A kind of transparent soil and its preparation method and application

By using pore fluid composed of nano-silicon sol and methylphenyl silicone oil, combined with transparent glass sand and nano-carbon tubes, the problem of existing transparent soil being inapplicable at high temperatures is solved, and the temperature range of 25-90℃ is achieved. High-efficiency physical model experiment.

CN118239750BActive Publication Date: 2024-11-29SHANDONG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410334785.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-22
Publication Date
2024-11-29
Estimated Expiration
2044-03-22

AI Technical Summary

Technical Problem

The existing transparent soil is not suitable under high temperature conditions. Traditional alkane pore fluids reach a flash point at around 70°C, and spontaneous combustion may occur, which cannot meet the physical model test needs of high-temperature formations.

Method used

Using pore fluid composed of nano-silicon sol and methylphenyl silicone oil, combined with transparent glass sand and nano-carbon tubes, the refractive index of pore fluid is controlled to make it suitable for Tests at different temperatures.

Benefits of technology

The prepared transparent soil has high transparency and good bonding properties in the temperature range of 25-90℃. It is suitable for physical model tests at room temperature and high temperatures, and avoids the occurrence of spontaneous combustion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004754707890000081
    Figure BDA0004754707890000081
  • Figure BDA0004754707890000091
    Figure BDA0004754707890000091
Patent Text Reader

Abstract

The invention discloses a transparent soil and a preparation method and application thereof, belonging to the field of geotechnical engineering visualization model test. Nano silica sol and methylphenyl silicone oil are mixed to obtain a mixed solution, heated, and the mass ratio of the nano silica sol and the methylphenyl silicone oil is adjusted so that the refractive index of the heated mixed solution and the refractive index of the transparent glass sand are in a ratio of 1:1 to obtain a pore fluid. The nano carbon tubes and the pore fluid are mixed and kept warm, and the heat-insulated transparent glass sand is added, mixed and vacuumed to obtain the transparent soil. The prepared transparent soil has high transparency and high bonding performance. The nano carbon tubes are added as tracer particles and can be effectively used in physical model tests in geotechnical engineering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of geotechnical engineering visualization model test, and in particular relates to transparent soil and a preparation method and application thereof. Background Art

[0002] In geotechnical engineering, physical model tests are usually used to analyze the damage of rocks or soil, and sensors are buried inside the soil. However, the operation of traditional physical model tests is complicated and easily interfered by external factors, resulting in inaccurate measurement results. CT scanning, X-ray diffraction, nuclear magnetic resonance and other means are usually required to monitor the damage of the soil, which not only makes the test more cumbersome, but also increases the cost of the test. The use of transparent soil to simulate natural soil and the use of PIV technology largely make up for the poor visualization of traditional physical model tests. Good results have been achieved by using transparent soil particles and pore fluids with equivalent refractive index to simulate natural soil for model tests.

[0003] The pore fluid of conventional transparent soil is mostly a mixture of alkanes and white oil, and the refractive index of the pore fluid is controlled by adjusting the ratio between the two to make it close to the refractive index of solid particles. However, the transparent soil currently prepared only considers room temperature tests. For example, patent CN 111650027 B discloses a method for preparing a transparent soil-rock mixture, which includes selecting irregular glass blocks, configuring pore liquid, mixing amorphous silicon powder with pore liquid, adding irregular glass blocks to pore liquid, vacuum treatment, and pressurized consolidation. The transparent soil-rock mixture preparation method of the invention is simple to operate and easy to implement; the artificially synthesized transparent soil-rock mixture has good transparency, good cohesion and transparency, and can be effectively used in model tests in geotechnical engineering. However, n-dodecane and phenylmethyl silicone oil are used in the preparation of pore fluid, among which n-dodecane reaches a flash point at about 70°C and may spontaneously combust under high temperature. For some deep high-temperature strata, the temperature of rocks and soil is relatively high, and the temperature of high-temperature water can reach above 80°C. Therefore, high temperature factors must be considered when conducting model tests. The alkanes used in the transparent soil provided by the prior art are very sensitive to high temperatures and are not suitable for physical model tests under high temperature conditions.

[0004] Therefore, there is an urgent need in the art for a transparent soil that can be used in model tests at both room temperature and high temperature. Summary of the invention

[0005] The purpose of the present invention is to provide a transparent soil and a preparation method and application thereof to solve the problems existing in the above-mentioned prior art.

[0006] One of the technical solutions provided by the present invention:

[0007] A transparent soil comprises the following raw materials: pore fluid, transparent glass sand and nano carbon tubes, wherein the mass ratio of the pore fluid, transparent glass sand and nano carbon tubes is 7:(100-120):1; the pore fluid is composed of nano silica sol and methylphenyl silicone oil.

[0008] Transparent glass sand has higher transparency and purity than fused quartz sand, so transparent glass sand is selected as the granular material component of the transparent soil in the present invention.

[0009] Nano-silica sol is a dispersion of nano-scale silicon dioxide particles in water or other solvents. It has a double-layer structure. Under the action of high temperature, the thickness of the double-layer structure decreases, resulting in cementation, which plays a bonding role. Therefore, nano-silica sol is selected as a binder for transparent soil materials. At different temperatures, the degree of gelation of nano-silica sol is different, and it will show different refractive indices. Methylphenyl silicone oil is a colorless, odorless, transparent liquid with low viscosity and surface tension. It has thermal stability and can remain stable in an environment of -50-250℃. It has excellent performance in transparency and radiation resistance, is shear-resistant, and has high compression, and can be used as a pore fluid component of transparent soil.

[0010] Carbon nanotubes are used as tracer particles to form a speckle field, which is convenient for particle image velocimetry (PIV) experimental analysis.

[0011] The second technical solution provided by the present invention is:

[0012] A method for preparing the above-mentioned transparent soil comprises the following steps: mixing nano-silica sol and methylphenyl silicone oil to obtain a mixed solution, heating so that the ratio of the refractive index of the heated mixed solution to the refractive index of the transparent glass sand is 1:1 to obtain a porous fluid, mixing the nano-carbon tubes and the porous fluid, keeping them warm, adding the heat-insulated transparent glass sand, mixing, and evacuating to prepare the transparent soil.

[0013] Preferably, the mass ratio of the nano-silica sol and the methylphenyl silicone oil mixed is: 1: (1.5-1.8).

[0014] The refractive index of the pore fluid can be controlled to be close to that of transparent glass sand by adjusting the mass ratio of nano-silica sol and methylphenyl silicone oil.

[0015] Preferably, the heating temperature is 25-90°C.

[0016] Preferably, the temperature at which the carbon nanotubes and the pore fluid are kept warm after being mixed is 25-90°C.

[0017] Preferably, the insulation temperature of the transparent glass sand is 25-90°C.

[0018] The reason why the mass ratio between the nano-silica sol and the methylphenyl silicone oil in the present invention is not fixed is that: for different test temperatures, in order to make the refractive index of the mixed liquid close to that of transparent glass sand, the mass ratio of the nano-silica sol and the methylphenyl silicone oil needs to be adjusted. A specific temperature corresponds to a specific mass ratio. From 25-90°C, the mass ratio of the nano-silica sol and the methylphenyl silicone oil needs to be adjusted within 1: (1.5-1.8).

[0019] Preferably, the transparent glass sand is kept warm for 1-2 hours, wherein the transparent glass sand needs to be sized according to test requirements before being kept warm, and needs to be washed and dried to remove impurities and moisture.

[0020] Preferably, the carbon nanotubes and the pore fluid are mixed and kept warm for 6-8 hours.

[0021] Preferably, the vacuuming time is 15-25 minutes. When the vacuum is drawn using a vacuum pump, the refractive index is substantially unaffected, and a higher transparency is more easily achieved.

[0022] Carbon nanotubes produce fluorescence after being irradiated with near-infrared light and can be used as tracer particles to generate a speckle field. The purpose of vacuuming is to remove bubbles, improve the transparency of the transparent soil, and meet the requirement of clearly observing the deformation field.

[0023] The third technical solution provided by the present invention is:

[0024] An application of the above transparent soil in a physical model test in geotechnical engineering is to load and consolidate the transparent soil, lay a layer of transparent soil, and then repeat the laying until the total thickness meets the model test requirements, and use distributed loading to carry out loading and consolidation.

[0025] Beneficial effects of the present invention:

[0026] The preparation method of the transparent soil provided by the present invention is simple. During the preparation process, the influence of temperature factors on the refractive index of nano-silica sol is considered. The mass ratio of nano-silica sol to methylphenyl silicone oil can be adjusted according to different temperature levels to obtain transparent soil with higher transparency. The obtained transparent soil body has high transparency and high bonding performance. Nano-carbon tubes are added as tracer particles, which can be effectively used in physical model tests in geotechnical engineering. In the prior art (CN 111650027 B), due to the use of n-dodecane, it reaches the flash point at about 70°C, and will spontaneously combust at higher temperatures, which cannot meet the high temperature test requirements. However, the transparent soil provided by the present invention can meet the test requirements at higher temperatures (70-90°C). DETAILED DESCRIPTION

[0027] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0028] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0029] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0030] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.

[0031] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0032] The normal temperature of the present invention refers to 25±2°C.

[0033] In the embodiments of the present invention, “parts” refer to “parts by mass” unless otherwise specified.

[0034] The size of the transparent glass sand in the embodiments of the present invention is selected to be 1.0-2.0 mm in diameter according to the requirements of the geotechnical engineering visualization model test.

[0035] The raw materials for preparing the nano-silica sol required in the embodiment of the present invention are: nano-scale silicon powder, water glass and sodium hydroxide, and the above raw materials are all purchased from the market.

[0036] The preparation method is as follows: water glass (modulus 2.7, Baume degree 48) and sodium hydroxide solution (concentration 8wt%) are mixed in a volume ratio of 3:1, heated to 80°C, and then nano-silicon powder (the mass ratio of nano-silicon powder to solid sodium hydroxide is 125:1) is added in batches for multiple times, and then the temperature is controlled to be constant at 80°C, reacted for 6 hours, cooled, and filtered through a vacuum machine to obtain the nano-silica sol in the present invention.

[0037] The preparation principle of the above-mentioned nano-silicon solvent is as follows: nano-scale silicon powder reacts with water in an alkaline environment (sodium hydroxide solution provides the alkaline environment) to generate amorphous silicate monomers, and after the monomers are polymerized, nano-silica sol is obtained.

[0038] The remaining raw materials in the examples of the present invention were purchased.

[0039] Example 1 A method for preparing transparent soil

[0040] S1. Wash and dry the transparent glass sand at room temperature for 30 minutes to remove impurities and moisture, put it in a constant temperature box, set the temperature to 25°C, and keep it warm for 2 hours;

[0041] S2. Nano-silica sol and methylphenyl silicone oil were mixed in a mass ratio of 1:1.5 and stirred evenly to obtain a mixed solution, the mixed solution was kept at 25°C for 1.5 hours, and the refractive index of the mixed solution after the insulation was measured using an Abbe refractometer, so that the refractive index ratio of the mixed solution to the transparent glass sand was 1:1, and the pore fluid was obtained;

[0042] S3. The carbon nanotubes and the pore fluid prepared in S2 were mixed in a mass ratio of 7:1, stirred with a stirrer to uniformly disperse the carbon nanotubes in the pore fluid, and the pore fluid to which the carbon nanotubes were added was obtained, and placed in a thermostat (25° C.) for 6 h;

[0043] S4. Slowly add 100 parts of the transparent glass sand insulated in S1 to 8 parts of the porous fluid containing carbon nanotubes prepared in S3. After mixing, use a vacuum pump at 200W to evacuate for 20 minutes to remove the bubbles in the prepared transparent soil until the transparency meets the requirements.

[0044] Example 2 A method for preparing transparent soil

[0045] S1. Wash and dry the transparent glass sand at room temperature for 30 minutes to remove impurities and moisture, put it in a constant temperature box, set the temperature to 40°C, and keep it warm for 2 hours;

[0046] S2. Nano-silica sol and methylphenyl silicone oil are mixed in a mass ratio of 1:1.6 and stirred to obtain a mixed solution, the mixed solution is heated to 40°C, and the refractive index of the mixed solution after heating is measured using an Abbe refractometer, so that the refractive index ratio of the mixed solution to the transparent glass sand is 1:1, and a pore fluid is obtained;

[0047] S3. The carbon nanotubes and the pore fluid prepared in S2 were mixed in a mass ratio of 7:1, and stirred using a stirrer to uniformly disperse the carbon nanotubes in the pore fluid to obtain a pore fluid with carbon nanotubes added, and placed in a thermostat (40° C.) for 6 h;

[0048] S4. Slowly add 110 parts of transparent glass sand insulated in S1 to 8 parts of porous fluid containing carbon nanotubes prepared in S3. After mixing, use a vacuum pump at 200W to evacuate for 20 minutes to remove bubbles in the prepared transparent soil until the transparency meets the requirements.

[0049] Example 3 A method for preparing transparent soil

[0050] S1. Wash and dry the transparent glass sand at room temperature for 30 minutes to remove impurities and moisture, put it in a constant temperature box, set the temperature to 60°C, and keep it warm for 2 hours;

[0051] S2. Nano-silica sol and methylphenyl silicone oil are mixed in a mass ratio of 1:1.7 and stirred to obtain a mixed solution, the mixed solution is heated to 60°C, and the refractive index of the mixed solution after heating is measured using an Abbe refractometer, so that the refractive index ratio of the mixed solution to the transparent glass sand is 1:1, and a pore fluid is obtained;

[0052] S3. The carbon nanotubes and the pore fluid prepared in S2 were mixed in a mass ratio of 7:1, stirred with a stirrer to uniformly disperse the carbon nanotubes in the pore fluid, and the pore fluid to which the carbon nanotubes were added was obtained, and placed in a thermostat (60° C.) for 6 h;

[0053] S4. Slowly add 120 parts of transparent glass sand kept warm in S1 into 8 parts of porous fluid containing carbon nanotubes prepared in S3. After mixing, use a vacuum pump at 200W to evacuate for 30 minutes to remove bubbles in the prepared transparent soil until the transparency reaches the required level.

[0054] Example 4 A method for preparing transparent soil

[0055] S1. Wash and dry the transparent glass sand at room temperature for 30 minutes to remove impurities and moisture, put it in a constant temperature box, set the temperature to 90°C, and keep it warm for 2 hours;

[0056] S2. Mix nano-silica sol and methyl phenyl silicone oil in a mass ratio of 1:1.8, and stir evenly to obtain a mixed solution. Heat the mixed solution to 90 °C, and use an Abbe refractometer to measure the refractive index of the mixed solution after heating, so that the refractive index ratio of the mixed solution to the transparent glass sand is 1:1 to obtain a pore fluid;

[0057] S3. Mix carbon nanotubes and the pore fluid prepared in S2 in a mass ratio of 7:1, and stir with a blender to evenly disperse the carbon nanotubes in the pore fluid to obtain a pore fluid added with carbon nanotubes, and place it in a constant temperature oven (90 °C) for heat preservation for 6 h;

[0058] S4. Slowly add 110 parts of the transparent glass sand after heat preservation in S1 to 8 parts of the pore fluid containing carbon nanotubes prepared in S3. After mixing, use a vacuum pump to evacuate at 200 W for 40 min to remove the bubbles in the prepared transparent soil until the transparency meets the requirements.

[0059] Comparative Example 1

[0060] Same as Example 1, the only difference is that the nano-silica sol and methyl phenyl silicone oil are in a mass ratio of 1:1.3.

[0061] Comparative Example 2

[0062] Same as Example 4, the only difference is that the nano-silica sol and methyl phenyl silicone oil are in a mass ratio of 1:2.0.

[0063] Comparative Example 3

[0064] Same as Example 1, the only difference is that the nano-scale silicon powder in the nano-silica sol is replaced with amorphous silicon powder.

[0065] Performance Test Experiment

[0066] 1. Conduct performance tests on the consolidated transparent soil in Application Examples 1-5. The test method is as follows: Use a vane shear test to measure the sensitivity of the prepared transparent soil. The sensitivity of the soil refers to the ratio of the undisturbed soil to the unconfined compressive strength of the remolded soil immediately after testing. In engineering, the sensitivity St is commonly used to measure the influence of the structure of cohesive soil on strength. The higher the sensitivity of the soil, the stronger the structure, and the more the strength of the soil decreases after being disturbed. According to the sensitivity, cohesive soil can be divided into low sensitivity (1 < St ≤ 2) and medium sensitivity (2 < St ≤ 4). The higher the sensitivity of the soil, the stronger its structure, and the more obvious the decrease in the strength of the soil after being disturbed. The performance test results are shown in Table 1.

[0067] Table 1

[0068]

[0069]

[0070] According to Table 1, the transparent soil prepared in Examples 1-4 of the present invention has a transparency of more than 20 cm in thickness in a translucent state and has high optical clarity.

[0071] Transparency test method: Use a black and white camera to observe the prepared transparent soil at a fixed distance to obtain the gray value of the transparent soil. Set the transparent soil prepared in Example 1 as zero. Obtain the gray values ​​of the transparent soil prepared at different times and temperatures and compare them with the zero value to evaluate the change of transparency of the transparent soil with time and temperature. As time goes by, the transparency decreases by less than 5% after 21 days. As the temperature increases, the transparency decreases by less than 10% for every 10°C increase. The strength, compressibility and sensitivity of the transparent soil are stable, indicating that the properties of the transparent soil are relatively stable and suitable for long-term and high-temperature physical model tests.

[0072] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A transparent soil, characterized in that: The invention comprises the following raw materials: pore fluid, transparent glass sand and nano carbon tubes, wherein the mass ratio of the pore fluid, transparent glass sand and nano carbon tubes is 7:(100-120):1; the pore fluid is composed of nano silica sol and methyl phenyl silicone oil; The preparation method of the transparent soil comprises the following steps: mixing nano silica sol and methylphenyl silicone oil to obtain a mixed solution, heating the mixed solution so that the ratio of the refractive index of the heated mixed solution to the refractive index of transparent glass sand is 1:1 to obtain a pore fluid, mixing nano carbon tubes and the pore fluid, keeping the temperature, adding the heat-insulated transparent glass sand, mixing, and evacuating to obtain the transparent soil; The mass ratio of the nano-silica sol and the methylphenyl silicone oil is 1:(1.5-1.8); The heating temperature is 25-90°C; The temperature at which the carbon nanotubes and the pore fluid are kept after being mixed is 25-90° C.; The insulation temperature of the transparent glass sand is 25-90°C.

2. An application of the transparent soil according to claim 1 in a physical model test in geotechnical engineering, characterized in that: The transparent soil is loaded and consolidated to complete the laying of a layer of transparent soil, and then the laying is repeated until the total thickness meets the requirements of the model test, and the loading and consolidation are performed in a distributed loading manner.

Citation Information

Patent Citations

  • A method for preparing a transparent soil-rock mixture

    CN111650027B

  • Preparation method, product and application of soft rock transparent similar material

    CN113248188A