A high water-blocking polyurethane adhesive and its preparation method and application
By using nano-silica and modified regenerated cellulose in polyurethane adhesives, the water resistance and adhesion are improved, and the water resistance and adhesion of polyurethane adhesives in the outdoor environment in the prior art is solved. The problem of insufficient is that stable bonding is achieved on the back panel of the solar cell.
Patent Information
- Application Number
- CN202410375269.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-29
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-03-29
AI Technical Summary
Existing polyurethane adhesives are susceptible to moisture penetration and light in outdoor environments, resulting in insufficient water barrier properties and adhesive strength, and cannot be effectively applied to outdoor environments.
Using a combination of component A and component B, component A includes polyols, plasticizers, silane coupling agents, water blockers and water absorbers, where the water blockers are nanosilicon dioxide and modified regenerated cellulose, Improve the polyurethane structure through silane coupling agent, nanosilica-filled colloids, and modify regenerated cellulose to reduce hydrophilicity and improve bonding properties.
It achieves high water resistance and strong adhesiveness, enhances the mechanical properties and thermal stability of polyurethane adhesives, and is suitable for outdoor environments, especially in bonding applications of solar cell back panels.
Smart Images

Figure BDA0004766862930000101
Abstract
Description
Technical Field
[0001] The invention relates to the field of polyurethane adhesive preparation, and in particular to a high water-resistant polyurethane adhesive and a preparation method and application thereof. Background Art
[0002] Polyurethane adhesives are adhesives that contain carbamate groups (-NHCOO-) or isocyanate groups (-NCO) in their molecular chains. They have good activity, low pollution or no pollution, non-flammability, and excellent impact resistance. They can be used as adhesives in the fields of chemical materials. However, in actual applications, polyurethane adhesives are inevitably used in outdoor environments, especially in rainy weather. Rainwater will penetrate the polyurethane adhesives and enter the interior of the bonded objects, affecting the performance of the objects. In addition, solar radiation and light will also cause polyurethane adhesives to undergo photodegradation reactions to varying degrees, affecting the viscosity and mechanical properties of the adhesives. Therefore, it is necessary to modify traditional polyurethane adhesives to improve the water resistance and bonding ability of polyurethane.
[0003] In recent years, polyurethane adhesives have become a research hotspot in the adhesive field due to their excellent chemical stability, viscoelasticity and excellent impact resistance.
[0004] For example: A Chinese patent document with publication number CN116554823A and publication date August 8, 2023, entitled "A water-resistant polyurethane adhesive and its preparation method" discloses a method for preparing a water-resistant polyurethane adhesive. In the technical solution disclosed in the patent document, the introduction of fluorine element can improve the hydrolysis resistance of the polyurethane molecular chain, the introduction of the intermediate structure can give the polyurethane excellent flame retardant properties, and the introduction of the benzene ring structure of triphenylmethane triisocyanate can give carbon-forming properties, cooperate with the intermediate, and improve the flame retardant effect.
[0005] However, it should be pointed out that although the technical solution disclosed in the patent document can achieve water resistance, fluorine is a hydrophilic element and cannot achieve a waterproof effect. In addition, there are problems such as poor mechanical properties and weak adhesion, and it cannot be used in outdoor environments.
[0006] For another example: The Chinese patent document with publication number CN202210084152 and publication date April 29, 2022, entitled “A Highly Water-Resistant Polyurethane Waterproof Coating and Preparation Method Thereof” describes that the main components of the highly water-resistant polyurethane waterproof coating are solid asphalt, silane-terminated polybutadiene, terminal hydroxyl polybutadiene, polyol chain extender, liquid filler, catalyst, zinc stearate, super calcium powder, and lycopodium powder. It is verified that the polyurethane waterproof coating has good water resistance, but poor adhesion. There is a high risk of coating falling off during use, and it is not suitable for the adhesive direction.
[0007] Based on the above, it can be seen that the prior art lacks an effective method that can greatly improve water barrier properties and bonding strength. Therefore, it is necessary to modify the traditional polyurethane adhesive to improve the water barrier properties and bonding ability of the polyurethane. Summary of the invention
[0008] The present invention aims to overcome the defects of the polyurethane adhesive in the prior art, namely, weak water-blocking performance and weak bonding force, and thus provides a high water-blocking polyurethane adhesive and a preparation method and application thereof to overcome the above-mentioned shortcomings.
[0009] In order to achieve the above-mentioned invention object, the present invention is implemented by the following technical solutions:
[0010] In a first aspect, the present invention first provides a high water-blocking polyurethane adhesive, which comprises a component A and a component B;
[0011] The component A comprises, by mass percentage, 30% to 50% of a polyol, 20% to 40% of a plasticizer, 1% to 5% of a silane coupling agent, 5% to 15% of a water-blocking agent, and 5% to 10% of a water absorbent;
[0012] Wherein, the water-blocking agent comprises nano-silicon dioxide and modified regenerated cellulose;
[0013] The regenerated cellulose comprises a cellulose main chain, the cellulose main chain comprises hydroxyl groups and silane segments chemically grafted to the cellulose main chain, and the cellulose main chain also comprises copper ions coordinated thereto;
[0014] The B component contains a polyurethane prepolymer and a catalyst, and the catalyst accounts for 0.5% to 1% of the total mass of the B component.
[0015] The high water-blocking polyurethane adhesive in the present application is composed of component A and component B. During use, it is only necessary to fully mix component A and component B without considering environmental conditions. After curing, a good water-blocking effect can be achieved.
[0016] In component A, silane coupling agent and water-blocking agent have good water-blocking effect. Among them, silane coupling agent can improve the surface hydrophilicity of polyurethane structural adhesive, so that it has good hydrophobicity, and the addition of silane coupling agent can greatly improve the bonding stability between polyurethane and substrate, thereby improving the bonding strength from the side.
[0017] In addition, the water-blocking agent described in the present invention includes nano-silicon dioxide and modified regenerated cellulose. Nano-silicon dioxide can fill the micropores and gaps in the adhesive due to its extremely small particle size, effectively improving the density of the colloid, thereby reducing the possibility of water passing through. At the same time, nano-silicon dioxide has a large specific surface area and surface activity, and can fully contact and combine with other adhesive components to enhance the overall consistency and water resistance of the adhesive.
[0018] In addition, the molecular structure of cellulose contains a large number of hydroxyl groups, and the presence of these hydroxyl groups makes traditional cellulose generally have good hydrophilicity. In this application, the cellulose structure is modified in a targeted manner, and a certain amount of silane segments are chemically grafted on the cellulose main chain, thereby changing the hydrophilicity of cellulose, thereby reducing the penetration rate of water in the adhesive. A portion of the hydroxyl groups retained on the cellulose main chain can participate in the synthesis of polyurethane, so that the cross-linking density of the polyurethane adhesive after curing can be greatly improved, thereby increasing the bonding performance of the adhesive. Thus, while the adhesive is more firm and reliable, the polyurethane adhesive has good mechanical properties, strong tensile strength and high hardness. In addition, the addition of silane segments in the modified regenerated cellulose can enhance the thermal stability of the adhesive, so that it can still maintain good bonding performance in a high temperature environment, which is crucial for the high temperature environment that solar cells need to face.
[0019] In addition, the inventors of the present application also found that when a certain amount of copper ions are coordinated on the main chain of cellulose, its water barrier properties can be improved to a certain extent. One explanation is that copper ions may form bonds with the hydroxyl groups or other active groups of cellulose, causing the copper ions and cellulose to combine into a complex structure. This complex structure may form a protective film on the surface, reducing the surface hydrophilicity of cellulose and reducing the penetration of water molecules, thereby improving the water barrier properties of modified regenerated cellulose. When the copper ions are thoroughly washed, the cellulose no longer contains copper ions or their complexes, and the modified structure and properties of the cellulose surface may change, resulting in a decrease in water barrier properties. This suggests that the special interaction between copper ions and modified regenerated cellulose has an important influence on the water barrier properties of modified regenerated cellulose.
[0020] In addition to the water-blocking agent, the present application also makes full use of the water absorption of the molecular sieve, which can absorb the water vapor entering the cured polyurethane and prevent it from further entering the deep layer of the polyurethane, thereby further improving the water-blocking performance of the polyurethane adhesive.
[0021] Finally, the resin used in this application has excellent adhesion and can be firmly bonded to the solar cell back panel. After curing, the adhesion is even stronger and can even be applied to more places and fields.
[0022] Preferably, the added amount of the modified regenerated cellulose is not higher than 5% of the total mass of component A, and not higher than 50% of the total mass of nano-silicon dioxide.
[0023] In the present application, the inventors found that the amount of modified regenerated cellulose added has a significant impact on the overall performance of polyurethane. When the amount of modified regenerated cellulose added to component A is too high, it is difficult to disperse evenly in component A, resulting in agglomeration of part of the modified regenerated cellulose. Since the hydroxyl groups in the molecules of this part of the agglomerated regenerated cellulose are not completely consumed, the polyurethane still contains a large number of hydrophilic hydroxyl groups after curing, which allows water vapor to easily enter the interior of the polyurethane, thereby reducing its water barrier performance.
[0024] In addition, adding too much modified regenerated cellulose will cause the viscosity of component A to increase significantly, resulting in mixing difficulties and uneven mixing during the subsequent mixing process with component B, thereby reducing the overall performance of the polyurethane after final curing.
[0025] Preferably, the method for preparing modified regenerated cellulose comprises the following steps:
[0026] (S.1) dissolving a cellulose raw material in a copper ammonia solution to obtain a cellulose solution;
[0027] (S.2) adding a silane coupling agent to the cellulose solution, stirring and reacting, and obtaining a modified regenerated cellulose solution;
[0028] (S.3) Under stirring conditions, the modified regenerated cellulose solution is added dropwise into a coagulation bath to solidify and precipitate the modified regenerated cellulose, and the precipitated modified regenerated cellulose is dried to obtain the modified regenerated cellulose.
[0029] In the process of preparing modified regenerated cellulose, the present application firstly complexes the cellulose raw material with copper ammonium ions, thereby destroying the interconnected hydrogen bonds in the cellulose, so that the cellulose can be dissolved in the copper ammonium solution, thereby completely exposing the hydroxyl groups originally connected together by hydrogen bonds, thereby ensuring that the silane coupling agent fully contacts and reacts with the cellulose, and ensuring the uniformity of the grafting of the silane coupling agent on the cellulose main chain, thereby improving the modification effect and the quality of the finished product.
[0030] Preferably, the cellulose raw material is any one or more combinations of reed fiber, bamboo cellulose, broadleaf pulp, coniferous pulp, bleached chemical mechanical wood pulp, bleached chemical straw pulp, bleached chemical bagasse pulp, cotton pulp, and white waste paper deinked pulp.
[0031] Preferably, the degree of polymerization of the cellulose raw material is 500-1000.
[0032] The inventors of the present application have found that the degree of polymerization of the cellulose raw material has an important influence on the water-blocking effect of the water-blocking agent. The degree of polymerization of cellulose within this range indicates that the cellulose molecular chain is relatively long and contains more glucose units. This longer molecular chain structure is conducive to the interaction between cellulose and other substances, such as reacting with copper ions or silane coupling agents, thereby realizing the modification process of cellulose. The degree of polymerization of the cellulose raw material is 500-1000, indicating that its molecular chain length is moderate, which can provide a suitable molecular structure and reactivity in the modification process, which is conducive to the interaction between cellulose and other components and the realization of the modification effect.
[0033] Preferably, the polyol is a mixture of one or more of polyester polyols, polyols, aromatic polyols, polyolefin polyols, polyacrylate polyols, castor oil, modified castor oil, palm oil, and soybean oil with a molecular weight of 1000-2000 and a functionality of 2-3.
[0034] Preferably, the water absorbent includes one or more composites of aluminosilicate molecular sieves, titanium silicon molecular sieves, ZSM-35 molecular sieves, ZSM-5 molecular sieves, and CR-500 molecular sieves.
[0035] Preferably, the plasticizer comprises a mixture of one or more of paraffin, asphalt, plasticizer DOP and plasticizer DIDP;
[0036] The catalyst includes one or more of an amine catalyst, an organic zinc catalyst, an organic bismuth catalyst, and a titanate catalyst;
[0037] The silane coupling agent is one of KH-560, KH-550, KH-570, KH-590, KH-902, KH-792, A-151, A-187, A-174, A-1891, A-1100, and A-1120, or a mixture of more thereof.
[0038] In a second aspect, the present invention also provides a method for preparing the high water-blocking polyurethane adhesive, the method comprising the following steps:
[0039] (1) According to mass percentage, 30% to 50% of polyol, 20% to 40% of plasticizer, 1% to 5% of silane coupling agent, 5% to 15% of water blocking agent and 5% to 10% of water absorbent are mixed and defoamed to obtain component A;
[0040] (2) Dehydrating 60% to 70% of isocyanate and reacting it with 30% to 40% of polyol for 2 to 3 hours, then adding 0.5% to 1% of the total mass of component B in a catalyst and continuing the reaction for 30 to 60 minutes, and obtaining component B after degassing and cooling;
[0041] (3) Component A and component B are mixed by vacuum degassing in a ratio of 100:10-30 to obtain the high water-blocking polyurethane adhesive.
[0042] In a third aspect, the present invention also provides the use of the high water-resistant polyurethane adhesive in bonding solar cell back panels.
[0043] Therefore, compared with the prior art, the present invention has the following beneficial effects:
[0044] (1) A polyurethane adhesive with high water-blocking effect was prepared by combining a silane coupling agent with a water-absorbing agent, modifying regenerated cellulose and gas-phase nano-silica to fill the intramolecular voids. During use, the operation is simple, non-toxic and pollution-free;
[0045] (2) The polyurethane adhesive has good bonding ability and can be firmly bonded to the solar cell back panel. After curing, the bonding force is even stronger and can even be applied to more places and fields;
[0046] (3) In addition, the polyurethane adhesive has good mechanical properties, with both strong tensile strength and high hardness. DETAILED DESCRIPTION
[0047] The present invention is further described below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.
[0048]
Preparation of modified regenerated cellulose
[0049] Modified regenerated cellulose A: bamboo fiber with a degree of polymerization of 700 is selected and dissolved in a copper ammonia solution (wherein the copper content in the copper ammonia solution is 2.5wt%, the ammonia content is 8.5wt%, and the glucose content is 0.7wt%) to prepare a cellulose solution with a bamboo cellulose solid content of 8wt%, and then 20wt% of the bamboo fiber mass of silane coupling agent KH-560 is added to the cellulose solution, and the reaction is stirred at 50°C for 3h to obtain a modified regenerated cellulose solution. Under high-speed stirring conditions of 5000rpm, the modified regenerated cellulose solution is dropped into a 90% ethanol solution to solidify and precipitate the modified regenerated cellulose, which is filtered and dried at 80°C to obtain the modified regenerated cellulose A.
[0050] Modified regenerated cellulose B: Cotton pulp with a degree of polymerization of 500 is selected and dissolved in a copper ammonia solution (wherein the copper content in the copper ammonia solution is 3wt%, the ammonia content is 7.5wt%, and the glucose content is 0.4wt%) to prepare a cellulose solution with a cotton pulp solid content of 6.8wt%, and then 20wt% of the cotton pulp mass of silane coupling agent KH-550 is added to the cellulose solution, and the reaction is stirred at 50°C for 3h to obtain a modified regenerated cellulose solution. Under high-speed stirring conditions of 5000rpm, the modified regenerated cellulose solution is dropped into a 90% ethanol solution to solidify and precipitate the modified regenerated cellulose, which is filtered and dried at 80°C to obtain the modified regenerated cellulose B.
[0051] Modified regenerated cellulose C: bamboo fiber with a degree of polymerization of 1000 is selected and dissolved in a copper ammonia solution (wherein the copper content in the copper ammonia solution is 4.3wt%, the ammonia content is 7.9wt%, and the glucose content is 0.55wt%) to prepare a cellulose solution with a bamboo cellulose solid content of 7.8wt%, and then 25wt% of the bamboo fiber mass of silane coupling agent KH-550 is added to the cellulose solution, and the reaction is stirred at 50°C for 3h to obtain a modified regenerated cellulose solution. Under high-speed stirring conditions of 5000rpm, the modified regenerated cellulose solution is dropped into a 90% ethanol solution to solidify and precipitate the modified regenerated cellulose, which is filtered and dried at 80°C to obtain the modified regenerated cellulose C.
[0052] Modified regenerated cellulose D: bamboo fiber with a degree of polymerization of 300 is selected and dissolved in a copper ammonia solution (wherein the copper content in the copper ammonia solution is 2.2wt%, the ammonia content is 7.5wt%, and the glucose content is 0.25wt%) to prepare a cellulose solution with a bamboo cellulose solid content of 6.4wt%, and then 20wt% of the bamboo fiber mass of silane coupling agent KH-550 is added to the cellulose solution, and the reaction is stirred at 50°C for 3h to obtain a modified regenerated cellulose solution. Under high-speed stirring conditions of 5000rpm, the modified regenerated cellulose solution is dropped into a 90% ethanol solution to solidify and precipitate the modified regenerated cellulose, which is filtered and dried at 80°C to obtain the modified regenerated cellulose D.
[0053] Modified regenerated cellulose E: bamboo fiber with a degree of polymerization of 1500 was selected and dissolved in a copper ammonia solution (wherein the copper content in the copper ammonia solution was 2.8wt%, the ammonia content was 8.5wt%, and the glucose content was 0.3wt%) to prepare a cellulose solution with a bamboo cellulose solid content of 6.9wt%, and then 20wt% of the bamboo fiber mass of silane coupling agent KH-550 was added to the cellulose solution, and the reaction was stirred at 50°C for 3h to obtain a modified regenerated cellulose solution. Under high-speed stirring conditions of 5000rpm, the modified regenerated cellulose solution was dropped into a 90% ethanol solution to solidify and precipitate the modified regenerated cellulose, which was filtered and dried at 80°C to obtain the modified regenerated cellulose E.
[0054] Modified regenerated cellulose F: bamboo fiber with a degree of polymerization of 700 is selected and dissolved in a copper ammonia solution (wherein the copper content in the copper ammonia solution is 2.5wt%, the ammonia content is 8.5wt%, and the glucose content is 0.7wt%) to prepare a cellulose solution with a bamboo cellulose solid content of 8wt%, and then 20wt% of the bamboo fiber mass of silane coupling agent KH-560 is added to the cellulose solution, and the reaction is stirred at 50°C for 3h to obtain a modified regenerated cellulose solution. Under high-speed stirring conditions of 5000rpm, the modified regenerated cellulose solution is dropped into a 90% ethanol solution to solidify and precipitate the modified regenerated cellulose, which is filtered and transferred to a 5% hydrochloric acid aqueous solution to wash and remove residual copper ammonia complexes, and then washed with clean water and dried at 80°C to obtain the modified regenerated cellulose F.
[0055] Example 1
[0056] Component A is prepared according to the following method: 40 parts of polyol DDL-1000, 36 parts of paraffin, 4 parts of silane coupling agent, 5 parts of modified regenerated cellulose A, 6 parts of nano-silicon dioxide and 9 parts of ZSM-35 molecular sieve are mixed, and component A is obtained by degassing with a vacuum stirring degasser.
[0057] Synthesis of prepolymer component B: dehydrate 60 parts of isocyanate liquefied MDI at 120°C for 2 hours, cool, add 39.5 parts of polyol DDL-1000 and react for 2 hours. Finally, add 0.5 parts of catalyst, react for 30 minutes, vacuum degas for 10 minutes, cool to room temperature, and seal and store in cans.
[0058] Step S3: Mix component A and component B in a ratio of 100:20 by vacuum degassing, apply film, and observe the surface drying time and curing time.
[0059] Example 2
[0060] Component A is prepared according to the following method: 40 parts of polyol DDL-1000, 36 parts of paraffin wax, 4 parts of silane coupling agent, 5 parts of modified regenerated cellulose B, 6 parts of nano-silicon dioxide and 9 parts of ZSM-35 molecular sieve are mixed, and component A is obtained by degassing with a vacuum stirring degassing machine.
[0061] Synthesis of prepolymer component B: dehydrate 60 parts of isocyanate liquefied MDI at 120°C for 2 hours, cool, add 39.5 parts of polyol DDL-1000 and react for 2 hours. Finally, add 0.5 parts of catalyst, react for 30 minutes, vacuum degas for 10 minutes, cool to room temperature, and seal and store in cans.
[0062] Step S3: Mix component A and component B in a ratio of 100:20 by vacuum degassing, apply film, and observe the surface drying time and curing time.
[0063] Example 3
[0064] Component A is prepared according to the following method: 40 parts of polyol DDL-1000, 36 parts of paraffin, 4 parts of silane coupling agent, 5 parts of modified regenerated cellulose C, 6 parts of nano-silicon dioxide and 9 parts of ZSM-35 molecular sieve are mixed, and component A is obtained by degassing with a vacuum stirring degassing machine.
[0065] Synthesis of prepolymer component B: dehydrate 60 parts of isocyanate liquefied MDI at 120°C for 2 hours, cool, add 39.5 parts of polyol DDL-1000 and react for 2 hours. Finally, add 0.5 parts of catalyst, react for 30 minutes, vacuum degas for 10 minutes, cool to room temperature, and seal and store in cans.
[0066] Step S3: Mix component A and component B in a ratio of 100:20 by vacuum degassing, apply film, and observe the surface drying time and curing time.
[0067] Example 4
[0068] Component A is prepared according to the following method: 30 parts of polyol EP280, 40 parts of paraffin, 5 parts of silane coupling agent, 3 parts of modified regenerated cellulose A, 12 parts of nano-silicon dioxide and 10 parts of ZSM-35 molecular sieve are mixed, and component A is obtained by degassing with a vacuum stirring degasser.
[0069] Synthesis of prepolymer component B: dehydrate 70 parts of isocyanate liquefied MDI at 120°C for 3 hours, cool, add 29 parts of polyol EP280 and react for 2 hours. Finally, add 1 part of catalyst, react for 60 minutes, vacuum degas for 10 minutes, cool to room temperature, and seal and store in cans.
[0070] Step S3: Mix component A and component B in a ratio of 100:10 by vacuum degassing, apply film, and observe the surface drying time and curing time.
[0071] Example 5
[0072] Component A is prepared according to the following method: 50 parts of polyol EP280, 20 parts of paraffin, 5 parts of silane coupling agent, 5 parts of modified regenerated cellulose A, 10 parts of nano-silicon dioxide and 10 parts of ZSM-35 molecular sieve are mixed, and component A is obtained by degassing with a vacuum stirring degassing machine.
[0073] Synthesis of prepolymer component B: dehydrate 70 parts of isocyanate liquefied MDI-2020 at 120°C for 3 hours, cool, add 29 parts of polyol EP280 and react for 2 hours. Finally, add 1 part of catalyst, react for 60 minutes, vacuum degas for 10 minutes, cool to room temperature, and seal and store in cans.
[0074] Step S3: Mix component A and component B in a ratio of 100:10 by vacuum degassing, apply film, and observe the surface drying time and curing time.
[0075] Example 6
[0076] Component A is prepared according to the following method: 50 parts of polyol EP280, 39 parts of paraffin, 1 part of silane coupling agent, 2 parts of modified regenerated cellulose A, 3 parts of nano-silicon dioxide and 5 parts of ZSM-35 molecular sieve are mixed, and component A is obtained by degassing with a vacuum stirring degassing machine.
[0077] Synthesis of prepolymer component B: dehydrate 70 parts of isocyanate liquefied MDI-2020 at 120°C for 3 hours, cool, add 29 parts of polyol DDL-1000 and react for 2 hours. Finally, add 1 part of catalyst, react for 60 minutes, vacuum degas for 10 minutes, cool to room temperature, and seal and store in cans.
[0078] Step S3: Mix component A and component B in a ratio of 100:10 by vacuum degassing, apply film, and observe the surface drying time and curing time.
[0079] Comparative Example 1
[0080] Component A is prepared according to the following method: 40 parts of polyol DDL-1000, 36 parts of paraffin, 4 parts of silane coupling agent, 5 parts of modified regenerated cellulose D, 6 parts of nano-silicon dioxide and 9 parts of ZSM-35 molecular sieve are mixed, and component A is obtained by degassing with a vacuum stirring degassing machine.
[0081] Synthesis of prepolymer component B: dehydrate 60 parts of isocyanate liquefied MDI at 120°C for 2 hours, cool, add 39.5 parts of polyol DDL-1000 and react for 2 hours. Finally, add 0.5 parts of catalyst, react for 30 minutes, vacuum degas for 10 minutes, cool to room temperature, and seal and store in cans.
[0082] Step S3: Mix component A and component B in a ratio of 100:20 by vacuum degassing, apply film, and observe the surface drying time and curing time.
[0083] Comparative Example 2
[0084] Component A is prepared according to the following method: 40 parts of polyol DDL-1000, 36 parts of paraffin, 4 parts of silane coupling agent, 5 parts of modified regenerated cellulose E, 6 parts of nano-silicon dioxide and 9 parts of ZSM-35 molecular sieve are mixed, and component A is obtained by degassing with a vacuum stirring degassing machine.
[0085] Synthesis of prepolymer component B: dehydrate 60 parts of isocyanate liquefied MDI at 120°C for 2 hours, cool, add 39.5 parts of polyol DDL-1000 and react for 2 hours. Finally, add 0.5 parts of catalyst, react for 30 minutes, vacuum degas for 10 minutes, cool to room temperature, and seal and store in cans.
[0086] Step S3: Mix component A and component B in a ratio of 100:20 by vacuum degassing, apply film, and observe the surface drying time and curing time.
[0087] Comparative Example 3
[0088] Component A is prepared according to the following method: 40 parts of polyol DDL-1000, 36 parts of paraffin wax, 4 parts of silane coupling agent, 5 parts of modified regenerated cellulose F, 6 parts of nano-silicon dioxide and 9 parts of ZSM-35 molecular sieve are mixed, and component A is obtained by degassing with a vacuum stirring degasser.
[0089] Synthesis of prepolymer component B: dehydrate 60 parts of isocyanate liquefied MDI at 120°C for 2 hours, cool, add 39.5 parts of polyol DDL-1000 and react for 2 hours. Finally, add 0.5 parts of catalyst, react for 30 minutes, vacuum degas for 10 minutes, cool to room temperature, and seal and store in cans.
[0090] Step S3: Mix component A and component B in a ratio of 100:20 by vacuum degassing, apply film, and observe the surface drying time and curing time.
[0091] Comparative Example 4
[0092] Component A is prepared according to the following method: 40 parts of polyol DDL-1000, 36 parts of paraffin, 4 parts of silane coupling agent, 10 parts of modified regenerated cellulose A, 5 parts of nano-silicon dioxide and 9 parts of ZSM-35 molecular sieve are mixed, and component A is obtained by degassing with a vacuum stirring degasser.
[0093] Synthesis of prepolymer component B: dehydrate 60 parts of isocyanate liquefied MDI at 120°C for 2 hours, cool, add 39.5 parts of polyol DDL-1000 and react for 2 hours. Finally, add 0.5 parts of catalyst, react for 30 minutes, vacuum degas for 10 minutes, cool to room temperature, and seal and store in cans.
[0094] Step S3: Mix component A and component B in a ratio of 100:20 by vacuum degassing, apply film, and observe the surface drying time and curing time.
[0095] Comparative Example 5
[0096] Component A is prepared according to the following method: 40 parts of polyol DDL-1000, 36 parts of paraffin wax, 4 parts of silane coupling agent, 5 parts of nano-silicon dioxide and 9 parts of ZSM-35 molecular sieve are mixed, and component A is obtained by degassing with a vacuum stirring degassing machine.
[0097] Synthesis of prepolymer component B: dehydrate 60 parts of isocyanate liquefied MDI at 120°C for 2 hours, cool, add 39.5 parts of polyol DDL-1000 and react for 2 hours. Finally, add 0.5 parts of catalyst, react for 30 minutes, vacuum degas for 10 minutes, cool to room temperature, and seal and store in cans.
[0098] Step S3: Mix component A and component B in a ratio of 100:20 by vacuum degassing, apply film, and observe the surface drying time and curing time.
[0099] The high water-resistant polyurethane adhesives prepared in Examples 1 to 6 and Comparative Examples 1 to 5 were tested, and the test results are shown in Table 1 below.
[0100] Table 1
[0101]
[0102] From the comparison between Examples 1 to 6 and Comparative Examples 1 to 5, it can be seen that the high water-blocking polyurethane adhesive in the present invention has excellent water-blocking performance and good aging resistance.
[0103] By comparing Examples 1 to 3 with Comparative Examples 1 to 2, we found that the molecular weight of the modified regenerated cellulose has a certain influence on the performance of the polyurethane adhesive. When the degree of polymerization of cellulose is low, it will lead to a decrease in the tensile strength of the polyurethane adhesive after curing. When the degree of polymerization of cellulose is high, it will affect the coupling effect of cellulose with other substances during the modification process, thereby causing a certain decrease in its water barrier performance.
[0104] By comparing Example 1 with Comparative Example 3, we found that after removing the copper ions in the modified regenerated cellulose, the mechanical properties of the polyurethane adhesive did not change significantly, but its water barrier properties decreased to a certain extent, indicating that the special interaction between copper ions and modified regenerated cellulose has a certain influence on the water barrier properties of the modified regenerated cellulose.
[0105] By comparing Example 1 with Comparative Example 4, we found that when the modified regenerated cellulose is added in excess, it will cause the modified regenerated cellulose to be difficult to be evenly dispersed in component A, resulting in a phenomenon that a part of the modified regenerated cellulose agglomerates. Since the hydroxyl groups in the molecules of this part of the agglomerated regenerated cellulose are not completely consumed, the polyurethane still contains a large number of hydrophilic hydroxyl groups after curing, which allows water vapor to easily enter the interior of the polyurethane, thereby reducing its water barrier performance.
[0106] By comparing Example 1 with Comparative Example 5, we found that when the modified regenerated cellulose was not added, the overall performance of the polyurethane adhesive decreased significantly.
[0107] The specific embodiments described herein are merely examples of the spirit of the present invention. A person skilled in the art of the present invention may make various modifications or additions to the specific embodiments described or replace them in a similar manner, but this will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.
Claims
1. A high water-blocking polyurethane adhesive, characterized in that: It comprises component A and component B; The component A comprises, by mass percentage, 30% to 50% of a polyol, 20% to 40% of a plasticizer, 1% to 5% of a silane coupling agent, 5% to 15% of a water-blocking agent, and 5% to 10% of a water absorbent; Wherein, the water-blocking agent comprises nano-silicon dioxide and modified regenerated cellulose; The modified regenerated cellulose comprises a cellulose main chain, the cellulose main chain comprises hydroxyl groups and silane segments chemically grafted to the cellulose main chain, and the cellulose main chain also comprises copper ions coordinated thereto; The modified regenerated cellulose preparation method comprises the following steps: (S.1) dissolving a cellulose raw material in a cuprammonia solution to obtain a cellulose solution, wherein the degree of polymerization of the cellulose raw material is 500-1000; (S.2) adding a silane coupling agent to the cellulose solution, stirring and reacting, and obtaining a modified regenerated cellulose solution; (S.3) under stirring conditions, dropping the modified regenerated cellulose solution into a coagulation bath to solidify and precipitate the modified regenerated cellulose, and drying the precipitated modified regenerated cellulose to obtain the modified regenerated cellulose; The amount of modified regenerated cellulose added is not higher than 5% of the total mass of component A and is not equal to 0, and is not higher than 50% of the total mass of nano-silicon dioxide; The B component contains a polyurethane prepolymer and a catalyst, and the catalyst accounts for 0.5% to 1% of the total mass of the B component.
2. A high water-blocking polyurethane adhesive according to claim 1, characterized in that: The cellulose raw material is any one or more combinations of reed fiber, bamboo cellulose, broadleaf pulp, coniferous pulp, bleached chemical mechanical wood pulp, bleached chemical straw pulp, bleached chemical bagasse pulp, cotton pulp, and white waste paper deinked pulp.
3. A high water-blocking polyurethane adhesive according to claim 1, characterized in that: The polyol is a mixture of one or more of polyester polyol, aromatic polyol, polyolefin polyol and polyacrylate polyol with a molecular weight of 1000-2000 and a functionality of 2-3.
4. The high water-resistant polyurethane adhesive according to claim 1, characterized in that: The water absorbent includes one or more composites of aluminosilicate molecular sieves, titanium silicon molecular sieves, ZSM-35 molecular sieves, ZSM-5 molecular sieves, and CR-500 molecular sieves.
5. The high water-resistant polyurethane adhesive according to claim 1, characterized in that: The plasticizer includes a mixture of one or more of paraffin, plasticizer DOP and plasticizer DIDP; The catalyst includes one or more of an amine catalyst, an organic zinc catalyst, an organic bismuth catalyst, and a titanate catalyst; The silane coupling agent is one of KH-560, KH-550, KH-570, KH-590, KH-902, KH-792, A-151, A-187, A-174, A-1891, A-1100, and A-1120, or a mixture of more thereof.
6. A method for preparing the high water-blocking polyurethane adhesive according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: (1) According to the mass percentage, 30% to 50% of polyol, 20% to 40% of plasticizer, 1% to 5% of silane coupling agent, 5% to 15% of water blocking agent and 5% to 10% of water absorbent are mixed and defoamed to obtain component A; (2) According to the mass percentage, 60% to 70% of the isocyanate is dehydrated and reacted with 30% to 40% of the polyol for 2 to 3 hours, and then 0.5% to 1% of the total mass of the B component is added with a catalyst to continue the reaction for 30 to 60 minutes, and after degassing and cooling, the B component is obtained; (3) Component A and component B are mixed by vacuum degassing in a ratio of 100:10-30 to obtain the high water-blocking polyurethane adhesive.
7. Use of the high water-resistant polyurethane adhesive as described in any one of claims 1 to 5 in bonding solar cell back panels.
Citation Information
Patent Citations
High-water-resistance polyurethane waterproof coating and preparation method thereof
CN114410214A
Waterproof polyurethane adhesive and preparation method thereof
CN116554823A
Cardiac pacemakers
EP0000280A1
Preparation method of high-temperature-resistant hydrolysis-resistant polyurethane pouring sealant
CN113773782A
A durable sealant with ultra-high elongation, high adhesion, and high toughness, and its preparation method.
CN114933882A