A polymer conductive film containing conductive additives and preparation method thereof
By coating a conductive emulsion containing carbon black particles grafted with conductive polymers and conductive chain extenders onto the surface of a polymer film substrate, the problems of reduced mechanical strength and uneven dispersion caused by high amounts of conductive agents are solved, thus achieving excellent conductivity and processability of the polymer conductive film.
Patent Information
- Application Number
- CN202410583510.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-05-11
AI Technical Summary
In existing methods for preparing polymer conductive films, the large amount of conductive agent added leads to a decrease in mechanical strength, and the conductive additives are difficult to disperse uniformly, affecting conductivity.
By coating a conductive emulsion onto the surface of a polymer film substrate, carbon black particles grafted with conductive polymers are used as conductive additives, and combined with conductive chain extenders, a stable conductive pathway is formed, preventing the aggregation of carbon black particles.
A good balance between conductivity and mechanical strength of polymer conductive films is achieved, making them suitable for large-scale production, and the preparation method is simple and efficient.
Smart Images

Figure CN118185109B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials, and in particular to a polymer conductive film containing a conductive additive and a preparation method thereof. Background Art
[0002] With the rapid development of science and technology, the field of electronic materials is undergoing unprecedented changes. Among them, polymer conductive film, as a new type of electronic material, has a wide range of applications due to its unique properties. For example, in the field of electronic devices, polymer conductive film can be used to make capacitors, resistors, etc. In the field of energy, polymer conductive film can be used to prepare solar cells, supercapacitors and other energy storage devices. Therefore, the preparation of high-performance polymer conductive film is gradually attracting widespread attention from scientific researchers and the industrial community.
[0003] At present, the preparation method of polymer conductive film is mainly through mixing conductive agents such as graphene with polymer materials such as polyimide, and then forming them through extrusion and film pressing processes. Generally speaking, in order to make the prepared polymer conductive film exhibit good conductivity, a large amount of conductive agent is generally required to be added. However, this method will cause the mechanical strength of the polymer film to drop sharply and lack processability. Therefore, this method has major defects in practical applications and is not conducive to large-scale production. Based on this, it is of great significance to develop a new method for preparing polymer conductive film.
[0004] Research has found that by coating the surface of a polymer film substrate with a conductive slurry, a conductive layer can be formed on the surface of the polymer film, thereby giving the film good conductive properties. This method is simple to operate and will not destroy the mechanical properties of the polymer film itself. It has strong processability and is suitable for large-scale promotion. However, conductive additives also need to be added to the conductive slurry. Since the conductive additives themselves are easy to agglomerate, it is difficult to achieve uniform dispersion and form a stable conductive path, which in turn has a significant negative impact on the conductive properties of the polymer conductive film. Summary of the invention
[0005] In order to solve the technical problems mentioned in the background technology, the object of the present invention is to provide a polymer conductive film containing conductive additives and a preparation method thereof.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A polymer conductive film containing a conductive additive, comprising a film substrate and a conductive coating; the conductive coating is formed by coating a conductive slurry on the surface of the film substrate and drying it;
[0008] The conductive emulsion comprises the following raw materials in parts by weight:
[0009] 50-60 parts of modified polyurethane prepolymer emulsion;
[0010] Conductive additive 4-8 parts;
[0011] The preparation method of the conductive emulsion is as follows:
[0012] Adding conductive additives to the modified polyurethane prepolymer emulsion, stirring and mixing at a rate of 1000-2000 r / min for 20-30 minutes, standing for degassing, and discharging to obtain a polyurethane conductive emulsion;
[0013] The conductive additive is carbon black particles with conductive high molecular polymer grafted on the surface.
[0014] A method for preparing a polymer conductive film containing a conductive additive is as follows:
[0015] Use the scraping method to evenly coat the conductive slurry on the surface of the film substrate, and control the coating amount to 15-30g / cm 2 After coating, it is dried at a temperature of 80-100°C to obtain a polymer conductive film.
[0016] As a further embodiment of the present invention, the method for preparing the conductive additive comprises the following steps:
[0017] Step A, p-phenylenediamine and purified water are mixed to form a mixed solution, concentrated nitric acid is added to the mixed solution, and then sodium nitrite is added to the mixed solution at a temperature of 0-10° C., and then carbon black particles are added. After the addition is completed, the mixture is stirred and dispersed evenly, and the mixture is kept for 4-6 hours, and the material is discharged to obtain a carbon black intermediate;
[0018] Step B: Mix the carbon black intermediate and purified water, and after ultrasonic treatment to form a dispersion, add sodium dodecylbenzene sulfonate to the dispersion and stir evenly, then add thiophene and a promoter to the dispersion, keep it warm at 60-70°C for 6-8h, then add 3,4-ethylenedioxythiophene, and after the addition, raise the temperature to 75-85°C, keep it warm and stir for 12-16h, cool it down and discharge it, and the conductive additive can be obtained.
[0019] The principle of the above scheme is: first, aniline groups are introduced on the surface of carbon black particles through diazotization reaction to obtain carbon black intermediates, and then the aniline groups are used as initiation sites to initiate in situ polymerization of thiophene monomers and 3,4-ethylenedioxythiophene monomers on the surface of carbon black to form carbon black particles with thiophene conductive polymers grafted on the surface, i.e., conductive additives.
[0020] As a further embodiment of the present invention, in step A, the average particle size of the carbon black particles is 5 μm.
[0021] As a further embodiment of the present invention, in step B, the accelerator is ferric chloride or aluminum chloride.
[0022] As a further embodiment of the present invention, the preparation method of the modified polyurethane prepolymer emulsion comprises the following steps:
[0023] Step A1, vacuum dehydrating the polyether polyol at 100-110° C. for 1-2 hours, lowering the temperature to 60-70° C., adding a diisocyanate monomer and a tin catalyst, stirring and mixing, and keeping the mixture warm in a nitrogen atmosphere for 2-3 hours to form a prepolymer;
[0024] Step A2, lowering the temperature to 50-60°C, then adding the conductive chain extender to the prepolymer, stirring continuously for 2-4 hours, stopping heating, cooling and discharging the material, and obtaining a modified polyurethane prepolymer emulsion.
[0025] The principle of the above technical solution is: using polyether polyol as a soft segment and diisocyanate as a hard segment, prepolymerization is carried out under the action of a tin catalyst to form a prepolymer, and then polypyrrole containing a large number of active hydroxyl groups in the structure is used as a chain extender to carry out chain extension polymerization to form a modified polyurethane prepolymer emulsion with a branched polyurethane molecular chain structure.
[0026] As a further embodiment of the present invention, in step A1, the diisocyanate monomer is any one of toluene-2,4-diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate or diphenylmethane-4,4'-diisocyanate.
[0027] As a further embodiment of the present invention, in step A1, the tin catalyst is any one of stannous octoate, dibutyltin didodecylsulfide or dibutyltin dilaurate.
[0028] As a further embodiment of the present invention, the preparation method of the conductive chain extender is as follows:
[0029] The polypyrrole and N,N-dimethylformamide are stirred and mixed to form a uniform solution, and then halogenated alcohol and potassium hydroxide are added to the solution. After the addition is completed, heating is turned on and the temperature is controlled at 60-70°C. After maintaining the temperature for 4-6 hours under continuous stirring, the material is cooled and discharged to obtain a conductive chain extender.
[0030] As a further embodiment of the present invention, the halogenated alcohol is any one of 3-bromo-1-propanol, 4-bromo-1-butanol, 5-bromo-1-pentanol, 8-bromo-1-octanol or 11-bromo-1-undecanol.
[0031] The principle of the above technical solution is that the polypyrrole structure contains a large number of secondary amine groups, which can be replaced by the halogen in the halohydrin structure under the action of an alkaline catalyst, thereby introducing a large number of active hydroxyl groups into the polypyrrole structure to obtain a conductive chain extender containing a large number of active hydroxyl groups in the structure.
[0032] Beneficial effects of the present invention:
[0033] (1) The present invention first prepares a conductive additive by modifying the surface of carbon black particles with a conductive high molecular polymer. The conductive high molecular polymers can generate a large steric hindrance, thereby avoiding mutual contact and aggregation between carbon black particles, thereby greatly improving the dispersibility of the carbon black particles and enabling them to be uniformly present in the conductive paste. In addition, the aniline groups modified by the diazotization reaction of the carbon black particles can participate in the drying and curing process of the conductive paste, thereby being able to be closely combined with the polyurethane, thereby avoiding falling off from the coating surface during use, resulting in a decrease in conductive performance.
[0034] (2) In order to compensate for the phenomenon that the conductive path is disconnected due to the separation of carbon black particles, the present invention prepares a polyurethane containing a conductive chain extender as a film-forming material, fills the gaps between the carbon black particles with conductive polymers, and then cooperates with the carbon black particles to form a stable conductive path. Therefore, it is possible to achieve the effect of adding a small amount of conductive additives to make the coating formed by curing the conductive slurry exhibit excellent conductive properties.
[0035] (3) The present invention forms a polymer film having a conductive coating on the surface by coating a conductive paste having high conductivity on the surface of the polymer film substrate, thereby avoiding the problem of reducing the strength of the polymer film due to the addition of a large amount of conductive agent. In addition, the preparation method is simple and efficient and is suitable for large-scale application.
[0036] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0038] Figure 1 This is the infrared analysis test diagram of the conductive chain extender. DETAILED DESCRIPTION
[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Example 1
[0041] 1. Preparation of conductive additives
[0042] Step A, 0.1 g of p-phenylenediamine and purified water are mixed to form a mixed solution, 0.5 mL of concentrated nitric acid is added to the mixed solution, then 0.06 g of sodium nitrite is added to the mixed solution at a temperature of 0° C., and then 4.5 g of carbon black particles with an average particle size of 5 μm are added. After the addition is completed, the mixture is stirred and dispersed evenly, and the mixture is kept for 6 hours, and the material is discharged to obtain a carbon black intermediate;
[0043] Step B: 1.4 g of carbon black intermediate and purified water are mixed, and after ultrasonic treatment to form a dispersion, 1.5 g of sodium dodecylbenzene sulfonate is added to the dispersion and stirred evenly. Then, 1.8 g of thiophene and 10 g of ferric chloride are added to the dispersion, and after keeping warm at 65 ° C for 8 hours, 0.5 g of 3,4-ethylenedioxythiophene is added. After the addition is completed, the temperature is raised to 80 ° C, and after keeping warm and stirring for 12 hours, the temperature is lowered and the material is discharged to obtain a conductive additive.
[0044] 1g of conductive additive sample was taken and analyzed using a PE-2400 element analyzer. The results showed that the percentage of nitrogen in the conductive additive was 1.08%, and the percentage of sulfur was 5.84%. It can be reasonably inferred that the nitrogen element came from the aniline introduced by the diazotization reaction, and the sulfur element came from the conductive polymer chain segment produced by the polymerization of thiophene and 3,4-ethylenedioxythiophene.
[0045] 2. Preparation of modified polyurethane prepolymer emulsion
[0046] Step A1, 3.5 g of polypyrrole and N,N-dimethylformamide were stirred and mixed to form a uniform solution, and then 1.2 g of 3-bromo-1-propanol and 1.5 g of potassium hydroxide were added to the solution. After the addition was completed, heating was turned on and the temperature was controlled at 65° C., and the mixture was kept under continuous stirring for 4 hours, and then the temperature was lowered and the material was discharged to obtain a conductive chain extender;
[0047] Take the conductive chain extender sample, make it into potassium bromide tablets, and conduct infrared analysis test. The results are shown in Figure 1 , of which 3391cm -1 The absorption peak at 3310 cm is the stretching vibration absorption peak of the secondary amine NH that does not participate in the reaction. -1The absorption peak at 2900 cm is the OH stretching vibration absorption peak of the hydroxyl group. -1 ~3000cm -1 The absorption peak at 1572 cm is the CH stretching vibration absorption peak in the methylene group. -1 The absorption peak at 1406 cm is the CC stretching vibration absorption peak of the pyrrole ring. -1 The absorption peak at is the CN stretching vibration absorption peak.
[0048] Step A2, after vacuum dehydrating 12 g of polytetrahydrofuran ether diol at 110° C. for 1 h, the temperature was lowered to 65° C., 8 g of toluene-2,4-diisocyanate and 0.2 g of stannous octoate were added, stirred and mixed, and kept warm in a nitrogen atmosphere for 3 h to form a prepolymer;
[0049] Step A3, lowering the temperature to 55°C, then adding 1.5 g of a conductive chain extender to the prepolymer, stirring for 3 hours, stopping heating, cooling and discharging the material to obtain a modified polyurethane prepolymer emulsion.
[0050] 3. Preparation of Conductive Latex
[0051] Add 4 parts of conductive additive to 50 parts of modified polyurethane prepolymer emulsion, stir and mix at a rate of 1000 r / min for 30 minutes, let it stand for degassing, and discharge the material to obtain a polyurethane conductive emulsion.
[0052] 4. Preparation of polymer conductive film
[0053] Use the scraping method to evenly coat the conductive slurry on the surface of the polyimide film substrate, and control the coating amount to 20g / cm 2 After coating, the polymer conductive film can be obtained by drying at a temperature of 100°C.
[0054] Example 2
[0055] 1. Preparation of Conductive Emulsion
[0056] Add 5 parts of the conductive additive prepared in Example 1 of the present invention to 55 parts of the modified polyurethane prepolymer emulsion prepared in Example 1 of the present invention, stir and mix at a rate of 1500 r / min for 25 minutes, let stand for degassing, and discharge the material to obtain a polyurethane conductive emulsion.
[0057] 2. Preparation of polymer conductive film
[0058] Use the scraping method to evenly coat the conductive slurry on the surface of the polyimide film substrate, and control the coating amount to 20g / cm 2 After coating, the polymer conductive film can be obtained by drying at a temperature of 100°C.
[0059] Example 3
[0060] 1. Preparation of Conductive Emulsion
[0061] 8 parts of the conductive additive prepared in Example 1 of the present invention were added to 60 parts of the modified polyurethane prepolymer emulsion prepared in Example 1 of the present invention, stirred and mixed at a rate of 2000 r / min for 20 minutes, allowed to stand for degassing, and discharged to obtain a polyurethane conductive emulsion.
[0062] 2. Preparation of polymer conductive film
[0063] Use the scraping method to evenly coat the conductive slurry on the surface of the polyimide film substrate, and control the coating amount to 20g / cm 2 After coating, the polymer conductive film can be obtained by drying at a temperature of 100°C.
[0064] Comparative Example 1
[0065] 1. Preparation of Conductive Emulsion
[0066] 5 parts of carbon black particles were added to 55 parts of the modified polyurethane prepolymer emulsion prepared in Example 1 of the present invention, and the mixture was stirred and mixed at a rate of 1500 r / min for 25 minutes, allowed to stand for degassing, and discharged to obtain a polyurethane conductive emulsion.
[0067] 2. Preparation of polymer conductive film
[0068] Use the scraping method to evenly coat the conductive slurry on the surface of the polyimide film substrate, and control the coating amount to 20g / cm 2 After coating, the polymer conductive film can be obtained by drying at a temperature of 100°C.
[0069] Comparative Example 2
[0070] 1. Preparation of Conductive Emulsion
[0071] 5 parts of the conductive additive prepared in Example 1 of the present invention were added to 55 parts of commercially available water-based polyurethane emulsion, stirred and mixed at a rate of 1500 r / min for 25 minutes, allowed to stand for degassing, and discharged to obtain a polyurethane conductive emulsion.
[0072] The commercially available water-based polyurethane emulsion was purchased from Beijing Dongfang Chennuo Chemical Technology Co., Ltd.
[0073] 2. Preparation of polymer conductive film
[0074] Use the scraping method to evenly coat the conductive slurry on the surface of the polyimide film substrate, and control the coating amount to 20g / cm 2 After coating, the polymer conductive film can be obtained by drying at a temperature of 100°C.
[0075] Test Case
[0076] The square resistance of the polymer conductive films prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 and 2 was tested using a four-probe tester. The test results are recorded in Table 1:
[0077] Table 1 - Test results
[0078] , it can be seen from the test results in Table 1 that the high molecular conductive film prepared by coating the film substrate with the conductive slurry prepared in Example 1 of the present invention has a low square resistance and good conductive performance, while the high molecular conductive film prepared by using untreated carbon black particles as conductive additives has a high square resistance and poor conductive performance, which may be due to the carbon black particles agglomerating with each other, resulting in no continuous and stable conductive path formed in the coating formed by the conductive slurry. In Comparative Example 2, a commercially available water-based polyurethane emulsion is used as a film-forming substance, and it is also difficult to form a continuous conductive path, so the conductive performance of the high molecular conductive film prepared is also poor.
[0079] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.
[0080] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A polymer conductive film containing a conductive additive, characterized in that: It includes a film substrate and a conductive coating; the conductive coating is formed by coating a conductive slurry on the surface of the film substrate and drying it; The conductive emulsion comprises the following raw materials in parts by weight: 50-60 parts of modified polyurethane prepolymer emulsion; Conductive additive 4-8 parts; The preparation method of the conductive emulsion is as follows: Adding conductive additives to the modified polyurethane prepolymer emulsion, stirring and mixing at a rate of 1000-2000 r / min for 20-30 minutes, standing for degassing, and discharging to obtain a polyurethane conductive emulsion; The conductive additive is carbon black particles with conductive high molecular polymer grafted on the surface; The preparation method of the conductive additive comprises the following steps: Step A, p-phenylenediamine and purified water are mixed to form a mixed solution, concentrated nitric acid is added to the mixed solution, and then sodium nitrite is added to the mixed solution at a temperature of 0-10° C., and then carbon black particles are added. After the addition is completed, the mixture is stirred and dispersed evenly, and the mixture is kept for 4-6 hours, and the material is discharged to obtain a carbon black intermediate; Step B, mixing the carbon black intermediate and purified water, and after ultrasonic treatment to form a dispersion, adding sodium dodecylbenzene sulfonate to the dispersion, stirring evenly, then adding thiophene and a promoter to the dispersion, keeping the temperature at 60-70° C. for 6-8 hours, and then adding 3,4-ethylenedioxythiophene. After the addition, the temperature is increased to 75-85° C., and after keeping the temperature and stirring for 12-16 hours, the material is cooled and discharged to obtain a conductive additive; The preparation method of the modified polyurethane prepolymer emulsion comprises the following steps: Step A1, vacuum dehydrating the polyether polyol at 100-110° C. for 1-2 hours, lowering the temperature to 60-70° C., adding a diisocyanate monomer and a tin catalyst, stirring and mixing, and keeping the mixture warm in a nitrogen atmosphere for 2-3 hours to form a prepolymer; Step A2, lowering the temperature to 50-60° C., then adding a conductive chain extender to the prepolymer, stirring for 2-4 hours, stopping heating, cooling and discharging the material, and obtaining a modified polyurethane prepolymer emulsion; The preparation method of the conductive chain extender is as follows: The polypyrrole and N,N-dimethylformamide are stirred and mixed to form a uniform solution, and then halogenated alcohol and potassium hydroxide are added to the solution. After the addition is completed, heating is turned on and the temperature is controlled at 60-70°C. After maintaining the temperature for 4-6 hours under continuous stirring, the material is cooled and discharged to obtain a conductive chain extender.
2. The polymer conductive film containing a conductive additive according to claim 1, characterized in that: In step A, the average particle size of the carbon black particles is 5 μm.
3. The polymer conductive film containing a conductive additive according to claim 1, characterized in that: In step B, the accelerator is ferric chloride or aluminum chloride.
4. The polymer conductive film containing a conductive additive according to claim 1, characterized in that: In step A1, the diisocyanate monomer is any one of toluene-2,4-diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate or diphenylmethane-4,4'-diisocyanate.
5. The polymer conductive film containing a conductive additive according to claim 1, characterized in that: In step A1, the tin catalyst is any one of stannous octoate, dibutyltin didodecylsulfide or dibutyltin dilaurate.
6. The polymer conductive film containing a conductive additive according to claim 1, characterized in that: The halogenated alcohol is any one of 3-bromo-1-propanol, 4-bromo-1-butanol, 5-bromo-1-pentanol, 8-bromo-1-octanol or 11-bromo-1-undecanol.
7. A method for preparing a polymer conductive film containing a conductive additive as claimed in claim 1, characterized in that: The preparation method is as follows: Use the scraping method to evenly coat the conductive slurry on the surface of the film substrate, and control the coating amount to 15-30g / cm 2 After coating, it is dried at a temperature of 80-100°C to obtain a polymer conductive film.