Investment casting mold material and preparation method and application thereof

By using paraffin, lignite wax, graphene modified maleic anhydride-vinyl acetate copolymer and tackifying resin in investment casting molds, the problem of insufficient strength and surface hardness of the existing mold material is solved, and the problem of insufficient strength and surface hardness of the existing mold material is achieved. High precision and high quality casting production.

CN118185326BActive Publication Date: 2024-11-22GUANGDONG LEFENG NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410420414.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-09
Publication Date
2024-11-22
Estimated Expiration
2044-04-09

AI Technical Summary

Technical Problem

In the application of existing investment casting molds in China, the injection temperature is low, the strength and surface hardness are low, resulting in low dimensional accuracy, large surface roughness and low quality of castings.

Method used

Using an investment casting mold including paraffin, lignite wax, graphene modified maleic anhydride-vinyl acetate copolymer and tackifying resin, the thermal stability of the mold is improved through specific preparation methods and component ratios. , strength and surface hardness, control shrinkage and ash content.

Benefits of technology

It achieves good thermal stability, high strength, small shrinkage and low ash content of the mold, meets the requirements of high dimensional accuracy and high surface quality of precision castings, and improves the overall performance of castings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004782252130000091
    Figure BDA0004782252130000091
Patent Text Reader

Abstract

The present invention discloses a kind of investment casting mold material and preparation method and application. According to the mass fraction, 40 to 60 parts of paraffin wax are placed in a reactor, firstly heated indirectly by a water jacket, and the temperature is controlled to be below 80°C for partial melting; heated to 100 to 120°C, 5 to 10 parts of lignite wax and 10 to 20 parts of graphene-modified maleic anhydride-vinyl acetate copolymer are added in sequence, stirred and mixed at 50 to 100 rpm, and then 5 to 10 parts of tackifying resin and 0 to 0.01 parts by weight of antioxidant are added after melting, and stirred and mixed evenly; granulated by steel belt material selection and molding technology, sieved, and casting wax particle mold material is obtained. The investment casting mold material of the present invention has good thermal stability, small needle penetration and linear shrinkage, large bending strength, small ash content, and can well meet the requirements of high dimensional accuracy and high surface quality of precision castings, and meet the needs of actual production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of precision casting, and in particular to an investment casting mold material and a preparation method and application thereof. Background Art

[0002] As a near-net-shape molding process, investment casting has the characteristics of high dimensional accuracy and good surface finish. With the widespread application of investment casting in aviation, aerospace and some commercial parts with high dimensional accuracy requirements, the requirements for investment castings are getting higher and higher. The production process of investment casting is relatively complicated and there are many influencing factors. Among them, the production of wax molds is the key link in investment casting production. High-quality wax molds are the premise and guarantee for obtaining high-quality castings. Therefore, the performance of the mold material and the quality of the die will directly affect the dimensional accuracy of the casting. The requirements for mold material performance generally include the following aspects:

[0003] 1. The melting point of the mold material should be moderate. A melting point that is too high or too low is not conducive to the preparation of the mold material, molding and demolding.

[0004] 2. Fluidity The fluidity of the mold material has a very important influence on the injection molding of the wax mold. The mold material with good fluidity can ensure that the mold cavity can be filled during the injection process of the mold material. Otherwise, there will be defects such as incomplete filling and high surface roughness of the wax mold.

[0005] 3. Shrinkage rate: Since the shape and size of the wax mold are the final shape and size of the casting, the shrinkage rate of the mold material is required to be small to ensure the dimensional accuracy of the casting.

[0006] 4. Strength and surface hardness In order to ensure that there is no cracking, wear and surface scratches during mold making, module welding, shell making and transportation, the mold material must have a certain strength and surface hardness after solidification.

[0007] 5. Weldability In order to ensure that a single wax mold can form a module, the mold material must have certain welding properties to ensure the weldability of the module and a certain welding strength after the module is welded.

[0008] 6. Coating performance: After the wax mold is welded, refractory materials and adhesives need to be coated on the wax mold. Therefore, the mold material is required to have good coating performance and be able to form a uniform shell layer to obtain a shell with a smooth surface.

[0009] 7. Ash content Ash content is the residue after the mold material is burned. The mold material remaining in the mold cavity after the shell is fired should be as little as possible to avoid affecting the quality of the casting.

[0010] At present, the mold material mainly used in the investment casting industry in my country has a low injection temperature, but the strength and surface hardness are relatively low, and the shrinkage rate is large. As a result, the resulting castings have low dimensional accuracy, large surface roughness, and low casting quality. Summary of the invention

[0011] In view of the deficiencies in the prior art, the primary purpose of the present invention is to provide an investment casting mold material with good thermal stability, high strength, high hardness, low shrinkage and low ash content.

[0012] Another object of the present invention is to provide a method for preparing the above-mentioned investment casting pattern material.

[0013] Another object of the present invention is to provide application of the above-mentioned investment casting pattern material in precision casting.

[0014] The purpose of the present invention is achieved through the following technical solutions:

[0015] An investment casting mold material comprises the following raw material components in parts by mass:

[0016] 40-60 parts of paraffin wax,

[0017] 5-10 parts of montan wax,

[0018] 10-20 parts of graphene modified maleic anhydride-vinyl acetate copolymer,

[0019] 5 to 10 parts of tackifying resin.

[0020] Furthermore, the graphene-modified maleic anhydride-vinyl acetate copolymer is prepared by the following steps:

[0021] (1) Preparation of graphene-modified horsepower anhydride

[0022] Add graphene oxide and an appropriate amount of DMF into a reaction container, disperse by ultrasonication at 40° C., add maleic anhydride, react by stirring at 80° C., centrifuge, wash, dry, and grind to obtain graphene-modified maleic anhydride; the mass ratio of graphene oxide to maleic anhydride is (1-3): (80-100);

[0023] (2) Preparation of graphene-modified maleic anhydride-vinyl acetate copolymer

[0024] Add toluene, vinyl acetate, graphene-modified maleic anhydride and initiator into a reaction container, heat and stir in a water bath at 63-65°C to react for 15-24 hours to obtain a precipitate, filter, wash and dry the precipitate to obtain a copolymer; the mass ratio of vinyl acetate: graphene-modified maleic anhydride: initiator is 10:(10-15):(0.2-0.5).

[0025] Furthermore, the graphene oxide is prepared by an improved Hummers' method, and the graphene content in the graphene-modified maleic anhydride is 8-12%.

[0026] Furthermore, the paraffin is at least one of 58# fully refined paraffin, 58# semi-refined paraffin, 56# semi-refined paraffin, 54# semi-refined paraffin, 60# fully refined paraffin, 60# semi-refined paraffin, 62# fully refined paraffin, 62# semi-refined paraffin, 64# fully refined paraffin, and 64# semi-refined paraffin.

[0027] Furthermore, the tackifying resin is at least one of C5 / C9 copolymer petroleum resin, C9 hydrogenated petroleum resin, C5 hydrogenated petroleum resin, hydrogenated rosin, disproportionated rosin, and polymerized rosin; and the softening point of the tackifying resin is ≤120°C.

[0028] Furthermore, the investment casting mold material also includes 0 to 0.01 parts by weight of an antioxidant, and the antioxidant can be any antioxidant conventionally used in the art, such as one or more of antioxidant 1010, antioxidant 264, antioxidant 1076, antioxidant 168, and antioxidant 300.

[0029] Furthermore, the investment casting mold material of the present invention also contains additives conventionally used in the art, such as colorants, etc., and the amount thereof can be a conventional amount.

[0030] The above-mentioned method for preparing the investment casting mold material comprises the following steps:

[0031] (1) 40 to 60 parts by weight of paraffin wax are placed in a reaction kettle, firstly heated indirectly by a water jacket, and the temperature is controlled below 80° C. for partial melting;

[0032] (2) heating to 100-120° C., adding 5-10 parts of montan wax and 10-20 parts of graphene-modified maleic anhydride-vinyl acetate copolymer in sequence, stirring and mixing at 50-100 rpm, and then adding 5-10 parts of tackifying resin and 0-0.01 parts by weight of antioxidant after melting, stirring and mixing evenly;

[0033] (3) Granulate and screen the steel belt material selection and molding technology to obtain the casting mold material.

[0034] Furthermore, the steel belt material selection, molding and granulation refers to sending the mixed wax liquid to a distributor, the distributor temperature is 90-100°C, and selecting and molding through the steel belt, the steel belt line speed is 4-5m / min; cold air or cold water is used to cool the wax droplets, the top of the steel belt is cold air cooling, the temperature is ≤20°C, the water cooling during the steel belt transmission is two-stage cooling, the front stage cooling water is room temperature cooling water, the rear stage is ≤10°C cooling water cooling, to obtain a casting mold material.

[0035] As the main component of precision casting mold materials, base wax has the most direct impact on the properties of the mold materials. Therefore, the material properties of base wax must meet the requirements of precision casting mold materials. Base wax is a common material in life or industrial production. Its main chemical composition is hydrocarbon compounds. Some waxes also contain a small amount of higher fatty acids and higher monohydric alcohols. Base wax is a mixed material of organic compounds with the characteristics of low cost, low melting point, low hardness, good flexibility and non-toxicity. Therefore, based on these characteristics, it is widely used in investment casting.

[0036] By properly selecting various wax materials and combining them appropriately, and by properly matching crystalline materials with amorphous materials, a matrix with high toughness is obtained, and then an appropriate amount of polymer materials is added to further strengthen and obtain a certain elasticity, while having various good process properties. Wax materials, especially paraffin as the main body of wax materials, have good plasticity and fluidity, but low strength, large shrinkage, and poor heat resistance, while various tackifying resins are hard and sticky. After they are properly fused, when cooled, the wax material with a higher melting point will first precipitate the crystal nucleus and prevent the formation of paraffin flakes, and then co-crystallize with paraffin. The crystal grains are small and uniform and connected to form a matrix network, and the amorphous resin is dispersed between the crystal grains.

[0037] The tackifying resin selected in the present invention is a typical amorphous material with a high softening point, high surface hardness and low shrinkage. When added to the mold material, the surface hardness of the mold material can be increased, while the shrinkage of the mold material can be reduced, which is conducive to obtaining a high-precision melt mold. However, if too much tackifying resin is added, the mold material will become sticky and easy to stick, which will deteriorate the working conditions and affect the performance of the mold material. Therefore, it is necessary to control the amount of tackifying resin added to the mold material and add other components to enhance the performance of the mold material.

[0038] Add solubility promoter, because wax material and rosin resin are all partially mutually soluble in liquid and solid state, need to add solubility promoter to improve their intermiscibility (compatibility), do not fold out, precipitate of resin in repeated heating, use process.Montane wax is added in the moulding material as the solubility promoter of moulding material, because montan wax and the selected tackifying resin of the present invention have good compatibility, so add tackifying resin again after adding montan wax first, to improve the solubility of tackifying resin in paraffin.In addition, moulding material paste is fine and smooth after adding montan wax, and the wax mould surface finish obtained is high, but montan wax itself melting point is not high, shrinkage ratio is larger, need to control the addition of montan wax.

[0039] By adding a proper amount of high molecular polymer, the wax mold can withstand a certain external force without breaking during operations such as mold removal, and can recover or at least partially restore its original shape after the external force is removed. The high strength, toughness, elasticity and flexibility required by the mold material must be achieved by adding a proper amount of high molecular polymer. The polymer must have good compatibility with the matrix and should not precipitate from the matrix over time during the placement of the wax mold; at the same time, it should not strongly increase the viscosity of the melt at the wax injection temperature; and it should not significantly reduce the cooling rate of the mold material after wax injection.

[0040] Graphene is a two-dimensional structural material composed of a single layer of carbon atoms, and its structure is similar to a honeycomb. Due to the special structure of graphene, it has extremely high mechanical strength and tensile properties. Its mechanical strength is 200 times that of steel and can be stretched to 20% of its own length. Its elastic modulus is very high, about 125 times that of steel. The theoretical value of the elastic modulus is about 0.5 to 1.0 terapascals (TPa). Its expansion coefficient is much smaller than that of three-dimensional materials, reaching 5.7×10 ~6 / K.

[0041] The surface of graphene oxide is rich in reactive groups. MAH monomer undergoes esterification reaction with hydroxyl groups and is inserted into the graphene sheets. The interlamellar spacing is enlarged, the degree of disorder of the crystal layered structure increases, and the regularity is destroyed, which effectively avoids the agglomeration of graphene and is beneficial to improving the dispersion of graphene in the wax matrix and the mechanical properties of the wax matrix.

[0042] The graphene-modified MAH forms a copolymer with vinyl acetate. Since the vinyl acetate monomer is introduced into the molecular chain, the high crystallinity is reduced, and the flexibility, impact resistance and compatibility are improved. At the same time, as a high molecular polymer, the graphene-modified maleic anhydride-vinyl acetate copolymer first precipitates in a dispersed state during the cooling and solidification process of the mold material, and becomes the crystal core when the paraffin solidifies, which plays a role in refining the paraffin grains, thereby refining the grains of the mold material, making the structure dense, reducing the roughness of the mold material, improving the strength of the mold material and increasing the melting point.

[0043] The graphene in the present invention not only has high thermal conductivity, but also can be stably dispersed in the wax mold material system. The graphene-modified maleic anhydride-vinyl acetate copolymer has both grain refining and toughening effects, so that the precision casting mold material prepared by the present invention has high mechanical strength, high stability and good toughness.

[0044] The investment casting mold material of the present invention has good thermal stability, small needle penetration and linear shrinkage, large bending strength and small ash content, and can well meet the requirements of high dimensional accuracy and high surface quality of precision castings and meet the needs of actual production. DETAILED DESCRIPTION

[0045] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0046] The reagents or instruments used in the present invention without indicating the manufacturer are all conventional products that can be purchased from the market.

[0047] The embodiment of the present invention comprises the following steps:

[0048] (1) Preparation of graphene-modified maleic anhydride-vinyl acetate copolymer

[0049] Add 3 parts by weight of graphene oxide and 700 parts by weight of DMF to a reaction container, disperse them by ultrasonic at 40° C. for 1 hour, add 100 parts by weight of maleic anhydride, stir and react in an oil bath at 80° C. for 2 hours, wash with anhydrous ethanol by centrifugation to remove excess MAH and solvent DMF, and finally freeze-dry the product at -20° C. for 12 hours and grind to obtain graphene-modified maleic anhydride;

[0050] Add 300 parts by weight of toluene, 10 parts by weight of vinyl acetate, 12 parts by weight of graphene-modified maleic anhydride and 0.4 parts by weight of benzoyl peroxide into a reaction container, heat and stir in a water bath at 65° C. to react for 20 hours to obtain a precipitate, filter the precipitate, wash with dichloroethane, and vacuum dry at 60° C. for 12 hours to obtain a copolymer.

[0051] (2) Preparation of investment casting mold material

[0052] (1) 40 to 60 parts by weight of paraffin wax are placed in a reaction kettle, firstly heated indirectly by a water jacket, and the temperature is controlled below 80° C. for partial melting;

[0053] (2) heating to 100-120° C., adding 5-10 parts of montan wax and 10-20 parts of graphene-modified maleic anhydride-vinyl acetate copolymer in sequence, stirring and mixing at 50-100 rpm, and then adding 5-10 parts of tackifying resin and 0-0.01 parts by weight of antioxidant after melting, stirring and mixing evenly;

[0054] (3) The mixed wax liquid is sent to a distributor with a temperature of 100°C, and is selected and formed by a steel belt with a linear speed of 4m / min; the wax droplets are cooled by cold air or cold water, the upper part of the steel belt is cooled by cold air with a temperature of ≤20°C, and the water cooling during the steel belt transmission is a two-stage cooling process, the front stage cooling water is room temperature cooling water, and the rear stage cooling is ≤10°C cooling water, and the casting wax particle mold material is sieved.

[0055] Example 1

[0056] According to the weight proportions, 20 parts of 58# fully refined paraffin wax and 20 parts of 58# semi-refined paraffin wax are placed in a reactor, and firstly heated indirectly by a water jacket, and the temperature is controlled below 70°C for partial melting; heated to 120°C, 6 parts of lignite wax and 10 parts of graphene-modified maleic anhydride-vinyl acetate copolymer are added in sequence, and stirred and mixed at 60 rpm; after melting, 5 parts of C5 / C9 copolymer petroleum resin and 0.001 parts by weight of antioxidant 1010 are added, and the mixture is stirred and mixed evenly; the mixed wax liquid is granulated by a steel belt, and sieved to obtain a casting wax particle mold material.

[0057] Example 2

[0058] According to the weight proportions, 30 parts of 60# fully refined paraffin wax and 20 parts of 60# semi-refined paraffin wax are placed in a reactor, and firstly heated indirectly by a water jacket, and the temperature is controlled below 70°C for partial melting; heated to 120°C, 8 parts of lignite wax and 15 parts of graphene-modified maleic anhydride-vinyl acetate copolymer are added in sequence, and stirred and mixed at 60 rpm; after melting, 8 parts of C9 hydrogenated petroleum resin and 0.003 parts by weight of antioxidant 264 are added, and the mixture is stirred and mixed evenly; the mixed wax liquid is granulated by a steel belt, and sieved to obtain a casting wax particle mold material.

[0059] Example 3

[0060] According to the weight proportions, 30 parts of 62# fully refined paraffin wax and 30 parts of 56# semi-refined paraffin wax are placed in a reactor, and firstly heated indirectly by a water jacket, and the temperature is controlled below 70°C for partial melting; the mixture is heated to 120°C, and 10 parts of lignite wax and 20 parts of graphene-modified maleic anhydride-vinyl acetate copolymer are added in sequence, and the mixture is stirred and mixed at 60 rpm; after the mixture is melted, 10 parts of C5 hydrogenated petroleum resin and 0.003 parts by weight of antioxidant 1076 are added, and the mixture is stirred and mixed evenly; the mixed wax liquid is granulated by a steel belt, and sieved to obtain a casting wax particle mold material.

[0061] Example 4

[0062] According to the weight proportions, 30 parts of 58# semi-refined paraffin wax and 20 parts of 64# fully refined paraffin wax are placed in a reactor, and firstly heated indirectly by a water jacket, and the temperature is controlled below 70°C for partial melting; heated to 120°C, 10 parts of lignite wax and 15 parts of graphene-modified maleic anhydride-vinyl acetate copolymer are added in sequence, and stirred and mixed at 60 rpm; after melting, 8 parts of polymerized rosin and 0.03 parts by weight of antioxidant 168 are added, and the mixture is stirred and mixed evenly; the mixed wax liquid is granulated by a steel belt, and sieved to obtain a casting wax particle mold material.

[0063] Example 5

[0064] According to the weight proportions, 30 parts of 58# semi-refined paraffin wax and 20 parts of 62# fully refined paraffin wax are placed in a reactor, and are firstly heated indirectly by a water jacket, and the temperature is controlled below 70°C for partial melting; the mixture is heated to 120°C, and 10 parts of lignite wax and 12 parts of graphene-modified maleic anhydride-vinyl acetate copolymer are added in sequence, and the mixture is stirred and mixed at 60 rpm; after the mixture is melted, 10 parts of hydrogenated rosin and 0.03 parts by weight of antioxidant 300 are added, and the mixture is stirred and mixed evenly; the mixed wax liquid is granulated by a steel belt, and sieved to obtain a casting wax particle mold material.

[0065] Comparative Example 1

[0066] According to the weight proportions, 30 parts of 58# semi-refined paraffin wax and 20 parts of 64# fully refined paraffin wax are placed in a reactor, and are firstly heated indirectly by a water jacket, and the temperature is controlled below 70°C for partial melting; the mixture is heated to 120°C, and 10 parts of lignite wax, 3 parts of graphene oxide and 12 parts of maleic anhydride-vinyl acetate copolymer are added in sequence, and the mixture is stirred and mixed at 60 rpm; after the mixture is melted, 10 parts of polymerized rosin and 0.03 parts by weight of an antioxidant are added, and the mixture is stirred and mixed evenly; the mixed wax liquid is granulated by a steel belt, and sieved to obtain a casting wax particle mold material.

[0067] Comparative Example 2

[0068] According to the weight proportions, 30 parts of 58# semi-refined paraffin wax and 20 parts of 64# fully refined paraffin wax are placed in a reactor, and are firstly heated indirectly by a water jacket, and the temperature is controlled below 70°C for partial melting; the mixture is heated to 120°C, and 10 parts of lignite wax, 3 parts of graphene oxide and 12 parts of ethylene-vinyl acetate copolymer are added in sequence, and the mixture is stirred and mixed at 60 rpm; after the mixture is melted, 10 parts of polymerized rosin and 0.03 parts by weight of an antioxidant are added, and the mixture is stirred and mixed evenly; the mixed wax liquid is granulated by a steel belt, and sieved to obtain a casting wax particle mold material.

[0069] Comparative Example 3

[0070] According to the weight proportions, 30 parts of 58# semi-refined paraffin wax and 20 parts of 64# fully refined paraffin wax are placed in a reactor, and are firstly heated indirectly by a water jacket, and the temperature is controlled below 70°C for partial melting; the mixture is heated to 120°C, and 10 parts of lignite wax and 15 parts of ethylene-vinyl acetate copolymer are added in sequence, and the mixture is stirred and mixed at 60 rpm; after the mixture is melted, 10 parts of polymerized rosin and 0.03 parts by weight of an antioxidant are added, and the mixture is stirred and mixed evenly; the mixed wax liquid is granulated by a steel belt, and sieved to obtain a casting wax particle mold material.

[0071] Comparative Example 4

[0072] According to the weight proportions, 30 parts of 58# semi-refined paraffin wax and 20 parts of 64# fully refined paraffin wax are placed in a reactor, and firstly heated indirectly by a water jacket, and the temperature is controlled below 70°C for partial melting; heated to 120°C, 10 parts of lignite wax and 10 parts of graphene oxide are added in sequence, and stirred and mixed at 60 rpm; after melting, 10 parts of polymerized rosin and 0.03 parts by weight of an antioxidant are added, and the mixture is stirred and mixed evenly; the mixed wax liquid is granulated by a steel belt, and sieved to obtain a casting wax particle mold material.

[0073] The mold materials prepared in Examples 1 to 5 and Comparative Examples 1-4 were tested for relevant properties. The test method is as follows:

[0074] As shown in Table 1:

[0075] Drop melting point GB / T 8026-2023 "Determination of drop melting point of petroleum waxes and petroleum fats" Softening point GB / T 4507-1999 "Determination of softening point of asphalt (ring and ball method)" Needle penetration GB / T 14235.5-1993 "Standard for determination of surface hardness of investment casting mold materials" Linear shrinkage GB / T 14235.4-1993 "Determination of linear shrinkage of investment casting mold materials" strength GB / T 14235.2-1993 "Determination of flexural strength of investment casting mold materials" Viscosity GB / T 14235.8-1993 "Determination of viscosity of investment casting materials" Ash GB / T 14235.3-1993 "Determination of ash content in investment casting mold materials" Thermal conductivity ASTM C518 Standard Test Method for Determining Steady-State Heat Transfer Characteristics Using a Heat Flow Meter Apparatus

[0076] The test results of the relevant properties of the mold materials obtained in Examples 1 to 5 and Comparative Examples 1-4 are shown in Table 2:

[0077] Table 2

[0078]

[0079] From the test data of Examples 1 to 5 and Comparative Examples 1 to 4 in the above table, it can be seen that the wax pattern material prepared by the present invention has a high drop melting point and a high softening point, indicating that it has good stability. Moreover, the wax pattern material prepared by the scheme of the present invention also has high bending strength, high strength, low linear shrinkage and low ash content, which can ensure that the precision casting wax pattern is not easy to break during production and can meet the dimensional accuracy requirements and surface quality requirements of complex precision castings.

[0080] According to the disclosure of the above description, those skilled in the art to which the present invention belongs may also make appropriate changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments disclosed and described above, and some modifications and changes to the present invention should also fall within the scope of protection of the claims of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.

Claims

1. An investment casting mold material, characterized in that: Calculated by mass, it includes the following raw material components: 40-60 parts of paraffin wax, 5-10 parts of montan wax, 10-20 parts of graphene modified maleic anhydride-vinyl acetate copolymer, 5-10 parts of tackifying resin; The graphene-modified maleic anhydride-vinyl acetate copolymer is prepared by the following steps: (1) Preparation of graphene-modified maleic anhydride Add graphene oxide and an appropriate amount of DMF into a reaction container, perform ultrasonic dispersion at 40° C., add maleic anhydride, stir and react at 80° C., centrifuge, wash, dry and grind to obtain graphene-modified maleic anhydride; (2) Preparation of graphene-modified maleic anhydride-vinyl acetate copolymer Add toluene, vinyl acetate, graphene-modified maleic anhydride and an initiator into a reaction container, heat and stir in a water bath at 63-65° C. for 15-24 hours to obtain a precipitate, filter, wash and dry the precipitate to obtain a copolymer; In the step (1), the mass ratio of graphene oxide to maleic anhydride is (1-3): (80-100); In the step (2), the mass ratio of vinyl acetate: graphene-modified maleic anhydride: initiator is 10: (10-15): (0.2-0.5).

2. The investment casting mold material according to claim 1, characterized in that: The graphene oxide is prepared by adopting the improved Hummers' method, and the graphene content in the graphene-modified maleic anhydride is 8-12%; the initiator is an azo free radical initiator or a peroxide free radical initiator.

3. The investment casting mold material according to claim 1, characterized in that: The paraffin wax is at least one of 58# fully refined paraffin wax, 58# semi-refined paraffin wax, 56# semi-refined paraffin wax, 54# semi-refined paraffin wax, 60# fully refined paraffin wax, 60# semi-refined paraffin wax, 62# fully refined paraffin wax, 62# semi-refined paraffin wax, 64# fully refined paraffin wax and 64# semi-refined paraffin wax.

4. The investment casting mold material according to claim 1, characterized in that: The tackifying resin is at least one of C5 / C9 copolymerized petroleum resin, C9 hydrogenated petroleum resin, C5 hydrogenated petroleum resin, hydrogenated rosin, disproportionated rosin and polymerized rosin; the softening point of the tackifying resin is ≤120°C.

5. The investment casting mold material according to claim 1, characterized in that: The invention also includes 0 to 0.01 parts by weight of an antioxidant, wherein the antioxidant is at least one of antioxidant 1010, antioxidant 264, antioxidant 1076, antioxidant 168, and antioxidant 300.

6. A method for preparing an investment casting pattern material according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) Place 40 to 60 parts of paraffin wax by weight in a reactor, and heat it indirectly with a water jacket at a temperature below 80°C for partial melting; (2) heating to 100-120° C., adding 5-10 parts of montan wax and 10-20 parts of graphene-modified maleic anhydride-vinyl acetate copolymer in sequence, stirring and mixing at 50-100 rpm, and then adding 5-10 parts of tackifying resin and 0-0.01 parts by weight of antioxidant after melting, stirring and mixing evenly; (3) Granulate and screen the steel belt material selection and molding technology to obtain the casting mold material.

7. The method for preparing investment casting mold material according to claim 6, characterized in that: The steel belt material selection, molding and granulation refers to sending the mixed wax liquid to a distributor, the temperature of the distributor is 90-100°C, and selecting and molding through a steel belt, the linear speed of the steel belt is 4-5m / min; cold air or cold water is used to cool the wax drops, the top of the steel belt is cooled by cold air, the temperature is ≤20°C, and the water cooling during the steel belt transmission is two-stage cooling, the front stage cooling water is room temperature cooling water, and the rear stage is cooled by cooling water of ≤10°C to obtain a casting mold material.

8. Use of the investment casting pattern material according to any one of claims 1 to 5 in precision casting.