layer, a middle layer and an outer layer, and the weight ratio of the inner layer, the middle layer and the outer layer is 2:3:2. The inner layer is a corrosion-resistant glass fiber / PBAT composite material, which includes: 25 parts of glass fiber, 40 parts of PBAT, 0.5 parts of epoxy chain extender ADR4468, 0.1 parts of plasticizer epoxy soybean oil, 1 part of titanate coupling agent, 0.1 parts of nucleating agent BTD-8808, and 0.3 parts of anti-hydrolysis agent BTWR-500.

[0072] The film was tested to have a tensile strength of 28.2MPa, an elongation at break of 608.2%, and a water vapor barrier of 215.3g / m2 24h. The induction period of the saline-alkali land covering experiment was up to 180 days, and the crop emergence rate reached 92.7%.

[0073] Example 6

[0074] The difference between this embodiment and embodiment 4 is that this embodiment provides a salt-alkali resistant degradable ground film, including an inner layer, a middle layer and an outer layer, and the weight ratio of the inner layer, the middle layer and the outer layer is 3:1:5. The inner layer is a corrosion-resistant rice husk extract / PBAT composite material, which includes: 20 parts of rice husk extract, 40 parts of PBAT, 0.5 parts of epoxy chain extender ADR4468, 0.1 parts of plasticizer epoxy soybean oil, 1 part of titanate coupling agent, 0.1 parts of nucleating agent BTD-8808, and 0.3 parts of anti-hydrolysis agent BTWR-500.

[0075] The film was tested to have a tensile strength of 24.1MPa, an elongation at break of 530.5%, and a water vapor barrier of 262.7g / m2 24h. The induction period of the film covering experiment on saline-alkali land was up to 140 days, and the crop emergence rate reached 91.7%.

[0076] Example 7

[0077] The difference between this embodiment and embodiment 4 is that this embodiment provides a salt-alkali resistant degradable ground film, including an inner layer, a middle layer and an outer layer, and the weight ratio of the inner layer, the middle layer and the outer layer is 3:2:5. The inner layer is a corrosion-resistant clay / PBAT composite material, which includes: 10 parts of clay, 40 parts of PBAT, 0.5 parts of epoxy chain extender ADR4468, 0.1 parts of plasticizer epoxy soybean oil, 1 part of titanate coupling agent, 0.1 parts of nucleating agent BTD-8808, and 0.3 parts of anti-hydrolysis agent BTWR-500.

[0078] The film was tested to have a tensile strength of 22.1MPa, an elongation at break of 503.6%, and a water vapor barrier of 242.3g / m2 24h. The induction period of the saline-alkali land covering experiment was up to 90 days, and the crop emergence rate reached 89.7%.

[0079] Example 8

[0080] The present embodiment provides a salt-alkali resistant degradable mulch film, comprising an inner layer, wherein the inner layer is a corrosion-resistant silica / PBAT composite material, and the preparation steps thereof include: uniformly mixing 40 parts of silica, 40 parts of PBAT, 0.5 parts of epoxy chain extender ADR4468, 0.1 parts of plasticizer epoxy soybean oil, 1 part of titanate coupling agent, 0.1 parts of nucleating agent BTD-8808, and 0.3 parts of anti-hydrolysis agent BTWR-500 for half an hour, granulating the mixture through a twin-screw forced feeding granulator, adjusting the temperature of the twin-screw machine to 200° C. in zone 1, 180° C. in zone 2, 180° C. in zone 3, 170° C. in zone 4, and 160° C. in zone 5, the main engine speed to 60 rpm, and the feeding rate to 40 rpm, to obtain a corrosion-resistant inner layer composite material.

[0081] Add the inner layer composite material into the feed bin of the film blowing machine; adjust the temperature of the film blowing machine to 200°C in zone 1, 180°C in zone 2, 170°C in zone 3, 160°C in zone 4, and 150°C in zone 5, the main engine speed to 10rpm, and the traction speed to 20rpm; start the film blowing machine, and obtain the salt-alkali resistant and degradable mulch film through film blowing and winding.

[0082] The film was tested to have a tensile strength of 26.3MPa, an elongation at break of 493.6%, and a water vapor barrier of 282.6g / m2 24h. The induction period of the film covering experiment on saline-alkali land was up to 80 days, and the crop emergence rate reached 80.6%.

[0083] Example 9

[0084] This embodiment provides a salt-alkali resistant and degradable ground film, including an inner layer and an outer layer, and the weight ratio of the inner layer to the outer layer is 1:1.

[0085] The inner layer is a corrosion-resistant glass fiber / PBAT composite material, and its preparation steps include: 20 parts of glass fiber, 40 parts of PBAT, 0.5 parts of epoxy chain extender ADR4468, 0.1 parts of plasticizer epoxy soybean oil, 1 part of titanate coupling agent, 0.1 parts of nucleating agent BTD-8808, and 0.3 parts of anti-hydrolysis agent BTWR-500 are uniformly mixed for half an hour, and granulated by a twin-screw strong feeding granulator, and the temperature of the twin-screw machine is adjusted to 200°C in zone one, 180°C in zone two, 180°C in zone three, 170°C in zone four, and 160°C in zone five, the main engine speed is 60rpm, and the feeding rate is 40rpm to obtain a corrosion-resistant inner layer composite material.

[0086] The outer layer is a UV-resistant PBAT composite material, and its preparation steps include: 70 parts of PBAT, 10 parts of PLA, 0.5 parts of epoxy chain extender ADR4468, 0.3 parts of plasticizer epoxy soybean oil, 10 parts of titanate coupling agent, 6 parts of nucleating agent BTD-8808, 2 parts of anti-hydrolysis agent BTWR-500, 10 parts of antioxidant 1010, 0.1 parts of anti-ultraviolet agent UV-531, 10 parts of straw, and 5 parts of degradation black masterbatch are uniformly mixed for half an hour, and granulated by a twin-screw granulator, and the temperature of the twin-screw machine is adjusted to 200°C in zone one, 180°C in zone two, 180°C in zone three, 170°C in zone four, and 160°C in zone five, the main engine speed is 70rpm, and the feeding rate is 55rpm to obtain a UV-resistant outer layer composite material.

[0087] Add equal weights of inner layer composite material and outer layer composite material into the inner and outer feed bins of the co-extrusion film blowing machine respectively; adjust the temperature of the film blowing machine to 200°C for zone 1, 180°C for zone 2, 170°C for zone 3, 160°C for zone 4, and 150°C for zone 5, the main engine speed to 10rpm, and the traction rate to 20rpm; start the film blowing machine, and obtain the salt-alkali resistant and degradable mulch film through film blowing and winding.

[0088] The film was tested to have a tensile strength of 27.2MPa, an elongation at break of 540.7%, and a water vapor barrier of 352.5g / m2 24h. The induction period of the film covering experiment on saline-alkali land was up to 125 days, and the crop emergence rate was 85.6%.

[0089] Example 10

[0090] This embodiment provides a salt-alkali resistant degradable ground film, including an inner layer and an outer layer, wherein the weight ratio of the inner layer to the outer layer is 10:1

[0091] The inner layer is a biochar / PBAT composite material, and its preparation steps include: 30 parts of biochar, 50 parts of PBAT, 0.8 parts of epoxy chain extender ADR4468, 0.3 parts of plasticizer epoxy soybean oil, 0.1 parts of titanate coupling agent, 0.2 parts of nucleating agent BTD-8808, and 0.5 parts of anti-hydrolysis agent BTWR-500 are uniformly mixed for half an hour, and granulated by a twin-screw strong feeding granulator, and the temperature of the twin-screw machine is adjusted to 200°C in zone one, 190°C in zone two, 190°C in zone three, 180°C in zone four, and 170°C in zone five, the main engine speed is 70rpm, and the feeding rate is 50rpm to obtain a corrosion-resistant inner layer composite material.

[0092] The outer layer is a UV-resistant PBAT composite material, and its preparation steps include: 70 parts of PBAT, 20 parts of PLA, 1 part of epoxy chain extender ADR4468, 0.5 parts of plasticizer epoxy soybean oil, 3 parts of titanate coupling agent, 2 parts of nucleating agent BTD-8808, 1 part of anti-hydrolysis agent BTWR-500, 6 parts of antioxidant 1010, 0.5 parts of anti-ultraviolet agent UV-531, 10 parts of straw, and 5 parts of degradation black masterbatch are uniformly mixed for half an hour, and granulated by a twin-screw granulator, and the temperature of the twin-screw machine is adjusted to 190°C in the first zone, 180°C in the second zone, 170°C in the third zone, 170°C in the fourth zone, and 165°C in the fifth zone, the main engine speed is 80rpm, and the feeding rate is 65rpm to obtain a UV-resistant outer layer composite material.

[0093] The inner layer composite material and the outer layer composite material are added into the inner and outer feed bins of the co-extrusion film blowing machine respectively; the temperature of the film blowing machine is adjusted to 200°C for zone 1, 190°C for zone 2, 180°C for zone 3, 160°C for zone 4 and 150°C for zone 5, the main engine speed is 10rpm and the traction speed is 25rpm; the film blowing machine is started, and the salt-alkali resistant and degradable mulch film is obtained through film blowing and winding.

[0094] The film was tested to have a tensile strength of 25.9MPa, an elongation at break of 510.7%, and a water vapor barrier of 372.5g / m2 24h. The induction period of the film covering experiment on saline-alkali land was up to 106 days, and the crop emergence rate reached 89.1%.

[0095] Embodiment 11

[0096] This embodiment provides a salt-alkali resistant and degradable ground film, including an inner layer and an outer layer, and the weight ratio of the inner layer to the outer layer is 1:10.

[0097] The inner layer is a corrosion-resistant calcium carbonate / PBAT composite material, and its preparation steps include: uniformly mixing 20 parts of calcium carbonate, 90 parts of PBAT, 5 parts of epoxy chain extender ADR4468, 3 parts of plasticizer epoxy soybean oil, 1 part of titanate coupling agent, 2 parts of nucleating agent BTD-8808, and 5 parts of anti-hydrolysis agent BTWR-500 for half an hour, and granulating them through a twin-screw strong feeding granulator, adjusting the temperature of the twin-screw machine to 190°C in zone one, 185°C in zone two, 180°C in zone three, 175°C in zone four, and 170°C in zone five, the main engine speed is 75rpm, and the feeding rate is 45rpm to obtain a corrosion-resistant inner layer composite material.

[0098] The outer layer is a UV-resistant PBAT composite material, and its preparation steps include: 70 parts of PBAT, 20 parts of PLA, 1.5 parts of epoxy chain extender ADR4468, 2.5 parts of plasticizer epoxy soybean oil, 10 parts of titanate coupling agent, 3 parts of nucleating agent BTD-8808, 10 parts of anti-hydrolysis agent BTWR-500, 1 part of antioxidant 1010, 1.5 parts of anti-ultraviolet agent UV-531, 10 parts of straw, and 5 parts of degradation black masterbatch are uniformly mixed for half an hour, and granulated by a twin-screw granulator, and the temperature of the twin-screw machine is adjusted to 190°C in zone one, 180°C in zone two, 175°C in zone three, 165°C in zone four, and 165°C in zone five, the main engine speed is 80rpm, and the feeding rate is 65rpm to obtain a UV-resistant outer layer composite material.

[0099] The inner layer composite material and the outer layer composite material are added into the inner and outer feed bins of the co-extrusion film blowing machine respectively; the temperature of the film blowing machine is adjusted to 200°C for zone 1, 190°C for zone 2, 180°C for zone 3, 160°C for zone 4 and 150°C for zone 5, the main engine speed is 10rpm and the traction speed is 25rpm; the film blowing machine is started, and the salt-alkali resistant and degradable mulch film is obtained through film blowing and winding.

[0100] The film was tested to have a tensile strength of 24.8MPa, an elongation at break of 498.7%, and a water vapor barrier of 325.5g / m2 24h. The induction period of the film covering experiment on saline-alkali land was up to 116 days, and the crop emergence rate reached 90.3%.

[0101] Example 12

[0102] This embodiment provides a salt-alkali resistant degradable ground film, including an inner layer and an outer layer, and the weight ratio of the inner layer to the outer layer is 3:2.

[0103] The inner layer is a corrosion-resistant glass fiber / PBAT composite material, and its preparation steps include: 20 parts of glass fiber, 80 parts of PBAT, 8 parts of epoxy chain extender ADR4468, 7 parts of plasticizer epoxy soybean oil, 1 part of titanate coupling agent, 10 parts of nucleating agent BTD-8808, and 10 parts of anti-hydrolysis agent BTWR-500 are uniformly mixed for half an hour, and granulated by a twin-screw strong feeding granulator, and the temperature of the twin-screw machine is adjusted to 200°C in zone one, 190°C in zone two, 190°C in zone three, 180°C in zone four, and 170°C in zone five, the main engine speed is 55rpm, and the feeding rate is 40rpm to obtain a corrosion-resistant inner layer composite material.

[0104] The outer layer is a UV-resistant PBAT composite material, and its preparation steps include: 70 parts of PBAT, 20 parts of PLA, 10 parts of epoxy chain extender ADR4468, 0.5 parts of plasticizer epoxy soybean oil, 3 parts of titanate coupling agent, 2 parts of nucleating agent BTD-8808, 1 part of anti-hydrolysis agent BTWR-500, 0.6 parts of antioxidant 1010, 0.5 parts of anti-ultraviolet agent UV-531, 10 parts of straw, and 1 part of degradation black masterbatch are uniformly mixed for half an hour, and granulated by a twin-screw granulator, and the temperature of the twin-screw machine is adjusted to 190°C in the first zone, 180°C in the second zone, 170°C in the third zone, 170°C in the fourth zone, and 165°C in the fifth zone, the main engine speed is 80rpm, and the feeding rate is 65rpm to obtain a UV-resistant outer layer composite material.

[0105] The inner layer composite material and the outer layer composite material are added into the inner and outer feed bins of the co-extrusion film blowing machine respectively; the temperature of the film blowing machine is adjusted to 200°C for zone 1, 190°C for zone 2, 180°C for zone 3, 160°C for zone 4, and 150°C for zone 5, the main engine speed is 15rpm, and the traction speed is 30rpm; the film blowing machine is started, and the salt-alkali resistant and degradable mulch film is obtained through film blowing and winding.

[0106] The film was tested to have a tensile strength of 23.7MPa, an elongation at break of 486.2%, and a water vapor barrier of 398.4g / m2 24h. The induction period of the film covering experiment on saline-alkali land was up to 103 days, and the crop emergence rate reached 88.4%.

[0107] Example 13

[0108] This embodiment provides a salt-alkali resistant and degradable ground film, comprising an inner layer and a middle layer, wherein the weight ratio of the inner layer to the middle layer is 10:3.

[0109] The inner layer is a corrosion-resistant silica / PBAT composite material, and its preparation steps include: 50 parts of silica, 40 parts of PBAT, 0.5 parts of epoxy chain extender ADR4468, 0.1 parts of plasticizer epoxy soybean oil, 1 part of coupling agent KH550, 0.1 parts of nucleating agent BTD-8808, and 0.3 parts of anti-hydrolysis agent BTWR-500 are uniformly mixed for half an hour, and granulated by a twin-screw strong feeding granulator, and the temperature of the twin-screw machine is adjusted to 200°C in zone one, 180°C in zone two, 180°C in zone three, 170°C in zone four, and 160°C in zone five, the main engine speed is 60rpm, and the feeding rate is 40rpm to obtain a corrosion-resistant inner layer composite material.

[0110] The middle layer is a high barrier PBAT / PCL composite material, and its preparation steps include: 50 parts of PBAT, 30 parts of PCL, 1 part of compatibilizer HP441, 0.1 part of nucleating agent BTD-8808, 10 parts of epoxy chain extender ADR4468, 0.2 parts of plasticizer epoxy soybean oil, and 0.5 parts of anti-hydrolysis agent BTWR-500 are uniformly mixed for half an hour, and granulated by a twin-screw granulator. The temperature of the twin-screw machine is adjusted to 200°C in zone one, 180°C in zone two, 180°C in zone three, 170°C in zone four, and 160°C in zone five. The main engine speed is 65rpm, and the feeding rate is 50rpm to obtain a high barrier middle layer composite material.

[0111] The inner layer composite material and the middle layer composite material are added into the inner and middle feed bins of the co-extrusion film blowing machine respectively; the temperature of the film blowing machine is adjusted to 200°C for zone 1, 180°C for zone 2, 170°C for zone 3, 160°C for zone 4 and 150°C for zone 5, the main engine speed is 10rpm and the traction speed is 20rpm; the film blowing machine is started, and the salt-alkali resistant and degradable ground film is obtained through film blowing and winding.

[0112] The film was tested to have a tensile strength of 23.2MPa, an elongation at break of 563.5%, and a water vapor barrier of 182.3g / m2 24h. The induction period of the saline-alkali land covering experiment was up to 115 days, and the crop emergence rate reached 92.8%.

[0113] Embodiment 14

[0114] This embodiment provides a salt-alkali resistant and degradable ground film, including an inner layer and a middle layer, and the weight ratio of the inner layer to the middle layer is 3:10.

[0115] The inner layer is a corrosion-resistant silica / PBAT composite material, and its preparation steps include: 50 parts of silica, 40 parts of PBAT, 5 parts of epoxy chain extender ADR4468, 0.1 parts of plasticizer epoxy soybean oil, 1 part of coupling agent KH550, 10 parts of nucleating agent BTD-8808, and 3 parts of anti-hydrolysis agent BTWR-500 are uniformly mixed for half an hour, and granulated by a twin-screw strong feeding granulator, and the temperature of the twin-screw machine is adjusted to 200°C in zone one, 180°C in zone two, 180°C in zone three, 170°C in zone four, and 160°C in zone five, the main engine speed is 60rpm, and the feeding rate is 35rpm to obtain a corrosion-resistant inner layer composite material.

[0116] The middle layer is a high barrier PBAT / PHA composite material, and its preparation steps include: 50 parts of PBST, 30 parts of PHA, 1 part of compatibilizer HP441, 0.1 part of nucleating agent BTD-8808, 10 parts of epoxy chain extender ADR4468, 10 parts of plasticizer epoxy soybean oil, and 5 parts of anti-hydrolysis agent BTWR-500 are uniformly mixed for half an hour, and granulated by a twin-screw granulator. The temperature of the twin-screw machine is adjusted to 200°C in zone 1, 180°C in zone 2, 180°C in zone 3, 170°C in zone 4, and 160°C in zone 5. The main engine speed is 65rpm, and the feeding rate is 50rpm to obtain a high barrier middle layer composite material.

[0117] The inner layer composite material and the middle layer composite material are added into the inner and middle feed bins of the co-extrusion film blowing machine respectively; the temperature of the film blowing machine is adjusted to 200°C for zone 1, 180°C for zone 2, 170°C for zone 3, 160°C for zone 4 and 150°C for zone 5, the main engine speed is 10rpm and the traction speed is 20rpm; the film blowing machine is started, and the salt-alkali resistant and degradable ground film is obtained through film blowing and winding.

[0118] The film was tested to have a tensile strength of 22.9MPa, an elongation at break of 587.1%, and a water vapor barrier of 162.2g / m2 24h. The induction period of the film covering experiment on saline-alkali land was up to 105 days, and the crop emergence rate was 89.4%.

[0119] Embodiment 15

[0120] This embodiment provides a salt-alkali resistant and degradable ground film, comprising an inner layer and a middle layer, wherein the weight ratio of the inner layer to the middle layer is 1:1.

[0121] The inner layer is a corrosion-resistant silica / PBAT composite material, and its preparation steps include: 50 parts of silica, 40 parts of PBAT, 0.1 parts of epoxy chain extender ADR4468, 0.1 parts of plasticizer epoxy soybean oil, 6 parts of coupling agent KH550, 0.1 parts of nucleating agent BTD-8808, and 4 parts of anti-hydrolysis agent BTWR-500 are uniformly mixed for half an hour, and granulated by a twin-screw strong feeding granulator, and the temperature of the twin-screw machine is adjusted to 200°C in zone one, 180°C in zone two, 180°C in zone three, 170°C in zone four, and 160°C in zone five, the main engine speed is 60rpm, and the feeding rate is 40rpm to obtain a corrosion-resistant inner layer composite material.

[0122] The middle layer is a high barrier composite material, and its preparation steps include: 30 parts of PBAT, 10 parts of PLA, 10 parts of PHA, 10 parts of PGA, 10 parts of PCL, 10 parts of PPC, 10 parts of PBST, 10 parts of compatibilizer HP441, 0.1 parts of nucleating agent BTD-8808, 10 parts of epoxy chain extender ADR4468, 0.2 parts of plasticizer epoxy soybean oil, and 0.1 parts of anti-hydrolysis agent BTWR-500 are uniformly mixed for half an hour, and granulated by a twin-screw granulator, and the temperature of the twin-screw machine is adjusted to 200°C in the first zone, 180°C in the second zone, 180°C in the third zone, 170°C in the fourth zone, and 160°C in the fifth zone, the main engine speed is 65rpm, and the feeding rate is 50rpm to obtain a high barrier middle layer composite material.

[0123] The inner layer composite material and the middle layer composite material are added into the inner and middle feed bins of the co-extrusion film blowing machine respectively; the temperature of the film blowing machine is adjusted to 200°C for zone 1, 180°C for zone 2, 170°C for zone 3, 160°C for zone 4 and 150°C for zone 5, the main engine speed is 10rpm and the traction speed is 20rpm; the film blowing machine is started, and the salt-alkali resistant and degradable ground film is obtained through film blowing and winding.

[0124] The film was tested to have a tensile strength of 25.3MPa, an elongation at break of 509.7%, and a water vapor barrier of 201.9g / m2 24h. The induction period of the saline-alkali land covering experiment was up to 102 days, and the crop emergence rate reached 91.7%.

[0125] Example 16

[0126] The difference between this embodiment and embodiment 15 is that the middle layer high barrier composite material components include: 40 parts of PBAT, 5 parts of PHA, 10 parts of PGA, 10 parts of PCL, 10 parts of compatibilizer HP441, 0.1 parts of nucleating agent BTD-8808, 10 parts of epoxy chain extender ADR4468, 0.2 parts of plasticizer epoxy soybean oil, and 0.1 parts of anti-hydrolysis agent BTWR-500.

[0127] The film was tested to have a tensile strength of 28.6MPa, an elongation at break of 573.2%, and a water vapor barrier of 181.7g / m2 24h. The induction period of the film covering experiment on saline-alkali land was up to 122 days, and the crop emergence rate reached 96.3%.

[0128] Embodiment 17

[0129] The difference between this embodiment and embodiment 15 is that the middle layer high barrier composite material includes: 30 parts of PBAT, 5 parts of PGA, 5 parts of PCL, 5 parts of PPC, 5 parts of PBST, 10 parts of compatibilizer HP441, 0.1 parts of nucleating agent BTD-8808, 10 parts of epoxy chain extender ADR4468, 0.2 parts of plasticizer epoxy soybean oil, and 0.1 parts of anti-hydrolysis agent BTWR-500.

[0130] The film was tested to have a tensile strength of 26.1MPa, an elongation at break of 528.3%, and a water vapor barrier of 263.5g / m2 24h. The induction period of the film covering experiment on saline-alkali land was up to 133 days, and the crop emergence rate reached 95.6%.

[0131] Embodiment 18

[0132] The difference between this embodiment and embodiment 15 is that the middle layer high barrier composite material includes: 30 parts of PBAT, 5 parts of PHA, 5 parts of PGA, 10 parts of PPC, 10 parts of PBST, 10 parts of compatibilizer HP441, 0.1 parts of nucleating agent BTD-8808, 10 parts of epoxy chain extender ADR4468, 0.2 parts of plasticizer epoxy soybean oil, and 0.1 parts of anti-hydrolysis agent BTWR-500.

[0133] The film was tested to have a tensile strength of 27.1MPa, an elongation at break of 518.9%, and a water vapor barrier of 191.3g / m2 24h. The induction period of the film covering experiment on saline-alkali land was up to 109 days, and the crop emergence rate reached 93.6%.

[0134] The obtained mulch film was tested for mechanical properties, water vapor barrier properties, and aging properties. The results showed that the mechanical properties of the mulch film were improved by 30% compared with pure PBAT mulch film, and the water vapor barrier properties were improved by 50%. In the saline-alkali land aging test, the degradation cycle was increased from 35 days to 180 days, which meets the use requirements of saline-alkali land.

[0135] Embodiment 19

[0136] See also Figure 1-9The present embodiment provides a twin-screw granulator for step (1) in a method for preparing a salt-alkali resistant and degradable mulch film, characterized in that it comprises a base 1, a guide air plate 20, a cooling and drying mechanism and a power shearing mechanism, an extrusion bin 2 is arranged at one end of the base 1, a heater 3 is evenly arranged on the surface of the extrusion bin 2, two groups of spiral material columns 4 are arranged inside the extrusion bin 2, and both ends of the spiral material columns 4 are connected to the extrusion bin 2 through bearings, one end of the spiral material columns 4 is fixedly connected to a first gear 5, and the first gear 5 is located outside the extrusion bin 2, one end of the base 1 is provided with a first motor 6, and the output end of the first motor 6 is fixedly connected to a second Gear 7, and the second gear 7 is meshed with the first gear 5, one end of the extrusion bin 2 is provided with an extrusion nozzle 8, and the other end of the extrusion bin 2 is provided with a vibration feeder 9, the control ends of the first motor 6 and the vibration feeder 9 are electrically connected to the external power supply through an external switch, and the user controls the device to work automatically. The user adds the mixed material into the vibration feeder 9, and the vibration feeder 9 is automatically fed, and the first motor 6 drives the first gear 5 and the spiral material column 4 to rotate through the second gear 7, and at the same time, the heater 3 heats the material inside the extrusion bin 2, and the heated material is extruded through the extrusion nozzle 8 through two sets of rotating spiral material columns 4;

[0137] See also Figure 2 , Figure 4 , Figure 5 and Figure 6In this embodiment, the cooling and drying mechanism includes a cooling trough 10, a lower pressure net 11, a guide positioning column 12, a support plate 13, a cooling box 14, a water pipe 15, a water pump 16, a heat dissipation fin 17, a fan 18, a wind collecting box 19, a blowing plate 21, a first air pipe 22, a second air pipe 23 and an intelligent temperature controller 24. A cooling trough 10 is arranged in the middle of the top of the base 1, and a lower pressure net 11 is arranged inside the cooling trough 10. Four groups of support plates 13 are fixedly connected to the inner wall of the middle part of the cooling trough 10, and the tops of the support plates 13 are all in contact with the bottom end of the lower pressure net 11. Ten groups of guide positioning columns 12 are fixedly connected to the inner wall of the bottom end of the cooling trough 10, and the guide positioning columns 12 are respectively located at the corners of the cooling trough 10, and the guide positioning columns 12 are all slidably connected to the lower pressure net 11. A cooling box 14 is provided at the bottom end of 10, and one end of the cooling box 14 is connected to one end of the cooling tank 10, and the other end of the cooling box 14 is connected to a water pipe 15, and one end of the water pipe 15 is connected to one end of the cooling tank 10, and a water pump 16 is provided in the middle of the water pipe 15, and the interior of the cooling box 14 is evenly and fixedly connected with heat dissipation fins 17, and the bottom ends of the heat dissipation fins 17 are all in contact with the top of the base 1, and a fan 18 is provided at the bottom end of the cooling box 14, and the fan 18 is located on one side of the heat dissipation fins 17, one end of the heat dissipation fin 17 is fixedly connected to an air collecting box 19, and one end of the air collecting box 19 is connected to a second air pipe 23, and one end of the cooling tank 10 is fixedly connected to a guide air plate 20, and the end of the guide air plate 20 connected to the cooling tank 10 is lower than the guide air plate At the other end of 20, a blowing plate 21 is arranged on the top of the guide air plate 20, and the blowing plate 21 is parallel to the guide air plate 20, both ends of the blowing plate 21 are connected to the first air pipe 22, and one end of the first air pipe 22 is connected to one end of the second air pipe 23, and one end of the second air pipe 23 is provided with an intelligent temperature controller 24, and the control ends of the water pump 16, the fan 18 and the intelligent temperature controller 24 are all electrically connected to the external power supply through an external switch, and the extruded material column enters the cooling tank 10, so that the material column is located between each group of guide positioning columns 12, and after the material column passes through the cooling tank 10, the user places the lower pressure net 11 inside the cooling tank 10, positions it through the guide positioning columns 12, and supports it through the support plate 13, at this time, the cooling tank 10 and the lower pressure net 11 can be The material column is immersed in cooling water, so it is convenient to cool the material column. The material column passes through the guide air plate 20 and the blowing plate 21. The cooling water can be circulated internally through the water pipe 15 and the water pump 16. The circulating cooling water can be cooled through the fan 18 and the heat dissipation fins 17. The heat conduction between the heat dissipation fins 17 and the hot water is generated. The heat at the bottom of the heat dissipation fins 17 is blown away by the fan 18, and the hot air is collected by the air collecting box 19, and then enters the inside of the first air pipe 22 through the second air pipe 23, and then enters the inside of the blowing plate 21 through the first air pipe 22, and finally blows to the surface of the material column through the blowing plate 21, so as to dry the material column. The water droplets blown down are collected by the guide air plate 20 and flow to the inside of the cooling tank 10.The temperature of the hot air entering the second air pipe 23 can be detected by the intelligent thermostat 24. If the temperature cannot reach the set temperature, the intelligent thermostat 24 is used to heat the hot air to meet the drying requirements. The hot air generated by cooling is used to dry the material column, thereby reducing the production cost of the user and reducing energy consumption.

[0138] See also Figure 2 , Figure 6 , Figure 7 , Figure 8 and Fig. 9In this embodiment, the power shearing mechanism includes a power frame 25, a power roller 26, a rotating member 27, a second motor 28, a belt 29, a pressure plate 30, a first movable groove 31, an elastic groove 32, a driven roller 33, an elastic sheet 34, a first movable plate 35, a connecting rod 36, an electric push rod 37, a receiving groove 38, a guide block 39, a first spring 40, a cutting plate 41, a second movable groove 42, a second movable plate 43, a threaded rotating rod 44, a pressure rod 45, a first clamping roller 46, a second clamping roller 47, a wide-mouth groove 48, a through groove 49, a slide 50, a slider 51, a bidirectional blade 52, a bracket 53, a reciprocating motor 54 and a second spring 55. One end of the base 1 is fixedly connected to the power frame 25, and the power frame 25 is located at one end of the guide air plate 20. The power frame 25 The top of the power frame 25 is connected with two groups of power rollers 26 through bearings, and one end of the power rollers 26 extends to the outside of the power frame 25, and one end of the power rollers 26 is fixedly connected with a rotating member 27, and a second motor 28 is provided at the bottom end of the power frame 25, and a belt 29 is provided at one end of the power frame 25, and the inner wall of the belt 29 fits with the output end of the second motor 28 and the rotating member 27, and a pressing plate 30 is provided at the top of the power frame 25, and first movable grooves 31 are symmetrically opened at both ends of the pressing plate 30, and elastic grooves 32 are opened in the middle of the first movable grooves 31, and two groups of driven rollers 33 are provided at the bottom end of the pressing plate 30, and both ends of the driven rollers 33 are located inside the first movable groove 31, and elastic sheets 34 are fixedly connected to the inside of the elastic grooves 32, and both ends of the driven rollers 33 are fixed. The first movable plate 35 is slidably connected to the middle part of the power frame 25, and the two ends of the power frame 25 are symmetrically slidably connected to the connecting rod 36, and the two ends of the connecting rod 36 are respectively fixedly connected to the pressure plate 30 and the first movable plate 35. The bottom end of the first movable plate 35 is provided with an electric push rod 37, and the bottom end of the electric push rod 37 is fixedly connected to the base 1. The top of the power frame 25 is evenly provided with a receiving groove 38, and the inside of the receiving groove 38 is slidably connected with a guide block 39, and the bottom end of the guide block 39 is fixedly connected to the first spring 40, and the bottom end of the first spring 40 is fixedly connected to the inner wall of the receiving groove 38, the top of the guide block 39 is in contact with the bottom end of the pressure plate 30, and one end of the base 1 is fixedly connected A cutting plate 41 is connected, and the cutting plate 41 is located on one side of the power frame 25. A second movable groove 42 is opened in the middle and upper part of the cutting plate 41. A second movable plate 43 is slidably connected inside the second movable groove 42. A pressure rod 45 is slidably connected inside the second movable groove 42, and the pressure rod 45 is located at the bottom end of the second movable plate 43. The top of the cutting plate 41 is connected to a threaded rotating rod 44 through a thread, and the bottom end of the threaded rotating rod 44 is connected to the top end of the second movable plate 43 through a bearing. The bottom end of the second movable plate 43 is evenly fixedly connected with a second spring 55, and the bottom ends of the second springs 55 are all fixedly connected to the top end of the pressure rod 45. Two groups of first clamping rollers 46 are connected to the middle part of the cutting plate 41 through bearings, and the bottom end of the pressure rod 45 is connected to two groups of second clamping rollers 47 through bearings.The surfaces of the first clamping roller 46 and the second clamping roller 47 are uniformly provided with corresponding wire grooves, one side of the cutting plate 41 is uniformly provided with a wide-mouth groove 48, and the other side of the cutting plate 41 is uniformly provided with a through groove 49, and the central axis of the wide-mouth groove 48, the through groove 49 and the wire groove on the surface of the first clamping roller 46 coincides, one side of the cutting plate 41 is provided with two groups of inclined slide grooves 50, and the angle between the slide groove 50 and the vertical direction is thirty degrees, and the inside of the slide groove 50 is slidably connected with a slider 51, a bidirectional blade 52 is provided on one side of the cutting plate 41, and both ends of the bidirectional blade 52 are fixedly connected to the slider 51, and a reciprocating motor 54 is provided on one side of the cutting plate 41, and the output end of the reciprocating motor 54 is fixedly connected to a bracket 53, and the bracket The two ends of 53 are fixedly connected with the two ends of the bidirectional blade 52, the bracket 53 is located at the top of the bidirectional blade 52, the wide-mouth slot 48 is trumpet-shaped, and the size of the smaller end of the wide-mouth slot 48 is the same as the diameter of the through slot 49. The control ends of the second motor 28, the electric push rod 37 and the reciprocating motor 54 are all electrically connected to the external power supply through an external switch. The user controls the electric push rod 37 to work through the first movable plate 35 and the connecting rod 36 to make the pressing plate 30 and the driven roller 33 rise. The user passes the material column through the power frame 25 and the driven roller 33, and at the same time makes the material column between the two sets of guide blocks 39, and separates the material column through the guide blocks 39. The user then controls the pressing plate 30 to reset, and at this time, the material column is pushed by the driven roller 33 The elastic sheet 34 is pressed downward, thereby deforming the elastic sheet 34. At the same time, the elastic force of the elastic sheet 34 itself presses the driven roller 33 downward, so that the material column is tightly located between the power roller 26 and the driven roller 33. The output end of the second motor 28 can drive the rotating member 27 to rotate through the belt 29, and the rotating member 27 drives the power roller 26 to rotate, so that the power roller 26 can provide power for the movement of the material column. The user passes the material column through the wide-mouth groove 48 and the through-groove 49. The horn-shaped wide-mouth groove 48 facilitates the penetration of the material column. At this time, the material column is between the first clamping roller 46 and the second clamping roller 47. The user can move the second movable plate 43 downward and compress the second spring 55 by rotating the threaded rotating rod 44. At this time, under the action of the second spring 55's own rebound force, the second clamping roller 47 at the bottom of the pressure rod 45 can clamp the material column. At this time, the material column is in the wire groove on the surface of the first clamping roller 46 and the second clamping roller 47. When the material column moves forward, the material column rotates with the first clamping roller 46 and the second clamping roller 47. At the same time, the output end of the reciprocating motor 54 drives the bracket 53, the bracket 53 and the slider 51 to reciprocate. The slider 51 and the slide 50 can limit the movement direction of the bidirectional blade 52 to ensure that the bidirectional blade 52 can be inclined to cut the material column when it is in reciprocating motion, thereby making the shearing work of the bidirectional blade 52 more convenient. The user can collect the small material column sheared.

[0139] The working principle of the twin-screw granulation in Example 19: When the user needs to use the device for granulation, the user controls the device to work automatically, the user adds the mixed material to the vibrating feeder 9, and the vibrating feeder 9 automatically discharges the material, the first motor 6 drives the first gear 5 and the spiral material column 4 to rotate through the second gear 7, and at the same time the heater 3 heats the material inside the extrusion bin 2, and the heated material is extruded through the extrusion nozzle 8 through two groups of rotating spiral material columns 4, and the extruded material column enters the cooling tank 10, so that the material column is located between each group of guide positioning columns 12. After the material column passes through the cooling tank 10, the user places the lower pressure net 11 inside the cooling tank 10, positions it through the guide positioning columns 12, and supports it through the support plate 13. At this time The material column can be immersed in cooling water through the cooling trough 10 and the lower pressure net 11, so as to facilitate the cooling treatment of the material column. The material column passes through the guide air plate 20 and the blowing plate 21. The cooling water can be circulated internally through the water pipe 15 and the water pump 16. The circulating cooling water can be cooled by the fan 18 and the heat dissipation fins 17. The heat conduction between the heat dissipation fins 17 and the hot water is generated. The heat at the bottom of the heat dissipation fins 17 is blown away by the fan 18, and the hot air is collected by the air collecting box 19, and then enters the interior of the first air pipe 22 through the second air pipe 23, and then enters the interior of the blowing plate 21 through the first air pipe 22, and finally blows to the surface of the material column through the blowing plate 21, so as to dry the material column, and the water blown down The beads are collected by the guide air plate 20 and flow into the cooling tank 10. The temperature of the hot air entering the second air pipe 23 can be detected by the intelligent thermostat 24. If the temperature cannot reach the set temperature, the intelligent thermostat 24 is used for heating to meet the drying requirements. The hot air generated by cooling is used to dry the material column, thereby reducing the user's production cost and energy consumption. The user controls the electric push rod 37 to work through the first movable plate 35 and the connecting rod 36 to make the pressing plate 30 and the driven roller 33 rise. The user passes the material column through the power frame 25 and the driven roller 33, and at the same time makes the material column between the two sets of guide blocks 39. The material column is separated by the guide blocks 39, and the user controls the pressing plate 30 to reset. At this time The driven roller 33 presses down the material column, so that the elastic sheet 34 is deformed, and at the same time, the elastic force of the elastic sheet 34 presses the driven roller 33 downward, so that the material column is tightly located between the power roller 26 and the driven roller 33. The output end of the second motor 28 can drive the rotating member 27 to rotate through the belt 29, and the rotating member 27 drives the power roller 26 to rotate, so that the power roller 26 can provide power for the movement of the material column. The user passes the material column through the wide-mouth groove 48 and the through groove 49. The horn-shaped wide-mouth groove 48 facilitates the penetration of the material column. At this time, the material column is between the first clamping roller 46 and the second clamping roller 47. The user can move the second movable plate 43 downward and compress the second spring 55 by rotating the threaded rotating rod 44.At this time, under the action of the second spring 55's own rebound force, the second clamping roller 47 at the bottom of the pressure rod 45 can clamp the material column. At this time, the material column is in the wire groove on the surface of the first clamping roller 46 and the second clamping roller 47. When the material column moves forward, the material column rotates with the first clamping roller 46 and the second clamping roller 47. At the same time, the output end of the reciprocating motor 54 drives the bracket 53, the bracket 53 and the slider 51 to reciprocate. The slider 51 and the slide 50 can limit the movement direction of the bidirectional blade 52 to ensure that the bidirectional blade 52 can be inclined to shear the material column when it is in reciprocating motion, thereby making the shearing work of the bidirectional blade 52 more convenient. The user can collect the small material column sheared. At this time, the granulation work is completed. The device is fully automated, which is convenient for users to use. At the same time, the device can recycle the hot air generated by cooling, thereby reducing the user's use cost. At the same time, the device can automatically and quickly perform shearing work, and can ensure the quality of shearing and the same shearing length.

[0140] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and range of equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing a salt-alkali resistant degradable mulch film, characterized in that: The salt-alkali resistant degradable mulch film comprises at least one inner layer, wherein the inner layer comprises the following components calculated by weight percentage: 5-50 parts of corrosion resistant additives, 40-90 parts of PBAT, 0.1-10 parts of epoxy chain extender ADR4468, 0.1-10 parts of plasticizer epoxy soybean oil, 0.1-10 parts of coupling agent, 0.1-10 parts of nucleating agent, and 0.1-10 parts of anti-hydrolysis agent; The preparation method of the salt-alkali resistant degradable mulch film comprises the following steps: (1) Granulation of composite materials: Determine the raw material components of the composite materials to be processed according to the type of salt-alkali resistant degradable mulch film to be produced, weigh the corresponding raw materials according to the weight ratio of each raw material component in the corresponding formula, mix them evenly for 30-40 minutes, and put them into the twin-screw granulator for granulation to obtain different composite materials; The twin-screw granulator in the preparation method comprises a base (1), a guide air plate (20), a cooling and drying mechanism and a power shearing mechanism, wherein an extrusion bin (2) is arranged at one end of the base (1), a heater (3) is evenly arranged on the surface of the extrusion bin (2), two groups of spiral material columns (4) are arranged inside the extrusion bin (2), and both ends of the spiral material columns (4) are connected to the extrusion bin (2) through bearings, one end of the spiral material columns (4) is fixedly connected to a first gear (5), and the first gear (5) is located outside the extrusion bin (2), one end of the base (1) is arranged with a first motor (6), the output end of the first motor (6) is fixedly connected to a second gear (7), and the second gear (7) is meshed with the first gear (5), one end of the extrusion bin (2) is arranged with an extrusion nozzle (8), and the other end of the extrusion bin (2) is arranged with a vibrating feeder (9), and the control ends of the first motor (6) and the vibrating feeder (9) are electrically connected to an external power supply through an external switch; The cooling and drying mechanism comprises a cooling trough (10), a downward pressure net (11), a guide positioning column (12), a support plate (13), a cooling box (14), a water pipe (15), a water pump (16), a heat dissipation fin (17), a fan (18), an air collecting box (19), an air blowing plate (21), a first air pipe (22), a second air pipe (23) and an intelligent temperature controller (24). A cooling trough (10) is arranged in the middle of the top of the base (1), a downward pressure net (11) is arranged inside the cooling trough (10), and four groups of support plates (13) are fixedly connected to the inner wall of the middle of the cooling trough (10), and the support plates (13) are arranged on the inner wall of the cooling trough (10). The top of the plate (13) is in contact with the bottom of the lower pressure net (11); the inner wall of the bottom of the cooling trough (10) is fixedly connected with ten groups of guide positioning columns (12); the guide positioning columns (12) are respectively located at the corners of the cooling trough (10); the guide positioning columns (12) are slidably connected with the lower pressure net (11); a cooling box (14) is provided at the bottom of the cooling trough (10); one end of the cooling box (14) is connected to one end of the cooling trough (10); the other end of the cooling box (14) is connected to a water pipe (15); one end of the water pipe (15) is connected to one end of the cooling trough (10); A water pump (16) is arranged in the middle of the water pipe (15); the interior of the cooling box (14) is evenly and fixedly connected with heat dissipation fins (17), and the bottom ends of the heat dissipation fins (17) are all in contact with the top of the base (1); a fan (18) is arranged at the bottom end of the cooling box (14), and the fan (18) is located on one side of the heat dissipation fins (17); one end of the heat dissipation fins (17) is fixedly connected with an air collecting box (19), and one end of the air collecting box (19) is connected to a second air pipe (23); one end of the cooling tank (10) is fixedly connected with a guide air plate (20), and the guide air plate ( 20) one end connected to the cooling trough (10) is lower than the other end of the guide air plate (20), a blowing plate (21) is arranged at the top of the guide air plate (20), and the blowing plate (21) is parallel to the guide air plate (20), both ends of the blowing plate (21) are connected to a first air pipe (22), and one end of the first air pipe (22) is connected to one end of a second air pipe (23), one end of the second air pipe (23) is provided with an intelligent temperature controller (24), and the control ends of the water pump (16), the fan (18) and the intelligent temperature controller (24) are electrically connected to an external power supply through an external switch; The power shearing mechanism comprises a power frame (25), a power roller (26), a rotating member (27), a second motor (28), a belt (29), a pressure plate (30), a first movable groove (31), an elastic groove (32), a driven roller (33), an elastic sheet (34), a first movable plate (35), a connecting rod (36), an electric push rod (37), a receiving groove (38), a guide block (39), a first spring (40), a cutting plate (41), a second movable groove (42), a second movable plate (43), a threaded rotating rod (44), a pressure rod (45), a first clamping roller (46), a second clamping roller (47), a wide-mouth groove (48), a threading groove (49), a sliding groove (50), a sliding block (51), a bidirectional blade (52), a bracket ( 53), a reciprocating motor (54) and a second spring (55), one end of the base (1) is fixedly connected to a power frame (25), and the power frame (25) is located at one end of the guide air plate (20), the top of the power frame (25) is connected to two groups of power rollers (26) through bearings, and one end of the power rollers (26) extends to the outside of the power frame (25), one end of the power rollers (26) is fixedly connected to a rotating member (27), the bottom end of the power frame (25) is provided with a second motor (28), one end of the power frame (25) is provided with a belt (29), and the inner wall of the belt (29) is in contact with the output end of the second motor (28) and the rotating member (27), and the top of the power frame (25) is provided with a pressure plate (30), both ends of the pressure plate (30) are symmetrically provided with first movable grooves (31), the middle of the first movable grooves (31) are provided with elastic grooves (32), the bottom end of the pressure plate (30) is provided with two sets of driven rollers (33), and both ends of the driven rollers (33) are located inside the first movable grooves (31), the inside of the elastic grooves (32) are fixedly connected with elastic sheets (34), both ends of the driven rollers (33) are fixedly connected with bearings, and the surface of the bearings is in contact with the middle of the elastic sheets (34), the middle and lower part of the power frame (25) is slidably connected with the first movable plate (35), both ends of the power frame (25) are symmetrically slidably connected with connecting rods (36), and both ends of the connecting rods (36) They are respectively fixedly connected to the pressing plate (30) and the first movable plate (35); the bottom end of the first movable plate (35) is provided with an electric push rod (37), and the bottom end of the electric push rod (37) is fixedly connected to the base (1); the top of the power frame (25) is evenly provided with receiving grooves (38); the inside of the receiving grooves (38) is slidably connected with guide blocks (39); the bottom ends of the guide blocks (39) are fixedly connected with first springs (40), and the bottom ends of the first springs (40) are fixedly connected to the inner wall of the receiving grooves (38); the top ends of the guide blocks (39) are in contact with the bottom end of the pressing plate (30); one end of the base (1) is fixedly connected with a cutting plate (41), and the cutting plate (41) is located on one side of the power frame (25);A second movable groove (42) is provided in the middle upper part of the cutting plate (41), the interior of the second movable groove (42) is slidably connected to the second movable plate (43), the interior of the second movable groove (42) is slidably connected to a pressure rod (45), and the pressure rod (45) is located at the bottom end of the second movable plate (43), the top end of the cutting plate (41) is connected to a threaded rotating rod (44) via a thread, and the bottom end of the threaded rotating rod (44) is connected to the top end of the second movable plate (43) via a bearing, and the bottom end of the second movable plate (43) is evenly A second spring (55) is fixedly connected, and the bottom end of the second spring (55) is fixedly connected to the top end of the pressure rod (45); the middle part of the cutting plate (41) is connected to two sets of first clamping rollers (46) through bearings, and the bottom end of the pressure rod (45) is connected to two sets of second clamping rollers (47) through bearings; the surfaces of the first clamping rollers (46) and the second clamping rollers (47) are uniformly provided with corresponding wire grooves; one side of the cutting plate (41) is uniformly provided with wide-mouth grooves (48), and the other side of the cutting plate (41) is uniformly provided with wide-mouth grooves (48). A through groove (49) is provided, and the central axes of the wire grooves opened on the surfaces of the wide-mouth groove (48), the through groove (49) and the first clamping roller (46) coincide with each other. Two sets of inclined slide grooves (50) are opened on one side of the cutting plate (41), and the angle between the slide grooves (50) and the vertical direction is thirty degrees. The insides of the slide grooves (50) are slidably connected with sliders (51). A bidirectional blade (52) is provided on one side of the cutting plate (41), and both ends of the bidirectional blade (52) are fixedly connected to the slider (51). One side of the cutting plate (41) A reciprocating motor (54) is provided, the output end of the reciprocating motor (54) is fixedly connected to a bracket (53), and the two ends of the bracket (53) are fixedly connected to the two ends of the bidirectional blade (52), the bracket (53) is located at the top of the bidirectional blade (52), the wide-mouthed slot (48) is trumpet-shaped, the size of the smaller end of the wide-mouthed slot (48) is the same as the diameter of the through slot (49), and the control end of the second motor (28), the electric push rod (37) and the reciprocating motor (54) are all electrically connected to an external power supply through an external switch; (2) Add different composite materials into the corresponding feed bin of the three-layer co-extrusion film blowing machine respectively; (3) Adjust the temperature of the film blowing machine to 190-200℃ in zone 1, 170-180℃ in zone 2, 160-170℃ in zone 3, 150-160℃ in zone 4, 140-150℃ in zone 5, main machine speed to 10-30rpm, and traction speed to 10-30rpm; (4) Start the film blowing machine, and obtain the salt-alkali resistant and degradable ground film through film blowing and winding.

2. The method for preparing a salt-alkali resistant degradable mulch film according to claim 1, characterized in that: It also includes a middle layer, the weight ratio of the inner layer to the middle layer is 1-10:1-10, and the middle layer includes the following components calculated by weight percentage: 30-50 parts of PBAT, 0-30 parts of PHA, 0-30 parts of PGA, 0-30 parts of PCL, 0-30 parts of PPC, 0-80 parts of PBST, 0.1-10 parts of compatibilizer HP441, 0.1-10 parts of nucleating agent, 0.1-10 parts of epoxy chain extender ADR4468, 0.1-10 parts of plasticizer epoxy soybean oil, and 0.1-10 parts of anti-hydrolysis agent.

3. The method for preparing a salt-alkali resistant degradable mulch film according to claim 1, characterized in that: It also includes an outer layer, the weight ratio of the inner layer to the outer layer is 1-10:1-10, and the outer layer includes the following components calculated by weight percentage: 50-90 parts of PBAT, 10-30 parts of PLA, 0.1-10 parts of epoxy chain extender ADR4468, 0.1-10 parts of plasticizer epoxy soybean oil, 0.1-10 parts of coupling agent, 0.1-10 parts of nucleating agent, 0.1-10 parts of anti-hydrolysis agent, 0.1-10 parts of antioxidant, 0.1-10 parts of anti-ultraviolet agent, 10-30 parts of straw, and 1-10 parts of degradable black masterbatch.

4. The method for preparing a salt-alkali resistant degradable mulch film according to claim 1, characterized in that: It also includes a middle layer and an outer layer, wherein the weight ratio of the inner layer, the middle layer and the outer layer is 1-10:1-10:1-10, and the middle layer includes the following components calculated by weight percentage: 30-50 parts of PBAT, 0-30 parts of PHA, 0-30 parts of PGA, 0-30 parts of PCL, 0-30 parts of PPC, 0-80 parts of PBST, 0.1-10 parts of compatibilizer HP441, 0.1-10 parts of nucleating agent, 0.1-10 parts of epoxy chain extender ADR4468, 0.1-10 parts of plasticizer epoxidized soybean oil, and 0.1-10 parts of anti-hydrolysis agent; the outer layer includes the following components calculated by weight percentage: 50-90 parts of PBAT, 10-30 parts of PLA, epoxy chain extender ADR4468 0.1-10 parts, plasticizer epoxidized soybean oil 0.1-10 parts, coupling agent 0.1-10 parts, nucleating agent 0.1-10 parts, anti-hydrolysis agent 0.1-10 parts, antioxidant 0.1-10 parts, anti-ultraviolet agent 0.1-10 parts, straw 10-30 parts, degradation black masterbatch 1-10 parts.

5. The method for preparing a salt-alkali resistant degradable mulch film according to any one of claims 1 to 4, characterized in that: The corrosion-resistant additive includes at least one of silicon dioxide, calcium carbonate, talcum powder, glass fiber, rice husk extract, clay, and biochar.

6. A method for preparing a salt-alkali resistant degradable mulch film according to any one of claims 1 to 4, characterized in that: The coupling agent is one of KH550, KH560, KH570 or titanate coupling agent.

7. The method for preparing a salt-alkali resistant degradable mulch film according to claim 3, characterized in that: The anti-ultraviolet agent is UV-531 or UV-327.

8. The method for preparing a salt-alkali resistant degradable mulch film according to claim 3, characterized in that: The nucleating agent is preferably BTD-8808, the anti-hydrolysis agent is preferably BTWR-500, and the antioxidant is preferably 1010.

9. The method for preparing a salt-alkali resistant degradable mulch film according to claim 1, characterized in that: In the step (1), the temperature of the twin-screw granulator is 180-200°C in zone 1, 180-200°C in zone 2, 160-180°C in zone 3, 160-180°C in zone 4, and 140-160°C in zone 5; the main engine speed is 60-100rpm, and the feeding rate is 40-120rpm.

Citation Information

Patent Citations

  • Preparation method of three-layer co-extrusion whole-biodegradable mulching film and the three-layer co-extrusion whole-biodegradable mulching film

    CN106363898A

  • Full-biodegradation mulch film for rice planting and production method thereof

    CN106633704A

  • Three-layer co-extrusion full-degradable mulching film and production process thereof

    CN110583326A

  • Environment-friendly plastic granulator with adjustable granulation size and using method of environment-friendly plastic granulator

    CN112809966A

  • Full-biodegradable mulching film for peanut planting

    CN113841551A