A self-repairing anti-corrosion coating based on MOF composite filler and its preparation method and use
By covering the organic photothermal layer in the MOF composite filler and loading the corrosion inhibitor, the photothermal effect or corrosion medium is used to promote the MOF transformation and form an LDH protective layer, which solves the problem of insufficient self-repair performance of the existing coating and achieves efficient Self-healing and corrosion resistance improve.
Patent Information
- Application Number
- CN202410459002.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-17
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-04-17
AI Technical Summary
The existing intelligent coatings are self-healed through the oxide film protective layer after damage, but they have defects such as volcanic pores and microcracks, which affect corrosion resistance and cannot effectively improve the service life of the coating and its base metals.
Using a self-healing anticorrosion coating based on MOF composite filler, the LDH protective layer is formed by covering the organic photothermal layer on the MOF nanoparticles and loading the corrosion inhibitor, using the photothermal effect to quickly release the corrosion inhibitor, or under light conditions The corrosion media promotes the collapse of the MOF framework and releases the corrosion inhibitor, forming a new protective layer.
It significantly improves the corrosion resistance and self-repair capabilities of the coating, and can efficiently restore the protective effect of the coating in various service environments, inhibit the further development of corrosion, and extend the service life of the metal.
Smart Images

Figure CN118185441B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of coating anti-corrosion, and in particular to a self-repairing anti-corrosion coating based on MOF composite filler, and a preparation method and use thereof. Background Art
[0002] Metal corrosion is one of the major challenges facing the world today. The physical barrier effect of the coating can effectively isolate the corrosive medium to achieve the effect of metal corrosion protection. It is one of the most widely used metal protection methods today. However, during transportation and service, the coated metal will be affected by environmental factors and mechanical damage, resulting in damage and cracking of the coating matrix and corrosion failure of the metal substrate, which greatly reduces the service life of the coating and its base metal. Therefore, it is urgent to develop smart anti-corrosion coatings with excellent self-healing functions. At present, smart coatings achieve self-repair of the coating by forming an oxide film protective layer on the exposed metal surface after damage, but the oxide film protective layer usually has certain defects, such as volcanic holes and microcracks, which affect the corrosion resistance of the protective layer. Summary of the invention
[0003] The purpose of the present application is to provide a self-repairing anti-corrosion coating based on MOF composite filler and its preparation method and use to solve the above problems.
[0004] To achieve the above objectives, this application adopts the following technical solutions:
[0005] A self-repairing anti-corrosion coating based on MOF composite filler, the raw materials of which include composite filler and resin, wherein the composite filler is composed of MOF nanoparticles loaded with corrosion inhibitor and an organic photothermal layer coated on the surface of the MOF nanoparticles.
[0006] Preferably, the MOF nanoparticles are zinc-magnesium binary MOF, and the corrosion inhibitor is selected from one or more of triazole corrosion inhibitors, quinoline corrosion inhibitors, thiadiazole corrosion inhibitors, imidazole corrosion inhibitors, and aldoxime corrosion inhibitors;
[0007] The loading rate of the corrosion inhibitor in the composite filler is 5-25wt%.
[0008] Preferably, the resin includes one or more of epoxy resin, polyurethane resin, polyurea resin, and polyester resin;
[0009] The resin accounts for 75-95wt% of the total mass of the raw materials.
[0010] Preferably, the raw materials of the organic photothermal layer include polyphenol monomers and iron ion solution or tris(hydroxymethyl)aminomethane and dopamine monomer or aniline and ammonium persulfate.
[0011] Preferably, the thickness of the self-repairing anti-corrosion coating based on MOF composite filler is 40-300 μm.
[0012] The present application also provides a method for preparing the self-repairing anti-corrosion coating based on MOF composite filler, comprising:
[0013] Dissolving a zinc source and a magnesium source in an organic solvent to obtain a first solution, and dissolving an organic ligand 2,5-dihydroxyterephthalic acid in an organic solvent to obtain a second solution; the zinc source comprises zinc acetate and / or zinc nitrate, the magnesium source comprises magnesium acetate and / or magnesium nitrate; and the organic solvent comprises N,N-dimethylformamide and / or N,N-dimethylacetamide;
[0014] Adding the first solution dropwise into the second solution at 40-130° C. with stirring, and reacting with stirring to obtain MOF nanoparticles;
[0015] Adding the MOF nanoparticles and the corrosion inhibitor into an ethanol-water mixed solution, performing a first stirring reaction under negative pressure conditions, and centrifuging to obtain the MOF nanoparticles loaded with the corrosion inhibitor;
[0016] The MOF nanoparticles loaded with the corrosion inhibitor and the raw materials of the organic photothermal layer are mixed, and after a second stirring reaction, centrifugation is performed to obtain the composite filler;
[0017] The composite filler is dispersed in the resin, coated on the surface of the protected object, and cured to obtain the self-repairing anti-corrosion coating based on the MOF composite filler.
[0018] Preferably, the method for preparing the self-repairing anti-corrosion coating based on MOF composite filler satisfies one or more of the following conditions:
[0019] A. The molar ratio of the zinc source, the magnesium source and the organic ligand is (7-14): (7-14): (8-15);
[0020] B. The time of the heat preservation and stirring reaction is 12-48h;
[0021] C. The particle size of the MOF nanoparticles is 50nm-20000nm;
[0022] D. The mass ratio of the MOF nanoparticles to the corrosion inhibitor is 1:(3-10);
[0023] E. The first stirring reaction time is 3-6h;
[0024] F. The mass ratio of the MOF nanoparticles loaded with corrosion inhibitor to the raw materials of the organic photothermal layer is 1:(1-3);
[0025] G. The second stirring reaction time is 1-3h.
[0026] The present application also provides a use of the self-repairing anti-corrosion coating based on MOF composite filler, which is used for self-repairing anti-corrosion of metals.
[0027] Preferably, the metal comprises an aluminum alloy.
[0028] Preferably, the self-repairing and anti-corrosion is carried out in the presence or absence of light.
[0029] Compared with the prior art, the beneficial effects of this application include:
[0030] The self-repairing anti-corrosion coating based on MOF composite filler provided in the present application selects to introduce MOF nanoparticles coated with organic photothermal layer and loaded with corrosion inhibitor into the anti-corrosion coating to construct a self-repairing anti-corrosion coating system. The surface of the organic photothermal layer usually contains groups such as amine, imine and hydroxyl, which can significantly improve the dispersibility of the composite filler in the polymer network; this type of material also has excellent photothermal conversion efficiency, has strong absorption characteristics in the wide-band light zone, and can effectively increase the local temperature of the coating irradiation area. When light is irradiated on the damaged area of the coating, the organic photothermal shell absorbs light energy to efficiently generate heat, increases the release rate of the corrosion inhibitor from the composite filler, forms a hydrothermal microenvironment, thereby shortening the cycle of MOF to LDH conversion, and quickly forms a protective layer on the exposed metal surface; when in the absence of light, the microenvironmental changes in the corrosion process promote the collapse of the MOF skeleton, which can not only release the corrosion inhibitor film, but also the metal ions generated by MOF dissociation can be converted into LDH film on the metal surface, as a new protective layer to inhibit further corrosion of the metal. Through the above steps, the self-repair of the coating can be achieved, which is adaptable to various service environments, can effectively restore the corrosion resistance of the coating and inhibit the further development of corrosion.
[0031] The self-healing anti-corrosion coating based on MOF composite filler exhibits good corrosion resistance and excellent self-healing properties.
[0032] The method for preparing a self-healing anti-corrosion coating based on MOF composite filler provided in the present application has a simple process, and the coating has good corrosion resistance and self-healing properties, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0034] Figure 1 The morphology photos of the zinc-magnesium MOF nanoparticles and the zinc-magnesium MOF composite filler prepared in Example 1;
[0035] Figure 2The morphology photos of the composite filler after 30 minutes and 60 minutes of the aqueous solution of the zinc-magnesium MOF composite filler prepared in Example 1 under the condition of light exposure and without light exposure;
[0036] Figure 3 The corrosion inhibitor release rate curve of the zinc-magnesium MOF composite filler in Example 2 in a 3.5% NaCl solution under the condition of light or not;
[0037] Figure 4 The Bode curves of the damaged area of the composite epoxy coating and the damaged area of the blank epoxy coating prepared in Example 3 after being immersed in a 3.5% NaCl solution for 3 days;
[0038] Figure 5 The damaged area of the composite epoxy coating prepared in Example 3 and the damaged area of the blank epoxy coating are immersed in a 3.5% NaCl solution for 14 days, and the surface microscopic morphology of the exposed metal in the damaged area is shown;
[0039] Figure 6 The Bode curve of the damaged area of the composite epoxy coating prepared in Example 3 after being immersed in a 3.5% NaCl solution for 6 hours with or without light exposure for a certain period of time;
[0040] Figure 7 The damaged area of the composite epoxy coating prepared in Example 3 and each comparative example is a microscopic morphology photograph of the exposed metal surface in the damaged area after the damaged area is immersed in a 3.5% NaCl solution for 2 days. DETAILED DESCRIPTION
[0041] First, an overall introduction to the technical solution is given:
[0042] A self-repairing anti-corrosion coating based on MOF composite filler, the raw materials of which include composite filler and resin, wherein the composite filler is composed of MOF nanoparticles loaded with corrosion inhibitor and an organic photothermal layer coated on the surface of the MOF nanoparticles.
[0043] Layered double hydroxide (LDH) can effectively block Cl - Therefore, by growing LDH on the surface of the oxide layer, the corrosion resistance of the oxide layer can be further improved. However, the synthesis and growth of LDH usually require the artificial introduction of foreign substances to adjust the system and growth environment, and it is difficult to synthesize it autonomously during the service of the coating. After research, it was found that MOF materials as precursors can be converted into LDH in situ by hydrothermal methods. The synthesis process is simple and does not require the introduction of foreign substances. In the field of anti-corrosion coatings, MOF is often used as a container for loading corrosion inhibitors due to its high porosity, large specific surface area and regular pores. However, most current studies only focus on the role of MOF as a loading container, ignoring the potential application of MOF's own skeleton in the self-healing process of the coating.
[0044] Using 1.5 W / cm 2 ~5 W / cm 2 When the damaged area of the coating is irradiated with a near-infrared laser, the corrosion inhibitor in the composite filler is quickly released and the MOF is accelerated to transform into LDH, forming a new protective layer to prevent metal corrosion; in the absence of light, the corrosive medium promotes the collapse of the MOF structure and transforms into an LDH film on the metal surface. At the same time, the corrosion inhibitor molecules are released to inhibit further corrosion of the metal, thereby restoring the protective effect of the coating on the metal substrate.
[0045] In an optional embodiment, the MOF nanoparticles are zinc-magnesium binary MOF, and the corrosion inhibitor is selected from one or more of triazole corrosion inhibitors, quinoline corrosion inhibitors, thiadiazole corrosion inhibitors, imidazole corrosion inhibitors, and aldoxime corrosion inhibitors;
[0046] The loading rate of the corrosion inhibitor in the composite filler is 5-25wt%.
[0047] Optionally, the loading rate of the corrosion inhibitor in the composite filler may be 5wt%, 10wt%, 15wt%, 20wt%, 25wt% or any value between 5-25wt%.
[0048] In an optional embodiment, the resin includes one or more of epoxy resin, polyurethane resin, polyurea resin, and polyester resin;
[0049] The resin accounts for 75-95wt% of the total mass of the raw materials.
[0050] Optionally, the proportion of the resin to the total mass of the raw material may be 75wt%, 80wt%, 85wt%, 90wt%, 95wt% or any value between 75-95wt%.
[0051] In an optional embodiment, the raw materials of the organic photothermal layer include polyphenol monomers and iron ion solution or tris(hydroxymethyl)aminomethane and dopamine monomers or aniline and ammonium persulfate.
[0052] In an optional embodiment, the thickness of the self-repairing anti-corrosion coating based on MOF composite filler is 40-300 μm.
[0053] Optionally, the thickness of the self-repairing anti-corrosion coating based on MOF composite filler can be 40 μm, 50 μm, 100 μm, 150 μm, 200 μm, 250 μm, 300 or any value between 40-300 μm.
[0054] The present application also provides a method for preparing the self-repairing anti-corrosion coating based on MOF composite filler, comprising:
[0055] Dissolving a zinc source and a magnesium source in an organic solvent to obtain a first solution, and dissolving an organic ligand 2,5-dihydroxyterephthalic acid in an organic solvent to obtain a second solution; the zinc source comprises zinc acetate and / or zinc nitrate, the magnesium source comprises magnesium acetate and / or magnesium nitrate; and the organic solvent comprises N,N-dimethylformamide and / or N,N-dimethylacetamide;
[0056] Add the first solution dropwise into the second solution at 40-130°C (which may be 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C or any value between 40-130°C) under stirring, and react by stirring and keeping the temperature to obtain MOF nanoparticles;
[0057] Adding the MOF nanoparticles and the corrosion inhibitor into an ethanol-water mixed solution, performing a first stirring reaction under negative pressure conditions, and centrifuging to obtain the MOF nanoparticles loaded with the corrosion inhibitor;
[0058] The MOF nanoparticles loaded with the corrosion inhibitor and the raw materials of the organic photothermal layer are mixed, and after a second stirring reaction, centrifugation is performed to obtain the composite filler;
[0059] The composite filler is dispersed in the resin, coated on the surface of the protected object, and cured to obtain the self-repairing anti-corrosion coating based on the MOF composite filler.
[0060] In an optional embodiment, the method for preparing the self-repairing anti-corrosion coating based on MOF composite filler satisfies one or more of the following conditions:
[0061] A. The molar ratio of the zinc source, the magnesium source and the organic ligand is (7-14): (7-14): (8-15);
[0062] Optionally, the molar ratio of the zinc source, the magnesium source and the organic ligand can be 7:7:8, 10:10:11, 14:14:15 or any value between (7-14):(7-14):(8-15); the sum of the zinc source and the magnesium source should not be greater than twice the organic ligand.
[0063] B. The time of the heat preservation and stirring reaction is 12-48h;
[0064] Optionally, the time of the heat preservation and stirring reaction can be 12h, 18h, 24h, 30h, 36h, 42h, 48h or any value between 12-48h;
[0065] C. The particle size of the MOF nanoparticles is 50nm-20000nm;
[0066] Optionally, the particle size of the MOF nanoparticles may be 50 nm, 100 nm, 500 nm, 1000 nm, 5000 nm, 10000 nm, 15000 nm, 20000 nm or any value between 50 nm and 20000 nm;
[0067] D. The mass ratio of the MOF nanoparticles to the corrosion inhibitor is 1:(3-10);
[0068] Optionally, the mass ratio of the MOF nanoparticles to the corrosion inhibitor may be 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10 or any value between 1:(3-10);
[0069] E. The first stirring reaction time is 3-6h;
[0070] Optionally, the first stirring reaction time can be 3h, 4h, 5h, 6h or any value between 3-6h;
[0071] F. The mass ratio of the MOF nanoparticles loaded with corrosion inhibitor to the raw materials of the organic photothermal layer is 1:(1-3);
[0072] Optionally, the mass ratio of the MOF nanoparticles loaded with the corrosion inhibitor to the raw material of the organic photothermal layer can be 1:1, 1:2, 1:3 or any value between 1:(1-2);
[0073] G. The second stirring reaction time is 1-3h.
[0074] Optionally, the second stirring reaction time can be 1 h, 2 h, 3 h or any value between 1-3 h.
[0075] The present application also provides a use of the self-repairing anti-corrosion coating based on MOF composite filler, which is used for self-repairing anti-corrosion of metals.
[0076] In an alternative embodiment, the metal comprises an aluminum alloy.
[0077] In an optional embodiment, the self-repairing and anti-corrosion is carried out in the presence or absence of light.
[0078] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0079] Example 1
[0080] This embodiment provides a self-repairing anti-corrosion coating based on MOF composite filler, and the preparation method thereof is as follows:
[0081] 1. Take 0.4 g zinc acetate and 0.2 g magnesium acetate, add them to 50 mL N,N-dimethylformamide organic solvent and make the solution uniform by ultrasound to obtain solution A; take 0.5 g 2,5-dihydroxyterephthalic acid and add it to 50 mL N,N-dimethylformamide solvent, heat it to 70°C in an oil bath, and keep the magnetic stirring at 400 rpm to obtain solution B; during the stirring process, add solution A dropwise to solution B, and then stir the mixed solution at 70°C and 400 rpm for 12 hours; after the reaction is completed, centrifuge at 8000 r / min and wash it with alcohol five times, and dry the precipitate in an oven at 80°C for 12 hours to obtain ZnMg MOF particles;
[0082] 2. Take 0.5 g ZnMg MOF and add it to 50 mL of alcohol solution containing 2 g benzotriazole, use ultrasound to evenly disperse it for 1 hour, pour the dispersed mixed solution into a suction filtration bottle, and stir the mixed solution under negative pressure for 5 hours; then centrifuge at a speed of 8000 r / min and wash it three times with deionized water, and dry the precipitate in a 70°C oven for 12 hours to obtain MOF particles loaded with corrosion inhibitor;
[0083] 3. Take 0.24 g of tris(hydroxymethyl)aminomethane) and 0.5 g of MOF particles loaded with benzotriazole and add them to 200 mL of deionized water, adjust the solution pH to 8.5, then add 0.6 g of dopamine hydrochloride, stir the solution for 2 hours, centrifuge at 6000 r / min and wash three times with alcohol, and dry the precipitate in an oven at 80°C for 12 hours to obtain a MOF-based composite filler;
[0084] 4. Prepare a certain amount of aqueous solution of composite filler and use 808 nm near-infrared laser (1.5 W / cm 2 ) irradiating the solution, and observing the morphology of the composite filler after irradiation for a certain period of time to analyze the effect of light on the conversion of MOF particles into LDH;
[0085] 5. Grind the 6061 aluminum alloy sheet with sandpaper, then ultrasonically clean it with acetone, alcohol, and deionized water in sequence, and then dry it for later use;
[0086] 6. Prepare polyurea resin with isophorone diisocyanate and amino-terminated polydimethylsiloxane with a molecular weight of 3000 in a molar ratio of 1:1 under nitrogen protection at 60°C and stirring overnight;
[0087] 7. Disperse the composite filler into the polyurea resin with a mass fraction of 5.0%;
[0088] 8. Spray the composite resin on the surface of the 6061 aluminum alloy sheet. Use a spray gun to evenly spray the composite resin on the 6061 aluminum alloy sheet at a pressure of 0.5 MPa, with the nozzle 10 cm away from the sample surface;
[0089] 9. The coating was cured at room temperature for 8 hours, then placed at 80°C for further curing for 12 hours, and then cured at 80°C for 12 hours. The coating thickness after curing was 80 μm.
[0090] Figure 1 This is a scanning electron micrograph of the MOF nanoparticles and MOF composite filler obtained in Example 1. After comparison, it can be seen that the rough surface of the composite filler indicates the successful coating of polydopamine, and the loading of the corrosion inhibitor and the coating of polydopamine do not cause the collapse of the MOF particles.
[0091] Figure 2 The morphology of the composite filler in the aqueous solution after 30 minutes and 60 minutes under the condition of no light exposure. The near-infrared laser (1.5 W / cm2) at 808 nm was used. 2 ) After 30 minutes of illumination, flake LDH substances (circled substances in the figure) appeared, indicating that MOF composite particles can be converted into LDH under illumination; after 60 minutes of illumination, a large area of LDH substances appeared. Without illumination, the composite filler did not convert into LDH after immersion for 30 minutes and 60 minutes, further confirming the feasibility of the MOF composite filler to achieve coating self-repair by converting into LDH film under illumination.
[0092] Example 2
[0093] This embodiment provides a self-repairing anti-corrosion coating based on MOF composite filler, and the preparation method thereof is as follows:
[0094] 1. Take 2.97 g of zinc nitrate hexahydrate and 3.59 g of magnesium nitrate hexahydrate, add them to 150 mL of N,N-dimethylacetamide organic solvent and make the solution uniform by ultrasound to obtain solution A; take 3 g of 2,5-dihydroxyterephthalic acid and add it to 150 mL of N,N-dimethylacetamide solvent, heat it to 80°C in an oil bath, and keep the magnetic stirring at 400 rpm to obtain solution B; during the stirring process, add solution A dropwise to solution B, and then stir the mixed solution at 80°C and 400 rpm for 18 hours; after the reaction is completed, centrifuge at a speed of 10000 r / min and wash it with alcohol five times, and dry the precipitate in an oven at 80°C for 12 hours to obtain ZnMg MOF particles;
[0095] 2. Take 1g ZnMg MOF and add it to 100mL alcohol solution containing 4g 8-hydroxyquinoline, use ultrasonic uniform dispersion for 1h, pour the dispersed mixed solution into a suction filtration bottle, and stir the mixed solution under negative pressure for 5 hours; then centrifuge at 8000 r / min and wash three times with deionized water, and dry the precipitate in a 60℃ oven for 12 hours to obtain MOF particles loaded with 8-hydroxyquinoline;
[0096] 3. Take 0.5g of tannic acid and 1g of MOF particles loaded with corrosion inhibitor and add them to 200mL of deionized water, then slowly add 200mL of 1M ferric chloride solution, stir the solution for 3 hours, centrifuge at 6000 r / min and wash three times with deionized water and alcohol respectively, and dry the precipitate in an oven at 60℃ for 12 hours to obtain a MOF-based composite filler;
[0097] 4. Take 0.03g of composite filler and add it to a dialysis bag containing 5 mL of 3.5% NaCl solution. Then immerse the dialysis bag in a beaker containing 500 mL of 3.5% NaCl solution. Take a certain amount of solution from the beaker at regular intervals for UV-visible spectrum test, calculate the corrosion inhibitor content and release rate in the beaker solution, and pour the solution back into the beaker immediately after the test. In order to analyze the effect of light on the release of corrosion inhibitor, use 808 nm near-infrared laser (2.5 W / cm 2 ) irradiating the composite filler for 5 minutes, then stirring for a certain period of time and then taking the solution for UV-visible spectrum testing;
[0098] 5. Grind the 5052 aluminum alloy sheet with sandpaper, then ultrasonically clean it with acetone, alcohol, and deionized water in sequence, and then dry it for later use;
[0099] 6. In a nitrogen atmosphere, polybutylene glycol with a molecular weight of 1400 and diphenylmethane diisocyanate in a molar ratio of 1:4 were added to N,N-dimethylacetamide at a temperature of 80°C and stirred for 3 hours, and then an appropriate amount of 1,4-butanediol was added to the solvent. After being fully stirred for 3 hours, the solution was poured into a mold and dried at 80°C for 24 hours to obtain polyurethane;
[0100] 7. Mix the composite filler and polyurethane in tetrahydrofuran evenly, and use a scraper to evenly apply the composite resin on the surface of the 5052 aluminum alloy sheet, where the composite filler accounts for 10.0% of the coating mass;
[0101] 8. The coating was cured at room temperature for 12 hours and then placed at 60°C for further curing for 24 hours. The coating thickness after curing was 140 μm.
[0102] Figure 3The results are shown in the presence or absence of 808 nm near-infrared laser (1.5 W / cm 2 ) The corrosion inhibitor release curve of the composite filler in 3.5% NaCl solution under the condition of light, where each light exposure time is 5 minutes. It can be seen intuitively from the figure that light can greatly promote the release of corrosion inhibitor from the composite filler, and the release efficiency is much higher than that without light.
[0103] Example 3
[0104] This embodiment provides a self-repairing anti-corrosion coating based on MOF composite filler, and the preparation method thereof is as follows:
[0105] 1. Take 3.10 g of zinc acetate and 2.17 g of magnesium acetate, add them to 150 mL of N,N-dimethylacetamide organic solvent and make the solution uniform by ultrasound to obtain solution A; take 2.80 g of 2,5-dihydroxyterephthalic acid and add it to 150 mL of N,N-dimethylacetamide solvent, heat it to 60°C in an oil bath, and keep the magnetic stirring at 400 rpm to obtain solution B; during the stirring process, add solution A dropwise to solution B, and then stir the mixed solution at 50°C and 400 rpm for 24 hours; after the reaction is completed, centrifuge at 8000 r / min and wash it with alcohol five times, and dry the precipitate in an oven at 80°C for 12 hours to obtain ZnMg MOF particles;
[0106] 2. Take 1 g of ZnMg MOF and add it to 100 mL of alcohol solution containing 5 g of salicylaldehyde oxime, use ultrasound to evenly disperse it, pour the dispersed mixed solution into a suction filtration bottle, and stir the mixed solution under negative pressure for 4 hours; then centrifuge at a speed of 8000r / min and wash it three times with deionized water, and freeze-dry the precipitate for 12 hours to obtain MOF particles loaded with corrosion inhibitor;
[0107] 3. Take 0.48 g of tris(hydroxymethyl)aminomethane) and 1 g of MOF particles loaded with salicylaldehyde oxime and add them to 400 mL of deionized water, adjust the solution pH to 8.5, then add 1.6 g of dopamine hydrochloride, stir the solution for 2 hours, centrifuge at 6000 r / min and wash three times with alcohol, freeze-dry the precipitate for 12 hours to obtain a MOF-based composite filler;
[0108] 4. Grind the 2024 aluminum alloy sheet with sandpaper, then ultrasonically clean it with acetone, alcohol, and deionized water in sequence, and then dry it for later use;
[0109] 5. The epoxy matrix is constructed according to the molar ratio of bisphenol A diglycidyl ether, neopentyl glycol diglycidyl ether and polyetheramine D230 of 1:1:1, and the mass fraction of the composite filler in the coating is 20.0%;
[0110] 6. Spin the composite resin onto the surface of the 2024 aluminum alloy sheet by spin coating at a speed of 200 rpm for 30 seconds;
[0111] 7. After the coating was cured at room temperature for 12 hours, it was placed at 60°C for further curing for 24 hours and at 60°C for 12 hours and 24 hours respectively. The coating thickness after curing was 120 μm.
[0112] 8. Use a scalpel to make a cut of about 70 μm in width on the coating surface, and test the electrochemical impedance spectroscopy of the damaged area of the composite epoxy coating and the blank epoxy coating after immersion in a 3.5wt.% NaCl solution for 3 days. The test solution is 3.5wt.% NaCl;
[0113] 9. Use a scalpel to make a cut of about 70 μm on the coating surface, and then use 2.5 W / cm 2 The scratch was irradiated with an 808 nm near-infrared laser for 15 min. The composite epoxy coating that was scratched but not irradiated was used as a control. The electrochemical impedance spectroscopy of the damaged area of the composite coating was tested after being immersed in 3.5wt.% NaCl solution for 6 hours with and without illumination for a certain period of time.
[0114] Figure 4 is the Bode curve of the damaged area of the composite epoxy coating and the blank epoxy coating in Example 3 after being immersed in a 3.5wt.% NaCl solution for 3 days, where the low-frequency impedance modulus |Z| 0.01 It can semi-quantitatively represent the barrier performance of the coating. After comparison, the low-frequency impedance modulus of the composite epoxy coating is significantly higher than that of the blank epoxy coating, and the composite epoxy coating exhibits a better self-healing effect.
[0115] Figure 5 The surface morphology of the metal in the damaged area of the composite epoxy coating and the blank epoxy coating after exposure to 3.5wt.% NaCl solution for 14 days in Example 3. It can be seen that the exposed metal surface of the blank epoxy coating is covered with corrosion products, and the exposed metal surface of the composite epoxy coating is not only covered with LDH, but also has significantly reduced corrosion products, indicating that the introduction of MOF composite fillers can not only slow down the corrosion of the metal, but also form a new protective layer.
[0116] Figure 6The Bode curve of the damaged area of the composite epoxy coating in Example 3 after being immersed in a 3.5wt.% NaCl solution for 6 hours with or without illumination for a certain period of time. It can be seen that the low-frequency impedance modulus of the damaged area after illumination is higher than that without illumination, indicating that illumination can promote the self-repair process of the composite coating. Therefore, the self-repairing coating based on MOF composite fillers prepared in this application can effectively improve the corrosion protection of the coating against metals.
[0117] Example 4
[0118] The difference from Example 3 is that steps 8 and 9 are not performed.
[0119] A scalpel was used to make a scratch with a width of about 70 μm on the coating surface. The damaged area was immersed in a 3.5wt.% NaCl solution for 2 days, and the surface morphology of the exposed metal in the damaged area was observed.
[0120] Figure 7 It can be seen that when the protected metal is 2024 aluminum alloy and the MOF material is zinc-magnesium binary MOF, a uniform and dense LDH layer is formed on the surface of the exposed aluminum alloy in the damaged area of the coating, which plays a self-repairing role and better restores the protection of the coating to the metal.
[0121] Comparative Example 1
[0122] The difference from Example 4 is that in Comparative Example 1, the metal is pure copper, the pure copper is polished with sandpaper, and then ultrasonically cleaned with acetone, alcohol, and deionized water in sequence, and the composite resin is spin-coated on the surface of the pure copper at a speed of 200 rpm for 30 s.
[0123] Figure 7 It can be seen that when the protected metal is pure copper and the MOF material is zinc-magnesium binary MOF, the surface of the pure copper exposed in the damaged area of the coating cannot form an LDH layer and cannot play a self-repair role.
[0124] Comparative Example 2
[0125] The difference from Example 4 is that in Comparative Example 2, the metal is Q345 carbon steel, the pure copper is polished with sandpaper, and then ultrasonically cleaned with acetone, alcohol, and deionized water in sequence, and the composite resin is spin-coated on the carbon steel surface by spin coating at a speed of 200 rpm for 30 s.
[0126] Figure 7 It can be seen that when the protected metal is Q345 carbon steel and the MOF material is zinc-magnesium binary MOF, the LDH layer cannot be formed on the surface of the exposed carbon steel in the damaged area of the coating, and the self-repairing effect cannot be achieved.
[0127] After replacing the metal, when corrosion occurs, the microenvironment for MOF to transform into LDH cannot be formed. The microenvironment includes the local pH value, the type and concentration of metal ions released from the metal surface, etc. Therefore, the LDH layer cannot be formed on the exposed metal surface, and the self-repair effect cannot be achieved.
[0128] Comparative Example 3
[0129] The difference from Example 4 is that in step 1 of Comparative Example 3, equal concentrations of nickel acetate and cobalt acetate are used to replace zinc acetate and magnesium acetate to prepare a nickel-cobalt binary MOF composite filler and the composite filler is added to the coating.
[0130] Figure 7 It can be seen that when the protected metal is 2024 aluminum alloy and the MOF material is nickel-cobalt binary MOF, the surface of the aluminum alloy exposed in the damaged area of the coating cannot form an LDH layer and cannot play a self-repair role.
[0131] Comparative Example 4
[0132] The difference from Example 4 is that in step 1 of Comparative Example 4, nickel acetate and cobalt acetate of equal concentrations are used to replace zinc acetate and magnesium acetate to prepare a nickel-cobalt binary MOF composite filler and add the composite filler to the coating. In addition, the metal is pure copper, which is polished with sandpaper, then ultrasonically cleaned with acetone, alcohol, and deionized water in sequence, and the composite resin is spin-coated on the pure copper surface by spin coating at a speed of 200 rpm for 30 s.
[0133] Figure 7 It can be seen that when the protected metal is pure copper and the MOF material is nickel-cobalt binary MOF, the LDH layer cannot be formed on the surface of the exposed pure copper in the damaged area of the coating, and the self-repair effect cannot be achieved.
[0134] Comparative Example 5
[0135] The difference from Example 4 is that in step 1 of Comparative Example 4, nickel acetate and cobalt acetate of equal concentrations are used to replace zinc acetate and magnesium acetate to prepare a nickel-cobalt binary MOF composite filler and add the composite filler to the coating. In addition, the metal is Q345 carbon steel, the carbon steel is polished with sandpaper, and then ultrasonically cleaned with acetone, alcohol, and deionized water in sequence, and the composite resin is spin-coated on the surface of the carbon steel by spin coating at a speed of 200 rpm for 30 s.
[0136] Figure 7 It can be seen that when the protected metal is Q345 carbon steel and the MOF material is nickel-cobalt binary MOF, the LDH layer cannot be formed on the surface of the exposed carbon steel in the damaged area of the coating, and the self-repair effect cannot be achieved.
[0137] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0138] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A method for preparing a self-repairing anti-corrosion coating based on MOF composite filler, characterized in that: The raw materials of the self-repairing anti-corrosion coating based on MOF composite filler include composite filler and resin, and the composite filler is composed of MOF nanoparticles loaded with corrosion inhibitor and an organic photothermal layer coated on the surface thereof; The preparation method comprises: Dissolving a zinc source and a magnesium source in an organic solvent to obtain a first solution, and dissolving an organic ligand 2,5-dihydroxyterephthalic acid in an organic solvent to obtain a second solution; the zinc source comprises zinc acetate and / or zinc nitrate, the magnesium source comprises magnesium acetate and / or magnesium nitrate; and the organic solvent comprises N,N-dimethylformamide and / or N,N-dimethylacetamide; Adding the first solution dropwise into the second solution at 40-130° C. with stirring, and reacting with stirring to obtain MOF nanoparticles; Adding the MOF nanoparticles and the corrosion inhibitor into an ethanol-water mixed solution, performing a first stirring reaction under negative pressure conditions, and centrifuging to obtain the MOF nanoparticles loaded with the corrosion inhibitor; The MOF nanoparticles loaded with the corrosion inhibitor and the raw materials of the organic photothermal layer are mixed, and after a second stirring reaction, centrifugation is performed to obtain the composite filler; The composite filler is dispersed in the resin, coated on the surface of the protected object, and cured to obtain the self-repairing anti-corrosion coating based on the MOF composite filler.
2. The method for preparing a self-repairing anti-corrosion coating based on MOF composite filler according to claim 1, characterized in that: The MOF nanoparticles are zinc-magnesium binary MOF, and the corrosion inhibitor is selected from one or more of triazole corrosion inhibitors, quinoline corrosion inhibitors, thiadiazole corrosion inhibitors, imidazole corrosion inhibitors, and aldoxime corrosion inhibitors; The loading rate of the corrosion inhibitor in the composite filler is 5-25wt%.
3. The method for preparing a self-repairing anti-corrosion coating based on MOF composite filler according to claim 1, characterized in that: The resin includes one or more of epoxy resin, polyurethane resin, polyurea resin, and polyester resin; The resin accounts for 75-95wt% of the total mass of the raw materials.
4. The method for preparing a self-repairing anti-corrosion coating based on MOF composite filler according to claim 1, characterized in that: The raw materials of the organic photothermal layer include polyphenol monomers and iron ion solution or tris(hydroxymethyl)aminomethane and dopamine monomer or aniline and ammonium persulfate.
5. The method for preparing a self-repairing anti-corrosion coating based on MOF composite filler according to any one of claims 1 to 4, characterized in that: The thickness of the self-repairing anti-corrosion coating based on MOF composite filler is 40-300 μm.
6. The method for preparing a self-repairing anti-corrosion coating based on MOF composite filler according to claim 1, characterized in that: One or more of the following conditions are met: A. The molar ratio of the zinc source, the magnesium source and the organic ligand is (7-14): (7-14): (8-15); B. The time of the heat preservation and stirring reaction is 12-48h; C. The particle size of the MOF nanoparticles is 50nm-20000nm; D. The mass ratio of the MOF nanoparticles to the corrosion inhibitor is 1:(3-10); E. The first stirring reaction time is 3-6h; F. The mass ratio of the MOF nanoparticles loaded with corrosion inhibitor to the raw materials of the organic photothermal layer is 1:(1-3); G. The second stirring reaction time is 1-3h.
Citation Information
Cited By
Preparation method of self-repairing and self-early-warning polymer coating of MOF-based magnesium alloy
CN119529672A
ZIF-67 silane coupling agent modified hydroxyapatite nanowire self-repairing epoxy resin anticorrosive coating and preparation method thereof
CN122465462A