Method for accelerating redissolution of rare earth elements of rare earth copper alloy in solution treatment process

By using deep cryogenic rolling pre-deformation and solution treatment, the rare earth-rich phase is broken up and the dislocation density is increased, which solves the problem of the difficulty in dissolving the cerium-rich phase in rare earth copper alloys in traditional methods, and realizes the efficient utilization of rare earth elements and the improvement of alloy performance.

CN118957461AActive Publication Date: 2024-11-15CENT SOUTH UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410966885.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-15
Estimated Expiration
2044-07-18

AI Technical Summary

Technical Problem

In traditional solution treatment, the cerium-rich phase in cerium-containing rare earth copper alloys is difficult to completely dissolve, resulting in low utilization of cerium and affecting alloy performance.

Method used

A method combining cryogenic rolling pre-deformation with solution treatment is adopted, including cryogenic treatment, rolling deformation, solution treatment and water quenching steps. By breaking up rare earth-rich phases and increasing dislocation density, the uniform distribution of rare earth elements in copper alloys is promoted.

Benefits of technology

This improves the utilization rate of rare earth elements and alloy properties, ensures the complete dissolution of rare earth-rich phases in the matrix, and yields excellent cerium-containing rare earth copper alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957461A_ABST
    Figure CN118957461A_ABST
Patent Text Reader

Abstract

A method for accelerating redissolution of rare earth elements of rare earth copper alloy in the solution treatment process comprises the steps that the copper alloy containing the rare earth elements is taken and machined into a plate, and the thickness ranges from 3 mm to 10 mm; the plate is subjected to subzero treatment in a subzero box, the temperature of the plate is reduced to be lower than-150 DEG C, and heat preservation is conducted for 5-20 min; carrying out rolling deformation on the plate subjected to subzero treatment; the second step and the third step are repeated till the total rolling reduction rate reaches 30%-50%, and cryogenic pre-deformation is completed; after the plate is stabilized to the room temperature, solution treatment is conducted on the plate; and quenching the plate subjected to solution treatment in water, so that the plate is rapidly cooled to the water temperature, and a supersaturated solid solution structure is obtained. According to the method, the combined process of deep cold rolling pre-deformation and solution treatment is adopted, residues of a cerium-rich phase in the cerium-containing rare earth copper alloy are reduced, the dissolution rate of the cerium element in an alloy matrix is increased, the effect of the cerium element in the alloy is further improved, and the cerium-containing rare earth copper alloy with more excellent performance is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of rare earth copper alloy preparation, and particularly relates to a method for accelerating the re-dissolution of rare earth elements in a rare earth copper alloy during a solid solution treatment process, which can promote the dissolution of a segregated rare earth element-rich phase in a copper-silver alloy containing the rare earth element. Background Art

[0002] Copper alloys are widely used in electrical and electronic information fields due to their good strength, electrical conductivity, wear resistance, heat transfer and other properties. With the rapid development of high-tech, higher requirements are placed on the performance of high-performance copper alloys, especially high-strength and high-conductivity copper alloys. The addition of alloying elements greatly improves the shortcomings of pure copper, such as low strength and low wear resistance, but the scattering effect of alloying elements on electrons also significantly reduces its electrical conductivity. How to balance the relationship between strength and conductivity has become a long-term topic in copper alloy research.

[0003] Since copper and silver both have good electrical conductivity in the metal world, copper-silver alloys naturally become important candidates for the study of high-strength and high-conductivity copper alloys. The amount of silver added determines the high performance of copper-silver alloys. In-situ fiber-reinforced copper-silver alloys containing 6wt.% to 30wt.% have extremely high strength (up to about 1.7GPa) and good electrical conductivity after large strain deformation, but the high price of silver limits the promotion of copper-silver alloys in general industrial applications. In order to reduce the cost of the alloy, a trace amount of rare earth element cerium is added to the alloy after appropriately reducing the silver content, in order to compensate for the performance degradation caused by the reduction in silver content through the solid solution strengthening, fine grain strengthening, purification and impurity removal effects of the rare earth element in the alloy. In addition, the added rare earth element cerium, as the most abundant rare earth element in the earth's crust, is also much cheaper than silver.

[0004] Since pure cerium has a lower melting point than pure copper and pure silver, rare earth copper-silver alloys containing cerium often have segregation of cerium-rich phases after melting and casting. Solid solution treatment is usually used to promote the uniform distribution of cerium in the alloy so that more cerium can fully participate in the alloy and play a better role. However, in the actual solid solution process, even if the solid solution temperature is increased or the holding time is extended, the cerium-rich phase still exists in the alloy after solid solution treatment, which is difficult to dissolve completely, which is not conducive to the efficient use of cerium. Summary of the invention

[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a method for accelerating the re-dissolution of rare earth elements in rare earth copper alloys during solid solution treatment, so as to solve the problem that the cerium-rich phase in cerium-containing rare earth copper alloys is difficult to completely dissolve under the traditional solid solution treatment system, promote the dissolution of the insoluble cerium-rich phase in the cerium-containing rare earth copper alloy, and improve the utilization rate of the cerium element.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for accelerating the re-dissolution of rare earth elements in a rare earth copper alloy during a solid solution treatment process, comprising:

[0008] The first step: take the copper alloy containing rare earth elements and process it into a plate with a thickness of 3 to 10 mm;

[0009] Step 2: subjecting the plate to cryogenic treatment in a cryogenic box, reducing its temperature to below -150°C and keeping it warm for 5 to 20 minutes;

[0010] Step 3: Rolling and deforming the plate after cryogenic treatment;

[0011] Step 4: Repeat steps 2 and 3 until the total rolling reduction rate reaches 30-50%, completing deep cold pre-deformation;

[0012] Step 5: After the plate stabilizes to room temperature, perform solution treatment on it;

[0013] Step 6: Quench the solution treated plate in water to quickly cool it to water temperature to obtain a supersaturated solid solution structure.

[0014] In one embodiment, in the first step, the copper alloy containing rare earth elements is processed into a plate by preliminary hot deformation or cutting.

[0015] In one embodiment, in the third step, the rolling speed is 1.0-3.0 m / min, and the single-pass reduction rate is 5-7%.

[0016] In one embodiment, in the fourth step, a corresponding total rolling reduction ratio is selected according to the proportion of the rare earth element-rich phase. When the proportion of the rare earth element-rich phase is low, the pre-rolling reduction ratio is selected to be 30%; when the proportion of the rare earth element-rich phase increases, the total rolling reduction ratio is increased to 50%.

[0017] In one embodiment, in the fifth step, the solutionizing process is protected by argon gas to prevent oxidation of the copper alloy.

[0018] In one embodiment, the solution treatment conditions are: temperature 700-1000° C., and holding time 1-10 h.

[0019] In one embodiment, the copper alloy containing rare earth elements is a copper-silver alloy containing cerium elements, and the content of silver is 4-10% by weight, the content of cerium elements is 0.05-0.08% by weight, and the balance is copper.

[0020] In one embodiment, the content of silver is 5%, the content of cerium is 0.075%, and the balance is copper.

[0021] Compared with the prior art, the method for accelerating the re-dissolution of rare earth elements in rare earth copper alloys during solid solution treatment of the present invention adopts deep cold rolling pre-deformation to increase the dislocation density in the rare earth copper alloy, and at the same time, crushes part of the rare earth-rich phase to activate the activity of the rare earth cerium element, and then performs solid solution treatment to reduce the residual cerium-rich phase in the cerium-containing rare earth copper alloy, increase the dissolution rate of the cerium element in the alloy matrix, further improve the role of the cerium element in the alloy, and obtain a cerium-containing rare earth copper alloy with better performance.

[0022] Compared with the traditional single solid solution treatment system under the same conditions, the cerium-containing rare earth copper alloy prepared by the method of the present invention can dissolve more cerium-rich phases in the matrix after solid solution treatment, thereby providing the possibility of fully exerting the role of the cerium element and obtaining a more excellent cerium-containing rare earth copper alloy. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The schematic diagram of the process of accelerating the re-dissolution of rare earth elements in rare earth copper alloy during the solid solution treatment process of the present invention. Among them, (a) is deep cryogenic treatment before rolling; (b) is pre-deformation during rolling; (c) is solid solution treatment under argon protection and water quenching. The black phase segregated at the grain boundary in metallographic structure 1 and metallographic structure 2 in the figure is a rare earth-rich phase.

[0024] Figure 2 The metallographic structure pictures of the products obtained in each step in the embodiments of the present invention are shown in FIG. DETAILED DESCRIPTION

[0025] The embodiments of the present invention are described in detail below with reference to the accompanying drawings and examples.

[0026] like Figure 1 As shown, the present invention adopts deep cold rolling pre-deformation + solution treatment to accelerate the re-dissolution of rare earth elements in rare earth copper alloy, which mainly includes the following steps:

[0027] Step 1: The material is a copper alloy containing cerium rare earth elements prepared by a casting method, the cerium content of which is 0.05-0.08%, and is processed into a plate with a thickness of 3-10 mm after preliminary thermal deformation or cutting.

[0028] Step 2: Place the rare earth copper alloy plate in a liquid nitrogen cryogenic box for cryogenic treatment. When the temperature of the plate drops to below -150°C, keep it warm for 5 to 20 minutes.

[0029] Step 3: Rolling the cryogenically treated plate at a rolling speed of 1.0 to 5.0 m / min and a single-pass reduction rate of 5 to 7%.

[0030] Step 4: Repeat steps 2 and 3 until the total rolling reduction rate reaches 30-50%. Select the corresponding total rolling reduction rate according to the subsequent requirements for alloy properties to complete the deep cold pre-deformation process.

[0031] Step 5: After the deep cold rolling pre-deformation is completed, the plate is stabilized to room temperature and then transported to the heat treatment workshop.

[0032] Step 6: The plate is subjected to solid solution treatment in the heat treatment workshop. Argon gas is used for protection during the solid solution process to prevent severe oxidation of the copper alloy. The solid solution treatment temperature is 700-1000°C and the insulation time is 1-10h to achieve solid solution of cerium element.

[0033] Step 7: The plate after solution treatment is quickly quenched in water to quickly cool it to water temperature to obtain a supersaturated solid solution structure.

[0034] The main principle of the present invention is: through deep cold rolling pre-deformation, firstly, the coarse segregated cerium-rich rare earth element phase existing in the alloy can be broken, the copper / rare earth element interface area is increased, and a spatial basis is provided for accelerating the dissolution of the rare earth element-rich phase; secondly, the low temperature environment of deep cold rolling pre-deformation can inhibit the dynamic recovery of dislocations in the alloy, bringing a higher dislocation density. At the same time, the dislocation cells formed by a large number of dislocation entanglements can further hinder the grain boundary migration, increase the grain boundary density, and realize grain refinement. High-energy crystal defects such as grain boundaries and dislocations provide an energy basis for the dissolution of rare earth elements in the subsequent solid solution treatment process.

[0035] The rare earth element-rich copper alloy prepared by this method has less residual rare earth element-rich phase, more uniform distribution of rare earth elements, higher utilization rate of rare earth elements and higher performance of alloy. Due to its good effect of promoting the dissolution of rare earth-rich phase, it has broad application prospects in the field of rare earth copper alloy production and manufacturing.

[0036] In a specific embodiment of the present invention, taking the dissolution of the cerium-rich phase in the rare earth copper-silver alloy containing cerium as an example, Figure 1 As shown, it mainly includes the following steps:

[0037] Step 1: Use a 2mm thick rare earth copper-silver alloy containing cerium elements. The material composition and content are shown in Table 1. The metallographic structure is observed. At this time, there are a large amount of white silver-rich phase and a small amount of light gray cerium-rich phase in the alloy. Figure 2 a, that is Figure 1 Metallographic structure 1.

[0038] Table 1 Composition of cerium-containing rare earth copper-silver alloy (wt.%)

[0039] Element Type Ag Ce Cu content 5.00 0.075 margin

[0040] Step 2: Place the cerium-containing rare earth copper-silver alloy plate into liquid nitrogen for deep freezing treatment. When the temperature of the plate drops to -196°C, keep it warm for 10 minutes.

[0041] Step 3: Roll the plate after deep cryogenic treatment at a rolling speed of 2.0 m / min and a single-pass reduction rate of 5%.

[0042] Step 4: Repeat steps 2 and 3 until the total rolling reduction ratio reaches 50%, completing the deep cold pre-deformation process.

[0043] Step 5: After the deep cold rolling pre-deformation is completed, the plate is stabilized to room temperature and transported to the heat treatment workshop for metallographic structure observation. Figure 1 The metallographic structure 2 in the alloy shows that the white and gray phases are elongated, and some coarse white phases are broken. Figure 2 Middle b.

[0044] Step 6: In the heat treatment workshop, the deep cold rolled pre-deformed plates and the plates that have not been deep cold rolled pre-deformed are subjected to solid solution treatment. Argon gas is used for protection during the solid solution process to prevent severe oxidation of the copper alloy. The solid solution treatment temperature is 780°C and the holding time is 1h.

[0045] Step 7: The plate after solution treatment is quickly quenched in water to quickly cool it to water temperature to obtain a supersaturated solid solution structure. The metallographic structure is observed. No obvious white or gray phase is observed in the plate after deep cold rolling pre-deformation + solution treatment. Figure 2 In the figure d, it is shown that the silver-rich phase and the cerium-rich phase are all dissolved back into the copper matrix. However, the gray second phase is observed in the plate that is only subjected to solution treatment. Figure 2 Middle c.

Claims

1. A method for accelerating the re-dissolution of rare earth elements in rare earth copper alloys during solution treatment, characterized in that: include: The first step: take the copper alloy containing rare earth elements and process it into a plate with a thickness of 3 to 10 mm; Step 2: subjecting the plate to cryogenic treatment in a cryogenic box, reducing its temperature to below -150°C and keeping it warm for 5 to 20 minutes; Step 3: Rolling and deforming the plate after cryogenic treatment; Step 4: Repeat steps 2 and 3 until the total rolling reduction rate reaches 30-50%, completing deep cold pre-deformation; Step 5: After the plate stabilizes to room temperature, perform solution treatment on it; Step 6: Quench the solution treated plate in water to quickly cool it to water temperature to obtain a supersaturated solid solution structure.

2. The method for accelerating the re-dissolution of rare earth elements in rare earth copper alloys during solution treatment according to claim 1, characterized in that: In the first step, the copper alloy containing rare earth elements is processed into a plate by preliminary thermal deformation or cutting.

3. The method for accelerating the re-dissolution of rare earth elements in rare earth copper alloy according to claim 1, characterized in that: In the third step, the rolling speed is 1.0-3.0 m / min, and the single-pass reduction rate is 5-7%.

4. The method for accelerating the re-dissolution of rare earth elements in rare earth copper alloys during solution treatment according to claim 1, characterized in that: In the fourth step, the corresponding total rolling reduction rate is selected according to the proportion of the rare earth element-rich phase; when the proportion of the rare earth-rich phase is low, the pre-rolling reduction rate is selected to be 30%; when the proportion of the rare earth-rich phase increases, the total rolling reduction rate is increased to 50%.

5. The method for accelerating the re-dissolution of rare earth elements in rare earth copper alloys during solution treatment according to claim 1, characterized in that: In the fifth step, argon gas is used as protection during the solid solution process to prevent the copper alloy from oxidizing.

6. The method for accelerating the re-dissolution of rare earth elements in rare earth copper alloys during solution treatment according to claim 1 or 5, characterized in that: The solution treatment conditions are: temperature 700-1000° C., and holding time 1-10 hours.

7. The method for accelerating the re-dissolution of rare earth elements in rare earth copper alloys during solution treatment according to claim 1, characterized in that: The copper alloy containing rare earth elements is a copper-silver alloy containing cerium elements, wherein the content of silver is 4-10% by weight, the content of cerium elements is 0.05-0.08% by weight, and the balance is copper.

8. The method for accelerating the re-dissolution of rare earth elements in rare earth copper alloys during solution treatment according to claim 7, characterized in that: The content of silver is 4-10%, the content of cerium element is 0.05-0.08%, and the balance is copper.

Citation Information

Patent Citations

  • High-strength and high-conductivity Cu-Sc alloy and preparation method thereof

    CN112251627A

  • Copper alloy sheet for electrical / electronic component excellent in heat resistance

    JP2009263690A

  • Copper-based alloy material, production method therefor, and members or parts made of copper-based alloy material

    US20210317557A1