Aluminum rod for ultra-thin aluminum profile, preparation method and ultra-thin aluminum profile

By adding SiCw and rare earth elements to the aluminum rod and using Ca-Al layered protective coating, the problem of easy corrosion of ultra-thin aluminum profiles is solved, its strength and corrosion resistance are improved, and high mechanical properties and wear resistance are achieved sex.

CN118256780BActive Publication Date: 2024-11-15CHANGZHOU SHUOYUAN NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410649642.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-24
Publication Date
2024-11-15
Estimated Expiration
2044-05-24

AI Technical Summary

Technical Problem

Ultra-thin aluminum profiles are susceptible to corrosive media and bacteria, resulting in poor mechanical properties and need to improve their corrosion resistance and strength.

Method used

By adding SiCw and rare earth elements to the aluminum rod and using an optimized ball milling and forming process, the grain size is refined, the dislocation density and corrosion resistance are increased; at the same time, the Ca-Al layer is used as the protective coating filler, combined with Chitosan and epoxychlorohydrin form a protective layer with high wear resistance and antibacterial properties, further improving the corrosion resistance of aluminum profiles.

Benefits of technology

It significantly improves the strength and corrosion resistance of aluminum profiles, enhances its effect on hindering dislocation movement, improves mechanical properties and wear resistance, and provides long-term corrosion protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present application relates to the technical field of aluminum profiles, and specifically discloses an aluminum rod for ultra-thin aluminum profiles, a preparation method, and an ultra-thin aluminum profile. An aluminum rod for ultra-thin aluminum profiles, comprising the following materials in mass percentage: Mg 0.5%-0.55%; Si 0.7%-0.75%; Cu 0.15%-0.25%; Mn 0.25%-0.30%; Cr 0.15%-0.20%; Ti 0.03%-0.06%; SiCw 0.4%-0.8%; the remainder is Al and impurities; its preparation method is: S1, sintering powder; S2, ball milling; S3, molding. An ultra-thin aluminum profile, using the above-mentioned aluminum rod for ultra-thin aluminum profiles, including a profile body and a protective layer. The ultra-thin aluminum profile of the present application can be used in the field of decoration, and has the advantages of light weight, excellent mechanical properties, and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of aluminum profiles, and more specifically, to an aluminum rod for ultra-thin aluminum profiles, a preparation method, and an ultra-thin aluminum profile. Background Art

[0002] Aluminum alloy is the most widely used type of nonferrous metal structural material in industry. It has been widely used in aviation, aerospace, automobile, machinery manufacturing, shipbuilding and chemical industries. With the rapid development of industrial economy, the demand for aluminum alloy welded structural parts is increasing, which has led to in-depth research on the weldability of aluminum alloy. At present, aluminum alloy is the most widely used alloy.

[0003] At present, ultra-thin aluminum profiles are widely used in the decoration field due to their low density, light weight and excellent mechanical properties. However, due to their thin thickness, they are more susceptible to erosion by corrosive media, bacteria, etc., resulting in poor mechanical properties of ultra-thin profiles, so this needs to be improved. Summary of the invention

[0004] In order to improve the problem that ultra-thin profiles are easily corroded, the present application provides an aluminum rod for ultra-thin aluminum profiles, a preparation method and an ultra-thin aluminum profile, which adopt the following technical solutions:

[0005] In a first aspect, the present application provides an aluminum rod for ultra-thin aluminum profiles, comprising the following materials in percentage by mass:

[0006] Mg 0.5%-0.55%;

[0007] Si 0.7%-0.75%;

[0008] Cu 0.15%-0.25%;

[0009] Mn 0.25%-0.30%;

[0010] Cr 0.15%-0.20%;

[0011] Ti 0.03%-0.06%;

[0012] SiCw 0.4%-0.8%;

[0013] The balance is Al and impurities.

[0014] By adopting the above technical solution, the present application adds SiCw to the aluminum rod material. First, SiCw can accumulate at the grain boundaries of the aluminum rod, increase the dislocation density of the aluminum rod, and produce dislocation strengthening; secondly, SiCw is dispersed in the aluminum rod substrate, and the whiskers can migrate with the flow of particles in the aluminum rod substrate. SiCw plays a restraining role at the grain boundaries, limits the growth trend of the grains, refines the grain size in the aluminum rod substrate, and increases the surface area of ​​the grains, thereby improving the hindering effect on dislocation movement, thereby effectively improving the strength of the aluminum rod; finally, the addition of whiskers can bear the pressure load, so the aluminum profile prepared using the above aluminum rod has higher strength.

[0015] In addition, the ratio of Ti and Mg is optimized. The appropriate Ti ratio can further refine the grain size in the aluminum rod and effectively improve the strength of the aluminum rod; the appropriate Mg ratio can make the aluminum rod have better corrosion resistance, eliminate the unstable β phase, and eliminate the sensitivity to intergranular corrosion or stress corrosion, thereby improving the corrosion resistance of aluminum rods and aluminum profiles.

[0016] Optional, aluminum bars for ultra-thin aluminum profiles, including the following materials in mass percentage:

[0017] Mg 0.5%-0.55%;

[0018] Si 0.7%-0.75%;

[0019] Cu 0.15%-0.25%;

[0020] Mn 0.25%-0.30%;

[0021] Cr 0.15%-0.20%;

[0022] Ti 0.03%-0.06%;

[0023] SiCw 0.4%-0.8%;

[0024] Rare earth 0.2%-0.3%;

[0025] The balance is Al and impurities.

[0026] By adopting the above technical solution, rare earth elements are added to the aluminum rod, and the introduction of rare earth elements can effectively improve the mechanical properties of the aluminum rod, neutralize the harmful effects of iron and silicon elements in the aluminum rod, and thus effectively improve the corrosion resistance of the aluminum rod and aluminum profiles. The amount of rare earth added is optimized, and the appropriate amount of addition can neutralize the harmful effects of iron and silicon elements, improve the mechanical properties and corrosion resistance of the aluminum rod; if the amount of rare earth added is too high, it is easy to affect the corrosion resistance of the aluminum rod.

[0027] In a second aspect, the present application provides a method for preparing an aluminum rod for ultra-thin aluminum profiles, using the following technical solution:

[0028] A method for preparing an aluminum rod for ultra-thin aluminum profiles comprises the following steps:

[0029] S1. Sintering and powdering: Mg, Si, Cu, Mn, Cr, Ti and Al are configured according to mass percentage, smelted at high temperature to obtain aluminum alloy solution, cast, extruded, cooled to obtain aluminum alloy profiles, crushed to obtain aluminum alloy powder;

[0030] S2, ball milling: aluminum alloy powder and SiCw are ball milled at a ball-to-material ratio of 2-3:1 to obtain ball milled powder;

[0031] S3. Molding: Take the ball-milled powder, cold press and sinter it to obtain an aluminum rod.

[0032] By adopting the above technical scheme, the ball-to-material ratio of aluminum alloy powder and SiCw in the ball milling process is optimized. The appropriate ball-to-material ratio can change the powder particles from the original spherical shape to regular discs, and the edges of the disc-shaped powders are relatively smooth, with almost no breakage. The aluminum alloy powders are not prone to agglomeration, so that SiCw can stably adhere to the surface of the aluminum alloy powder, thereby stably improving the strength of aluminum rods and aluminum profiles.

[0033] In a third aspect, the present application provides an ultra-thin aluminum profile, which adopts the following technical solution:

[0034] An ultra-thin aluminum profile, using the above-mentioned aluminum rod for ultra-thin aluminum profile, includes a profile body and a protective layer, wherein the protective layer is coated with a protective coating, and the protective coating includes the following materials in parts by weight:

[0035] Chitosan 0.03-0.06 parts;

[0036] 15-25 parts of octadecylamine;

[0037] Ascorbic acid 0.03-0.06 parts;

[0038] Ca-Al layer 0.01-0.03 parts;

[0039] Epichlorohydrin 1-3 parts;

[0040] 10 parts water.

[0041] By adopting the above technical solution, the Ca-Al layer is selected as the filler of the protective coating. The Ca-Al layer is a three-dimensional network composite, so that the protective layer obtains a better stress dispersion effect, and the protective layer obtains excellent wear resistance and abrasion resistance, thereby improving the mechanical properties and wear resistance of the aluminum profile. At the same time, chitosan is added to the protective coating. Under the cross-linking effect of epichlorohydrin, chitosan can be loaded on the Ca-Al layer, which can not only improve the bonding effect between the Ca-Al layer and the aluminum profile body, so that the protective layer can stably protect the aluminum profile; it can also give the protective coating a certain antibacterial effect, further improving the corrosion resistance of the aluminum profile.

[0042] Optionally, the Ca-Al layer is a Ca-Al layer intercalated with an intercalating agent, and the intercalating agent includes dodecyl sulfonic acid.

[0043] By adopting the above technical scheme, dodecyl sulfonate is inserted into the lamellar structure of the Ca-Al layer, the original hydrophilic structure in the Ca-Al layer is destroyed, the interlayer spacing of the hydrotalcite-like structure is increased, and hydrophobic segments are introduced into the Ca-Al layer, which effectively improves the hydrophobicity of the protective layer, thereby reducing the retention time of corrosive liquids on the protective layer, thereby improving the corrosion resistance of the aluminum profile.

[0044] Optionally, the intercalant further comprises molybdate.

[0045] By adopting the above technical scheme, molybdate, as a low-toxic water treatment corrosion inhibitor, has an excellent corrosion inhibition effect. After the molybdate is intercalated in the Ca-Al layer, when the Ca-Al layer receives the stimulation response of the corrosive ions, it can release the molybdate ions between the layers. On the one hand, the molybdate ions are used to delay the occurrence of corrosion. On the other hand, the corrosive ions are prevented from entering the interlayer and contacting the aluminum profile, thereby improving the corrosion resistance of the aluminum profile.

[0046] Optionally, the intercalant further comprises sorbate.

[0047] By adopting the above technical scheme, sorbate is selected as the intercalation agent, and sorbic acid root is intercalated in the Ca-Al layer. Sorbic acid root has excellent antiseptic effect and can have a good inhibitory effect on various fungi such as mold. Sorbic acid root can be slowly released from between the layers, so that the protective layer obtains excellent bacterial corrosion resistance.

[0048] Optionally, the protective coating further comprises 1-2 parts by weight of silicon dioxide.

[0049] By adopting the above technical solution, silica is added to the protective coating, which can further increase the density of the protective layer, improve the wear resistance and strength of the protective layer; and the addition of silica can form a micro-nano structure in the protective layer, further improve the hydrophobic effect of the protective layer, and further improve the corrosion resistance of the protective layer.

[0050] Optionally, the profile body is subjected to surface treatment, and the surface treatment is as follows: the profile body is immersed in an etching solution, immersed, washed, and dried to obtain an etched body, i.e., a profile body subjected to surface treatment; the etching solution includes hydrochloric acid, hydrogen peroxide, and oxalic acid.

[0051] By adopting the above technical solution, the profile body is etched, and hydrochloric acid, hydrogen peroxide and oxalic acid are used as etching liquid, which can form a stepped micro-nano structure on the surface of the profile body, so that the profile surface can obtain a uniform hydrophobic effect. The generation of micro-nano structure can not only trap air, form a certain air layer, and prevent corrosive materials from corroding the profile body; it can also improve the tightness of the bonding between the protective layer and the profile body, so that the protective layer can stably protect the aluminum profile.

[0052] Optionally, the surface treatment further comprises a deposition treatment: immersing the etched body in a Ni / Ni(OH)2 deposition solution, performing deposition treatment, washing, and drying to obtain a deposited body, i.e., a profile body after surface treatment.

[0053] By adopting the above technical solution, a uniform micron / nano structure can be formed on the surface of the profile body through deposition treatment, and a primary protective layer can be formed on the surface of the aluminum profile, which can stably trap air and form a stable air layer, effectively reducing the contact between the profile body and the outside world, and further improving the corrosion resistance of the aluminum profile. In addition, the bonding between the protective layer and the aluminum profile can be further improved, so that the aluminum profile can obtain long-term corrosion protection.

[0054] In summary, this application has the following beneficial effects:

[0055] 1. Since the present application adds SiCw to the aluminum rod material, firstly, SiCw can accumulate at the grain boundaries of the aluminum rod, thereby increasing the dislocation density of the aluminum rod and generating dislocation strengthening; secondly, SiCw is dispersedly distributed in the aluminum rod substrate, and the whiskers can migrate along with the flow of particles in the aluminum rod substrate. SiCw plays a restraining role at the grain boundaries, restricts the growth trend of the grains, refines the grain size in the aluminum rod substrate, and increases the surface area of ​​the grains, thereby increasing the hindering effect on the dislocation movement, thereby effectively improving the strength of the aluminum rod; finally, the addition of whiskers can bear the pressure load, so the aluminum profile prepared using the above-mentioned aluminum rod has a higher strength.

[0056] In addition, the ratio of Ti and Mg is optimized. The appropriate Ti ratio can further refine the grain size in the aluminum rod and effectively improve the strength of the aluminum rod; the appropriate Mg ratio can make the aluminum rod have better corrosion resistance, eliminate the unstable β phase, and eliminate the sensitivity to intergranular corrosion or stress corrosion, thereby improving the corrosion resistance of aluminum rods and aluminum profiles.

[0057] 2. In this application, Ca-Al layered materials are selected as fillers for protective coatings. Ca-Al layered materials are three-dimensional network-like composites, which enable the protective layer to obtain better stress dispersion effects, and enable the protective layer to obtain excellent wear resistance and abrasion resistance, thereby improving the mechanical properties and wear resistance of the aluminum profile. At the same time, chitosan is added to the protective coating. Under the cross-linking effect of epichlorohydrin, chitosan can be loaded on the Ca-Al layered materials, which can not only improve the bonding effect between the Ca-Al layered materials and the aluminum profile body, so that the protective layer can stably protect the aluminum profile; it can also give the protective coating a certain antibacterial effect, further improving the corrosion resistance of the aluminum profile.

[0058] 3. This application can form a uniform micron / nano structure on the surface of the profile body through deposition treatment, can form a primary protective layer on the surface of the aluminum profile, can stably trap air, form a stable air layer, effectively reduce the contact between the profile body and the outside world, and further improve the corrosion resistance of the aluminum profile. In addition, it can further improve the bonding between the protective layer and the aluminum profile, so that the aluminum profile can obtain long-term corrosion protection. DETAILED DESCRIPTION

[0059] The present application is further described in detail below with reference to the embodiments.

[0060] In the examples of the present application, the drugs used are as follows, but not limited thereto:

[0061] Drugs: Chitosan is industrial-grade chitosan from Shandong Yatu Biotechnology Co., Ltd.; octadecylamine was purchased from Sinopharm Chemical Reagent Co., Ltd.; ascorbic acid was purchased from Sinopharm Chemical Reagent Co., Ltd.

[0062] Preparation Example

[0063] Preparation Example of Ca-Al Layer

[0064] Preparation Example 1

[0065] 4mmol of hydrated calcium nitrate, 2mmol of hydrated aluminum nitrate, 4mL of water and 10mL of ethanol were stirred to dissolve, and then 5mL of propylene oxide was added and mixed thoroughly. The mixture was gelled at 40°C and aged for 12h to allow ethanol to be fully exchanged as an exchange solvent. The mixture was supercritically dried and then calcined at high temperature to obtain an aerogel, i.e., a Ca-Al layered material.

[0066] Preparation Example 2

[0067] Take Ca-Al layered material and sodium dodecyl sulfonate in a molar ratio of 1:2 respectively, mix the sodium dodecyl sulfonate with water to obtain a dispersion; then mix the Ca-Al layered material with water to obtain a slurry, mix the dispersion and the slurry, adjust the pH to 5-6 with 0.1 mol / L hydrochloric acid, vigorously stir at 70°C for 2h, filter, retain the solid, wash with water, and dry at 80°C to obtain a Ca-Al layered material intercalated with dodecylbenzene sulfonic acid.

[0068] Preparation Example 3

[0069] The Ca-Al layered material and sodium molybdate are taken at a molar ratio of 1:2 respectively, and the sodium molybdate is mixed with water to obtain a dispersion; the Ca-Al layered material is then mixed with water to obtain a slurry, the dispersion and the slurry are mixed, the pH is adjusted to 9-10 with 0.1 mol / L sodium hydroxide, and the mixture is vigorously stirred at 80°C for 2h, filtered, the solid is retained, washed with water, and dried at 60°C to obtain a molybdenum-intercalated Ca-Al layered material.

[0070] Preparation Example 4

[0071] The Ca-Al layered material and potassium sorbate are taken at a molar ratio of 1:2 respectively, and the potassium sorbate is mixed with water to obtain a dispersion; the Ca-Al layered material is then mixed with water to obtain a slurry, the dispersion and the slurry are mixed, the pH is adjusted to 8 using 0.1 mol / L sodium hydroxide, vigorously stirred at 80°C for 2h, crystallized at 60°C for 12h, filtered, the solids are retained, immersed in ethanol for 30min, washed with water, filtered, the solids are retained, and dried at 60°C to obtain a Ca-Al layered material with sorbate intercalation.

[0072] Protective coating preparation example

[0073] Preparation Example 5-8

[0074] Chitosan, octadecylamine, ascorbic acid, Ca-Al layered material, epichlorohydrin and water were taken respectively, and the specific masses are shown in the table below.

[0075] The Ca-Al layered material is dispersed in deionized water to obtain a 2 mg / mL suspension, chitosan is added to the suspension, ultrasonic vibration is performed, octadecylamine, ascorbic acid and epichlorohydrin are added, and the mixture is stirred and mixed to obtain a protective coating.

[0076] Table 1 Composition of protective coatings

[0077]

[0078] Preparation Example 9

[0079] The difference from Preparation Example 8 is that an equal mass of Ca-Al layered material intercalated with dodecylbenzenesulfonic acid is used to replace the Ca-Al layered material in Preparation Example 8 to prepare the protective coating.

[0080] Preparation Example 10

[0081] The difference from Preparation Example 8 is that a mixture of equal masses of Ca-Al layered materials intercalated with dodecylbenzenesulfonic acid and Ca-Al layered materials intercalated with molybdenum is used to replace the Ca-Al layered materials in Preparation Example 8 to prepare the protective coating.

[0082] Preparation Example 11

[0083] The difference from Preparation Example 8 is that an equal mass of Ca-Al layered material intercalated with dodecylbenzenesulfonic acid, a mixture of Ca-Al layered material intercalated with molybdenum, and Ca-Al layered material intercalated with sorbate are used to replace the Ca-Al layered material in Preparation Example 8 to prepare the protective coating.

[0084] Example

[0085] Examples 1-4

[0086] On the one hand, the present application provides an aluminum rod for ultra-thin aluminum profiles, comprising the following materials: Mg, Si, Cu, Mn, Cr, Ti, SiCw, and rare earth cerium, and the specific masses are shown in the table below.

[0087] In a second aspect, the present application provides a method for preparing an aluminum rod for an ultra-thin aluminum profile, comprising the following steps:

[0088] S1. Sintering powder making: Mg, Si, Cu, Mn, Cr, Ti and Al are arranged according to mass percentage, smelted at high temperature, the smelting temperature is 760°C, to obtain aluminum alloy melt, refined, kept at 740°C for 15 minutes, cast, extruded, cooled to obtain aluminum alloy profiles, crushed to obtain aluminum alloy powder;

[0089] S2, ball milling: aluminum alloy powder and SiCw are ball milled at a ball-to-material ratio of 2:1 to obtain ball milled powder;

[0090] S3. Molding: Take the ball-milled powder, cold press it, and sinter it at 617°C to obtain an aluminum rod.

[0091] In a third aspect, the present application provides an ultra-thin aluminum profile, including a profile body and a protective layer, wherein the protective layer is formed by coating with a protective coating. Specifically, this embodiment uses the protective coating prepared in Preparation Example 5 to prepare the protective layer.

[0092] The preparation method is as follows: immersing the profile body in the protective coating, ultrasonically oscillating for 1 hour, maintaining at 40°C for 24 hours, taking out the profile body, immersing and cleaning, and drying at 60°C for 10 hours to obtain the aluminum profile.

[0093] Table 2 Composition of aluminum rods in Examples 1-4

[0094]

[0095] Example 5

[0096] The difference from Example 2 is that this example uses the protective coating prepared in Preparation Example 6 to prepare the protective layer.

[0097] Example 6

[0098] The difference from Example 2 is that this example uses the protective coating prepared in Preparation Example 7 to prepare the protective layer.

[0099] Example 7

[0100] The difference from Example 2 is that this example uses the protective coating prepared in Preparation Example 8 to prepare the protective layer.

[0101] Example 8

[0102] The difference from Example 2 is that this example uses the protective coating prepared in Preparation Example 9 to prepare the protective layer.

[0103] Example 9

[0104] The difference from Example 2 is that this example uses the protective coating prepared in Preparation Example 10 to prepare the protective layer.

[0105] Example 10

[0106] The difference from Example 2 is that this example uses the protective coating prepared in Preparation Example 11 to prepare the protective layer.

[0107] Embodiment 11

[0108] The difference from Example 2 is that: the profile body is surface treated, the profile body is immersed in an etching solution, immersed, washed, and dried to obtain an etched body, that is, a profile body with surface treatment; the etching solution includes 2 mol / L hydrochloric acid, 2 mol / L hydrogen peroxide and 0.08 mol / L oxalic acid, and the etching time is 2 hours.

[0109] Example 12

[0110] The difference from Example 2 is that: the profile body is surface treated, the etched body is immersed in Ni / Ni (OH) 2 deposition liquid, deposited, washed, and dried to obtain a deposited body, that is, a profile body with surface treatment.

[0111] Deposition treatment: The etched body was used as the working electrode, the Pt wire was used as the counter electrode, the electrolyte consisted of 2 mol / L NH4Cl, 0.1 mol / L NiCl2·6H2O and 0.5 mol / L stearic acid, at room temperature and a constant cathode current of 1.0 A / cm 2 The electrodeposition was carried out for 300s under the conditions of , water washing, and drying at 60°C to obtain a surface-treated profile body.

[0112] Comparative Example

[0113] Comparative Example 1

[0114] The difference between this comparative example and Example 2 is that in this comparative example, SiCw is not added to the aluminum rod to prepare the ultra-thin aluminum profile.

[0115] Comparative Example 2

[0116] The difference between this comparative example and Example 2 is that in this comparative example, no protective layer is provided on the surface of the profile body.

[0117] Performance testing

[0118] (1) Corrosion resistance test: Refer to "GB / T10125-2012 Artificial Atmosphere Corrosion Test" to evaluate the corrosion resistance of aluminum profiles. Test conditions: neutral salt spray test, sodium chloride solution concentration 50g / L, pH value adjusted to 6.5±0.5, temperature 35±2℃, after observing for 96h, calculate the average corrosion rate. Reference formula: Average corrosion rate (mm / a) = (K×W) / (A×T×D). Where: K = 3.65×103; W = sample corrosion weight loss, g; A = sample area, cm 2 ; T = test time, days; D = material density, g / cm 3 The results are shown in Table 1. The lower the average corrosion rate, the better the corrosion resistance.

[0119] (2) Wear resistance test: The wear resistance of aluminum profiles was evaluated with reference to the standard "GB / T 12967.1-2020 Test methods for anodized films and organic polymer films of aluminum and aluminum alloys Part 1: Determination of wear resistance". The abrasive blasting method was used. The abrasive blasting tester was used. The abrasive was green silicon carbide with a particle size of F100. The test angle was 45°, the test pressure was 15 kPa, and the test height was 10 mm. The abrasive blasting experiment was conducted to test the abrasive blasting time. The longer the time, the better the wear resistance.

[0120] (3) Mechanical properties testing: The mechanical properties of ultra-thin decorative aluminum profile samples were tested in accordance with the test standard GB / T 228-2010.

[0121] Table 1 Performance test of preparation examples 1-3

[0122]

[0123] Combining the performance test comparison in Table 2, we can find that:

[0124] 1. By comparing Examples 1-3 with Comparative Examples 1-2, it can be found that the corrosion resistance, wear resistance and mechanical strength of the aluminum profiles prepared in Examples 1-3 are improved, which indicates that SiCw is added to the aluminum rod material in the present application to produce dislocation strengthening; SiCw plays a restraining role at the grain boundary, limits the growth trend of the grains, refines the grain size in the aluminum rod substrate, and improves the strength of the aluminum rod; and the addition of whiskers can bear the pressure load, so that the prepared ultra-thin aluminum profile has better strength and corrosion resistance.

[0125] 2. By comparing Example 4 with Example 2, it can be found that the corrosion resistance, wear resistance and mechanical strength of the aluminum profile prepared in Example 4 are improved, which shows that the introduction of rare earth elements in the present application can effectively improve the mechanical properties of the aluminum rod, neutralize the harmful effects of iron and silicon elements in the aluminum rod, and thus effectively improve the corrosion resistance of the aluminum rod and aluminum profile.

[0126] 3. By comparing Examples 5-6 with Example 2, it can be found that the corrosion resistance, wear resistance and mechanical strength of the aluminum profiles prepared in Examples 5-6 are improved, which means that the Ca-Al layered material is selected as the filler of the protective coating in the present application. The Ca-Al layered material is a three-dimensional network-like composite, which enables the protective layer to obtain better stress dispersion effect, and the protective layer obtains excellent wear resistance and abrasion resistance, thereby improving the mechanical properties and wear resistance of the aluminum profile.

[0127] 4. By comparing Example 7 with Example 2, it can be found that the corrosion resistance, wear resistance and mechanical strength of the aluminum profile prepared in Example 7 are improved, which means that in the present application, silica is added to the protective coating, and silica can further increase the density of the protective layer, improve the wear resistance and strength of the protective layer; and the addition of silica can form a micro-nano structure in the protective layer, further improve the hydrophobic effect of the protective layer, and further improve the corrosion resistance of the protective layer.

[0128] 5. By comparing Examples 8-10 with Example 2, it can be found that the corrosion resistance, wear resistance and mechanical strength of the aluminum profiles prepared in Examples 8-10 are improved, which means that in the present application, dodecyl sulfonate, molybdate or sorbate is inserted into the lamellar structure of the Ca-Al layer, and the original hydrophilic structure in the Ca-Al layer is destroyed. A hydrophobic segment is introduced into the Ca-Al layer, which effectively improves the hydrophobicity of the protective layer and reduces the residence time of the corrosive liquid on the protective layer. The corrosion inhibition of molybdate and the anti-corrosion of sorbate are utilized to effectively improve the corrosion resistance of the aluminum profile.

[0129] 6. By comparing Examples 11-12 with Example 2, it can be found that the corrosion resistance, wear resistance and mechanical strength of the aluminum profiles prepared in Examples 11-12 are improved, which means that in this application, the profile body is etched, and hydrochloric acid, hydrogen peroxide and oxalic acid are used as etching liquids to form a stepped micro-nano structure on the surface of the profile body, so that the profile surface obtains a uniform hydrophobic effect. Through deposition treatment, a uniform micron / nano structure can be formed on the surface of the profile body, and a primary protective layer can be formed on the surface of the aluminum profile, which can stably trap air and form a stable air layer, effectively reducing the contact between the profile body and the outside world, and further improving the corrosion resistance of the aluminum profile.

[0130] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An ultra-thin aluminum profile, characterized in that: The ultra-thin aluminum profile is prepared from aluminum rods, including a profile body and a protective layer, wherein the protective layer is coated with a protective coating, and the protective coating includes the following materials in parts by weight: Chitosan 0.03-0.06 parts; 15-25 parts of octadecylamine; Ascorbic acid 0.03-0.06 parts; Ca-Al layer 0.01-0.03 parts; Epichlorohydrin 1-3 parts; 10 parts water; The profile body is subjected to surface treatment, and the surface treatment is as follows: the profile body is immersed in an etching solution, immersed, washed, and dried to obtain an etched body, i.e., a profile body subjected to surface treatment; the etching solution includes hydrochloric acid, hydrogen peroxide, and oxalic acid; The surface treatment also includes a deposition treatment: immersing the etched body in a Ni / Ni(OH)2 deposition solution, performing a deposition treatment, washing, and drying to obtain a deposited body, i.e., a profile body subjected to surface treatment; The aluminum rod for ultra-thin aluminum profiles comprises the following materials in percentage by mass: Mg 0.5%-0.55%; Si 0.7%-0.75%; Cu 0.15%-0.25%; Mn 0.25%-0.30%; Cr 0.15%-0.20%; Ti 0.03%-0.06%; SiCw 0.4%-0.8%; The balance is Al and impurities.

2. The ultra-thin aluminum profile according to claim 1, characterized in that: The aluminum rod for ultra-thin aluminum profiles comprises the following materials in percentage by mass: Mg 0.5%-0.55%; Si 0.7%-0.75%; Cu 0.15%-0.25%; Mn 0.25%-0.30%; Cr 0.15%-0.20%; Ti 0.03%-0.06%; SiCw 0.4%-0.8%; Rare earth 0.2%-0.3%; The balance is Al and impurities.

3. The ultra-thin aluminum profile according to claim 1, characterized in that: The method for preparing the aluminum rod for ultra-thin aluminum profiles comprises the following steps: S1. Sintering and powdering: Mg, Si, Cu, Mn, Cr, Ti and Al are configured according to mass percentage, smelted at high temperature to obtain aluminum alloy solution, cast, extruded, cooled to obtain aluminum alloy profiles, crushed to obtain aluminum alloy powder; S2, ball milling: aluminum alloy powder and SiCw are ball milled at a ball-to-material ratio of 2-3:1 to obtain ball milled powder; S3. Molding: Take the ball-milled powder, cold press and sinter it to obtain an aluminum rod.

4. The ultra-thin aluminum profile according to claim 1, characterized in that: The Ca-Al layered material is a Ca-Al layered material treated with an intercalation agent, and the intercalation agent includes dodecyl sulfonic acid.

5. The ultra-thin aluminum profile according to claim 4, characterized in that: The intercalating agent also includes molybdate.

6. The ultra-thin aluminum profile according to claim 4, characterized in that: The intercalating agent also includes sorbate.

7. The ultra-thin aluminum profile according to claim 1, characterized in that: The protective coating also includes 1-2 parts by weight of silicon dioxide.