Low-loss high DC bias FeSi soft magnetic composite material and preparation method thereof

By adhering FeSiAl particles on the surface of FeSi powder, the FeSi@FeSiAl composite powder with core-shell structure was prepared, combined with insulation treatment and annealing heat treatment, the shortcomings of FeSi soft magnetic composite material at high frequency were solved, and the low performance of FeSi soft magnetic composite material was achieved. Loss, high magnetic permeability and high frequency stability, suitable for industrial production.

CN118248450BActive Publication Date: 2024-11-12CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410467019.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-18
Publication Date
2024-11-12
Estimated Expiration
2044-04-18

AI Technical Summary

Technical Problem

While reducing eddy current losses, the existing FeSi soft magnetic composite materials are difficult to maintain high DC bias and saturated magnetic induction strength, and the insulating layer of the traditional preparation method is easily damaged, affecting magnetic permeability and loss performance.

Method used

By adhering ultrafine FeSiAl particles to the surface of FeSi powder, FeSi@FeSiAl composite powder with core-shell structure is prepared, and the eddy current loss is reduced by using the skin effect at high frequency, and material performance is improved through insulating treatment and annealing heat treatment.

Benefits of technology

FeSi soft magnetic composite materials with low loss, high DC bias and high magnetic permeability are achieved, suitable for high-frequency applications, good frequency stability, low cost, and suitable for industrial mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118248450B_ABST
    Figure CN118248450B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of electronic materials, and specifically relates to a low-loss high DC bias FeSi soft magnetic composite material and a preparation method thereof. The preparation method comprises: (1) mixing and stirring FeSi powder, FeSiAl particles and steel balls to obtain a core-shell type FeSi@FeSiAl composite powder; (2) subjecting the FeSi@FeSiAl composite powder to an inorganic and / or organic insulation treatment to obtain an insulation-coated composite powder; (3) further mixing the insulation-coated composite powder with a lubricant, pressing it into a blank by pressure, and then annealing and heat treating it in a protective gas atmosphere to obtain a FeSi soft magnetic composite material. The preparation method has mild process conditions and simple equipment, and is suitable for mass production; and the prepared FeSi soft magnetic composite material has high magnetic permeability and lower loss.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electronic materials, and in particular relates to a low-loss high DC bias FeSi soft magnetic composite material and a preparation method thereof. Background Art

[0002] Soft magnetic composite materials are made of metal magnetic powder after insulation coating, forming, heat treatment and other processes. They are also called metal magnetic powder cores. They have high magnetic permeability, low loss and three-dimensional isotropy. They are used as the core part of transformers, inductors and motor stators, and are widely used in power supply, motor and other technologies.

[0003] The metal magnetic powders used to make soft magnetic composite materials include pure Fe, FeSi, FeSiAl, FeNi or FeNiMo, etc. Among these soft magnetic composite materials, FeSi and FeSiAl have excellent performance and low price, and have become the two most widely used soft magnetic composite materials. Compared with FeSiAl soft magnetic composite materials, FeSi has lower price, better saturation magnetic induction intensity and DC bias, but its resistivity is low, so the loss is also larger. In order to maintain the high saturation magnetic induction intensity and high DC bias of the FeSi soft magnetic composite material, while obtaining low loss, especially low eddy current loss, and increasing its application range, for example, Chinese invention patent 201610797220.0 uses at least two of aerosolized FeSi6.5 powder, crushed FeSiAl powder and Mn-Zn ferrite powder as raw materials, the mass percentage of FeSi6.5 and / or FeSiAl is 95-97%, and the mass percentage of Mn-Zn ferrite powder is 1-5%, to obtain FeSi6.5 soft magnetic composite material; Chinese invention patent 202111607751.6 obtains a low-power metal soft magnetic composite material by coating and diffusing a low-melting point, high-resistivity, and easily oxidizable substance on the FeSi alloy grain boundary, so that the overall resistivity of the material is improved.

[0004] However, Patent 201610797220.0 mixes some FeSiAl into FeSi. Although the high resistivity of FeSiAl is beneficial to reducing the eddy current loss, it also reduces the DC bias characteristics and saturation magnetic induction intensity of FeSi. In addition, the FeSiAl powder prepared by the crushing method has an irregular shape, and the insulating layer is easily damaged during the pressing process, which is also an unfavorable factor for reducing magnetic loss; Patent 202111607751.6 uses a method of precipitating oxides at grain boundaries. Although it can increase the resistivity and reduce eddy current loss, it will also increase the hysteresis loss, and the oxide is a non-magnetic substance, which will make it difficult to increase the magnetic permeability. Summary of the invention

[0005] In view of the above problems, the present invention provides a method for preparing a low-loss high DC bias FeSi soft magnetic composite material, which is prepared into a core-shell structure FeSi@FeSiAl composite powder by adhering a layer of ultrafine FeSiAl particles on the surface of FeSi powder. At high frequencies, due to the skin effect, eddy currents flow through the surface of the FeSi@FeSiAl composite particles, and the resistivity of the FeSiAl particles on the surface is high. Therefore, the eddy currents generated are much smaller than those of pure FeSi particles, so that the eddy currents and eddy current losses of the entire soft magnetic composite material are reduced. The higher the frequency, the lower the loss, thereby improving the use frequency and performance stability of the product. In addition, due to the low content of FeSiAl and the fine particles, the high DC bias of FeSi is still maintained.

[0006] In order to achieve the above object, the present invention can adopt the following technical solutions:

[0007] On the one hand, the present invention provides a method for preparing a low-loss high DC bias FeSi soft magnetic composite material, which comprises: (1) mixing and stirring FeSi powder, FeSiAl particles and steel balls to obtain a core-shell type FeSi@FeSiAl composite powder; (2) subjecting the FeSi@FeSiAl composite powder to an inorganic and / or organic insulation treatment to obtain an insulation-coated composite powder; (3) further mixing the insulation-coated composite powder with a lubricant, pressing it into a blank by pressure, and then annealing and heat treating it in a protective gas atmosphere to obtain a low-loss high DC bias FeSi soft magnetic composite material.

[0008] Preferably, in the above step (1), in the Fe-Si powder, the Si content is 3wt.% to 6.5wt.%, and the rest is Fe; in the Fe-Si-Al powder, the Si content is 9.0wt.% to 9.6wt.%, the Al content is 5.4wt.% to 6.4wt.%, and the rest is Fe.

[0009] Preferably, in the above step (1), the average particle size of the FeSi powder is 5 μm to 200 μm, the particle size of the FeSiAl particles is 0.01 μm to 4 μm, and the ratio of the FeSi particle size to the FeSiAl particle size is ≥20.

[0010] It should be noted that the ratio of FeSi particle size to FeSiAl particle size is ≥20. The specific ratio data needs to be calculated and determined based on the frequency of use and the skin depth. When the working frequency is met, the skin depth of the FeSi powder particles is preferably equivalent to the FeSiAl particle size.

[0011] Preferably, in the above step (1), the weight ratio of FeSiAl powder to FeSi powder is (0.5-10):(99.5-90).

[0012] Preferably, in the above step (2), the FeSi powder, FeSiAl particles and steel balls are mixed and stirred for 20 minutes to 300 minutes at a stirring speed of 100 rpm to 1000 rpm to obtain FeSi@FeSiAl coated powder.

[0013] It should be noted that the above-mentioned mixing and stirring process can be completed in any equipment capable of achieving mixing and ball milling, such as a mixer or a ball mill; in addition, the mixing time of the mixing and stirring can be 20min to 300min, such as 50min to 250min, 80min to 200min or 120min to 150min, etc., and the stirring rate can be 100 rpm to 1000 rpm, such as 150 rpm to 900 rpm, 200 rpm to 800 rpm. n, 300 rpm ~ 700 rpm, 400 rpm ~ 600 rpm or 450 rpm ~ 550 rpm, etc.; until the two powders are evenly mixed and the small FeSiAl particles adhere to the large FeSi particles; in the present invention, 50min ~ 250min, 300 rpm ~ 700 rpm can be preferred. Under this parameter, the two powders can be mixed most quickly and evenly, and the small FeSiAl particles can effectively adhere to the large FeSi particles.

[0014] It should also be noted that in the present invention, fine particles of FeSiAl are coated on the surface of coarse particles of FeSi powder. On the one hand, the resistivity of the core-shell FeSi@FeSiAl composite powder is higher than that of FeSi, which is conducive to reducing eddy current loss; on the other hand, under the action of an alternating magnetic field, due to the skin effect, the eddy current generated by each particle of the soft magnetic composite material prepared in this way is mainly distributed in the FeSiAl particles in the outer layer, and the resistivity of the FeSiAl particles is significantly higher than that of FeSi. Therefore, the eddy current is much lower than that of a pure FeSi soft magnetic composite material, and the eddy current loss generated in this way is also significantly lower than that generated by a pure FeSi soft magnetic composite material. The combined effect of the two aspects results in a lower total loss of the prepared soft magnetic composite material.

[0015] Preferably, in the above step (2), the inorganic substance includes at least one of SiO2, Al2O3 or TiO2, and the organic substance includes one or more combinations of silicone resin or epoxy resin, and the total coating amount is 0.5wt.% to 5wt.%.

[0016] It should be noted that in the present invention, the FeSi@FeSiAl coated powder is further insulated and coated with a layer of organic and / or inorganic insulating material, and the coating method can be a mechanical mixing, physical bonding or chemical generation method.

[0017] Preferably, in the above step (3), the lubricant is one or more combinations of zinc stearate or lithium stearate; the content of the lubricant is 0.2wt.% to 1.2wt.% of the weight of the insulating coated composite powder.

[0018] It should be noted that during the pressurized forming process of the above-mentioned powder, the lubricant can reduce the friction between the powder particles and the forming die wall and between the powder particles, thereby facilitating the increase of the effective pressure during forming and the density of the pressed green body.

[0019] It should also be noted that if the lubricant content is too low, it will not play a role in reducing friction, and thus has no effect on increasing the density of the compact; if the content is too high, the compact density will be reduced, because the lubricant itself is a substance with very low density and is a non-magnetic substance, and will be discharged through thermal decomposition during the subsequent annealing heat treatment process, and become pores in the material. Therefore, in the present invention, 0.2wt.% to 1.2wt.%, more preferably 0.4wt.% to 0.6wt.%, is the best effect.

[0020] Preferably, in the above step (3), the annealing heat treatment includes a temperature of 400° C. to 800° C., a holding time of 30 min to 120 min, and an atmosphere of argon or nitrogen or a mixture of the two.

[0021] Preferably, in the above step (3), the pressure for pressing the green body may be 600 MPa to 2200 MPa, such as 1000 MPa to 2000 MPa, 1200 MPa to 1800 MPa or 1500 MPa to 1600 MPa.

[0022] Preferably, in the above step (3), the annealing heat treatment may include: a temperature of 400°C to 800°C, such as 450°C, 500°C, 550°C, 650°C, 700°C or 750°C, etc.; the holding time may be 30min to 120min, such as 50min, 70min, 90min or 100min, etc.

[0023] It should be noted that the role of annealing heat treatment is to remove the internal stress generated by the plastic deformation of the powder particles during the forming process, thereby reducing the coercive force, etc. If the annealing temperature is too low, the purpose of completely removing the internal stress cannot be achieved; if the temperature is too high, while removing the internal stress, it will also cause thermal decomposition of the insulating layer and promote grain growth, thereby increasing eddy current loss and deteriorating magnetic properties. In the present invention, the preferred temperature is 400°C to 800°C, and the holding time can be 30min to 120min, and the more preferred temperature is 600°C to 700°C, and the holding time can be 40min to 80min.

[0024] Preferably, in the above step (3), the protective gas may be Ar or N2 atmosphere.

[0025] Preferably, in the above step (3), the shape of the blank can be ring-shaped, E-shaped or U-shaped.

[0026] The embodiment of the present invention also provides a FeSi soft magnetic composite material prepared by the method for preparing the above-mentioned low-loss and high DC bias FeSi soft magnetic composite material.

[0027] The beneficial effects of the present invention include at least:

[0028] (1) The FeSi soft magnetic composite material prepared by the method for preparing a low-loss high DC bias FeSi soft magnetic composite material provided by the present invention has high magnetic permeability and lower loss, especially with the increase of frequency, the low loss is more obvious, and the frequency stability is good. With the increase of frequency, the magnetic permeability attenuation is very small, and it has smaller magnetic loss at high frequency.

[0029] (2) The preparation method of the low-loss high DC bias FeSi soft magnetic composite material provided by the present invention is very simple, easy to operate, low in cost, and suitable for industrial mass production; and the loss value of the FeSi soft magnetic composite material can be adjusted within a certain range by the particle size and content of the FeSiAl powder; and due to the low content of FeSiAl, the high DC bias of FeSi is still maintained.

[0030] (3) The low-loss high DC bias FeSi soft magnetic composite material provided by the present invention has a high resistivity, and at high frequencies, due to the skin effect, the eddy current of a single powder particle flows through the surface of the powder, and the surface layer of the powder is FeSiAl, and the resistivity of FeSiAl is significantly higher than that of FeSi, so that the eddy current loss of FeSi@FeSiAl is much lower than that of the pure FeSi magnetic powder core.

[0031] (4) The method for preparing the low-loss high DC bias FeSi soft magnetic composite material provided by the present invention has mild process conditions, simple equipment, and is easy to operate, and is suitable for mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Schematic diagram of core-shell FeSi@FeSiAl composite powder;

[0033] Figure 2 This is a SEM image of powder particles coated with an Al2O3 insulating layer on the core-shell FeSi@FeSiAl composite powder in Example 4;

[0034] Figure 3 This is the EDS diagram of the element distribution of the powder particles of the core-shell FeSi@FeSiAl composite powder in Example 4 coated with an Al2O3 insulating layer. DETAILED DESCRIPTION

[0035] The examples are provided to better illustrate the present invention, but the present invention is not limited to the examples. Therefore, those skilled in the art may make non-essential improvements and adjustments to the implementation scheme according to the above invention content, which still fall within the protection scope of the present invention.

[0036] The terms used herein are only used to describe specific embodiments and are not intended to limit the present disclosure. Unless the context has a significantly different meaning, expressions in the singular include expressions in the plural. As used herein, it should be understood that terms such as "include", "have", "include" are intended to indicate the presence of features, numbers, operations, components, parts, elements, materials or combinations. The terms of the present invention are disclosed in the specification, and are not intended to exclude the possibility that one or more other features, numbers, operations, components, parts, elements, materials or combinations thereof may exist or may be added. As used herein, " / " may be interpreted as "and" or "or", depending on the circumstances.

[0037] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with specific examples, but the content of the present invention is not limited to the following examples.

[0038] 1. Preparation of FeSi soft magnetic composite materials

[0039] Example 1

[0040] Prepare Fe-4.0Si powder by atomization method, weigh 100g of Fe-4.0Si powder with a particle size of 54μm and slowly put it into a mixer, then add 1.8g of 1.2μm Fe-9Si-6Al particles into the mixer, and put in several steel balls, the ball-to-material weight ratio (the weight ratio of steel balls to the total of FeSi powder and FeSiAl powder) is 1:1, turn on the mixer and adjust the speed to 300r / min to mix for 2h to obtain a mixed powder; mix the FeSi@FeSiAl composite powder with 20nm SiO2 powder for insulation coating, the SiO2 content is 1.5wt.%, then add 0.5wt.% KH550 and stir evenly, then add 1wt.% of silicone resin and stir evenly to obtain an insulation-coated composite powder. The schematic diagram of the insulation-coated composite powder is as shown below. Figure 1 shown.

[0041] 0.5wt.% zinc stearate lubricant was added to the coated composite powder and mixed evenly, and pressed into an annular compact (outer diameter 14mm*inner diameter 6mm*height 5mm) at a pressure of 2000MPa; the annular compact was heat treated in an Ar atmosphere for 50min at a heat treatment temperature of 660°C; and then cooled to room temperature in the furnace (ventilation was maintained during the process of cooling to room temperature in the furnace (to prevent the sample from being oxidized)) to obtain a FeSi soft magnetic composite material sample.

[0042] Example 2

[0043] The Fe-4.5Si powder prepared by atomization method, 100g of Fe-4.5Si powder with a particle size of 62μm is weighed and slowly put into a mixer, then 1.6g of 1.0μm Fe-9Si-6Al particles are added into the mixer, and a number of steel balls are put in, the ball-to-material weight ratio (the weight ratio of steel balls to the total weight of FeSi powder and FeSiAl powder) is 1:1, the mixer is turned on, the speed is adjusted to 350r / min, and mixed for 1.5h to obtain a mixed powder; the FeSi@FeSiAl composite powder is mixed with 30nm Al2O3 powder for insulation coating treatment, the Al2O3 content is 1.2wt.%, and then 0.8wt.% KH550 is added and stirred evenly, and then 1.2wt.% of silicone resin is added and stirred evenly to obtain an insulation-coated composite powder.

[0044] 0.6wt.% zinc stearate lubricant was added to the coated composite powder and mixed evenly, and pressed into an annular compact (outer diameter 14mm*inner diameter 6mm*height 5mm) at a pressure of 1800MPa; the annular compact was heat treated in an Ar atmosphere for 60min at a heat treatment temperature of 650°C; and then cooled to room temperature in the furnace (ventilation was maintained during the process of cooling to room temperature in the furnace (to prevent the sample from being oxidized)) to obtain a FeSi soft magnetic composite material sample.

[0045] Example 3

[0046] The Fe-5.2Si powder prepared by atomization method, 100g of Fe-5.2Si powder with a particle size of 48μm is weighed and slowly put into a mixer, then 1.4g of 0.8μm Fe-9Si-6Al particles are added into the mixer, and a number of steel balls are put in, the ball-to-material weight ratio (the weight ratio of steel balls to the total weight of FeSi powder and FeSiAl powder) is 1:1, the mixer is turned on, the speed is adjusted to 400r / min, and mixed for 1.2h to obtain a mixed powder; the FeSi@FeSiAl composite powder is mixed with 20nm SiO2 powder for insulation coating treatment, the SiO2 content is 1.0wt.%, and then 1.0wt.% of KH550 is added and stirred evenly, and then 1.0wt.% of silicone resin is added and stirred evenly to obtain an insulation-coated composite powder.

[0047] 0.4wt.% zinc stearate lubricant was added to the coated composite powder and mixed evenly, and pressed into an annular compact (outer diameter 14mm*inner diameter 6mm*height 5mm) at a pressure of 1700MPa; the annular compact was heat treated in an Ar atmosphere for 40min at a heat treatment temperature of 700°C; and then cooled to room temperature in the furnace (ventilation was maintained during the process of cooling to room temperature in the furnace (to prevent the sample from being oxidized)) to obtain a FeSi soft magnetic composite material sample.

[0048] Example 4

[0049] The Fe-3.8Si powder prepared by atomization method, 100g of Fe-4.8Si powder with a particle size of 42μm is weighed and slowly put into a mixer, then 1.3g of 1.2μm Fe-9Si-6Al particles are added into the mixer, and several steel balls are put in, the ball-to-material weight ratio (the weight ratio of steel balls to the total weight of FeSi powder and FeSiAl powder) is 1:1, the mixer is turned on, the speed is adjusted to 520r / min, and mixed for 1h to obtain a mixed powder; the FeSi@FeSiAl composite powder is mixed with 30nm Al2O3 powder for insulation coating treatment, the Al2O3 content is 1.5wt.%, and then 0.8wt.% KH550 is added and stirred evenly, and then 1.5wt.% of silicone resin is added and stirred evenly to obtain an insulation-coated composite powder.

[0050] 0.3wt.% zinc stearate lubricant was added to the coated composite powder and mixed evenly, and pressed into an annular compact (outer diameter 14mm*inner diameter 6mm*height 5mm) at a pressure of 1900MPa; the annular compact was heat treated in an Ar atmosphere for 50min at a heat treatment temperature of 680°C; and then cooled to room temperature in the furnace (ventilation was maintained during the process of cooling to room temperature in the furnace (to prevent the sample from being oxidized)) to obtain a FeSi soft magnetic composite material sample.

[0051] Among them, the SEM image and element distribution EDS image of the powder particles of the core-shell FeSi@FeSiAl composite powder coated with an Al2O3 insulating layer are shown in Figure 2 and Figure 3 shown.

[0052] Comparative Example 1

[0053] The Fe-4.0Si powder prepared by atomization method is weighed, 100 g of Fe-4.0Si powder with a particle size of 54 μm is slowly put into a mixer, and then 1.6 g of 34 μm Fe-9Si-6Al particles are added into the mixer, and a number of steel balls are put in, with a ball-to-material weight ratio (the weight ratio of steel balls to the total weight of FeSi powder and FeSiAl powder) of 1:1. The mixer is turned on and the speed is adjusted to 200 r / min and mixed for 3 hours to obtain a mixed powder; the powder is mixed with 30 nm Al2O3 powder for insulation coating treatment, the Al2O3 content is 1.5 wt.%, and then 0.8 wt.% of KH550 is added and stirred evenly, and then 1.5 wt.% of silicone resin is added and stirred evenly to obtain an insulation-coated composite powder.

[0054] 0.5wt.% zinc stearate lubricant was added to the coated composite powder and mixed evenly, and pressed into an annular compact (outer diameter 14mm*inner diameter 6mm*height 5mm) at a pressure of 1900MPa; the annular compact was heat treated in an Ar atmosphere for 50min at a heat treatment temperature of 680°C; and then cooled to room temperature in the furnace (ventilation was maintained during the process of cooling to room temperature in the furnace (to prevent the sample from being oxidized)) to obtain a FeSi soft magnetic composite material sample.

[0055] Comparative Example 2

[0056] Prepare Fe-5.2Si powder by atomization method, weigh 100g of Fe-5.2Si powder with a particle size of 48μm and slowly put it into a mixer, then add 1.4g of 20μm Fe-9Si-6Al particles into the mixer, and put in several steel balls, the ball-to-material weight ratio (the weight ratio of steel balls to the total of FeSi powder and FeSiAl powder) is 1:1, turn on the mixer, adjust the speed to 200r / min and mix for 3h to obtain a mixed powder; mix the powder with 20nm SiO2 powder for insulation coating treatment, the SiO2 content is 1.0wt.%, then add 1.0wt.% KH550 and stir evenly, then add 1.0wt.% of silicone resin and stir evenly to obtain an insulation-coated composite powder.

[0057] 0.4wt.% zinc stearate lubricant was added to the coated composite powder and mixed evenly, and pressed into an annular compact (outer diameter 14mm*inner diameter 6mm*height 5mm) at a pressure of 1700MPa; the annular compact was heat treated in an Ar atmosphere for 40min at a heat treatment temperature of 700°C; and then cooled to room temperature in the furnace (ventilation was maintained during the process of cooling to room temperature in the furnace (to prevent the sample from being oxidized)) to obtain a FeSi soft magnetic composite material sample.

[0058] 2. Performance Test

[0059] The FeSi soft magnetic composite material samples prepared in Examples 1 to 4 and the FeSi soft magnetic composite material sample prepared in Comparative Example 1 were respectively tested for magnetic permeability and magnetic loss using a SY-8218 AC BH analyzer. The obtained sample properties are shown in Table 1 (B max =50mT).

[0060] Table 1 Performance of samples prepared differently

[0061]

[0062]

[0063] From Table 1 above, we can see that:

[0064] Compared with the existing FeSi soft magnetic composite materials (prepared by Comparative Examples 1 and 2), the FeSi soft magnetic composite material sample prepared in Example 1 has better magnetic permeability and frequency characteristics. As the frequency increases, the magnetic permeability has better stability; it has smaller magnetic loss at high frequencies; and the DC bias is equivalent.

[0065] Compared with the existing FeSi soft magnetic composite materials (prepared by Comparative Examples 1 and 2), the FeSi soft magnetic composite material sample prepared in Example 2 has better magnetic permeability and frequency characteristics. As the frequency increases, the magnetic permeability has better stability; it has smaller magnetic loss at high frequencies; and the DC bias is equivalent.

[0066] Compared with the existing FeSi soft magnetic composite materials (prepared by Comparative Examples 1 and 2), the FeSi soft magnetic composite material sample prepared in Example 3 has better magnetic permeability and frequency characteristics. As the frequency increases, the magnetic permeability has better stability; it has smaller magnetic loss at high frequencies; and the DC bias is equivalent.

[0067] Compared with the existing FeSi soft magnetic composite materials (prepared by Comparative Examples 1 and 2), the FeSi soft magnetic composite material sample prepared in Example 4 has better magnetic permeability and frequency characteristics. As the frequency increases, the magnetic permeability has better stability; it has smaller magnetic loss at high frequencies; and the DC bias is equivalent.

[0068] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be covered by the scope of the claims of the present invention.

Claims

1. A method for preparing a low-loss high DC bias FeSi soft magnetic composite material, characterized in that: include: (1) mixing FeSi powder, FeSiAl particles and steel balls to obtain core-shell FeSi@FeSiAl composite powder; (2) subjecting the FeSi@FeSiAl composite powder to an inorganic and / or organic insulation treatment to obtain an insulation-coated composite powder; (3) further mixing the insulation-coated composite powder with a lubricant, pressing it into a green body by pressure, and then annealing and heat treating it in a protective gas atmosphere to obtain a low-loss high DC bias FeSi soft magnetic composite material; wherein the average particle size of the FeSi powder is 5 μm to 200 μm, the particle size of the FeSiAl particles is 0.01 μm to 4 μm, and the ratio of the FeSi particle size to the FeSiAl particle size is ≥20; and the weight ratio of the FeSiAl powder to the FeSi powder is (0.5 to 10): (99.5 to 90).

2. The method for preparing the low-loss high DC bias FeSi soft magnetic composite material according to claim 1, characterized in that: In Fe-Si powder, the Si content is 3wt.% to 6.5wt.%, and the rest is Fe; in Fe-Si-Al powder, the Si content is 9.0wt.% to 9.6wt.%, the Al content is 5.4wt.% to 6.4wt.%, and the rest is Fe.

3. The method for preparing the low-loss high DC bias FeSi soft magnetic composite material according to claim 1 or 2, characterized in that: In step (1), FeSi powder, FeSiAl particles and steel balls are mixed and stirred for 20 minutes to 300 minutes at a stirring speed of 100 rpm to 1000 rpm to obtain FeSi@FeSiAl coated powder.

4. The method for preparing the low-loss high DC bias FeSi soft magnetic composite material according to claim 1 or 2, characterized in that: In step (2), the inorganic substance includes at least one of SiO2, Al2O3 or TiO2; the organic substance includes one or more combinations of silicone resin or epoxy resin, and the total coating amount is 0.5wt.% to 5wt.%.

5. The method for preparing the low-loss high DC bias FeSi soft magnetic composite material according to claim 1 or 2, characterized in that: In step (3), the lubricant is one or more combinations of zinc stearate or lithium stearate; the content of the lubricant is 0.2wt.% to 1.2wt.% of the weight of the insulating coated composite powder.

6. The method for preparing a low-loss high DC bias FeSi soft magnetic composite material according to claim 1 or 2, characterized in that: In step (3), the annealing heat treatment includes a temperature of 400°C to 800°C, a holding time of 30min to 120min, and an atmosphere of argon or nitrogen or a mixture of the two.

7. The FeSi soft magnetic composite material prepared by the method for preparing the low-loss and high DC bias FeSi soft magnetic composite material according to any one of claims 1 to 6.