Antibacterial nonwoven fabric and preparation method thereof
By using selenium to modify zinc oxide or selenium to modify neodymium doped zinc oxide in nonwoven fabrics, combined with maleic anhydride grafting polypropylene, the problems of antibacterial agent uniformity and cost in antibacterial nonwoven fabrics are solved, and high antibacterial performance is achieved and the improvement of dispersion performance, maintaining antibacterial and friction resistance.
Patent Information
- Application Number
- CN202410409385.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-07
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-04-07
AI Technical Summary
The existing antibacterial non-woven fabrics have poor uniformity in spinning solutions and high cost of selecting antibacterial agents, especially the cost of silver particles and the cost of porous graphene microns is high and difficult to prepare.
Selenium-modified zinc oxide or Selenium-modified neodymium doped zinc oxide is used as antibacterial agent. By introducing rare earth metal neodymium on the surface of zinc oxide, the surface performance of zinc oxide is improved, and combined with maleic anhydride grafted polypropylene as a compatibility agent, it is prepared with high efficiency. Non-woven fabric with antibacterial properties.
The antibacterial and dispersive properties of non-woven fabrics are improved, the agglomeration of zinc oxide is inhibited, and the efficient antibacterial properties are maintained. After multiple washing and friction, the cost is reduced.
Smart Images

Figure CN118257062B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textile manufacturing, and in particular to an antibacterial nonwoven fabric and a preparation method thereof. Background Art
[0002] Non-woven fabrics are also called non-woven fabrics, needle-punched cotton, and needle-punched non-woven fabrics. They can be made in different thicknesses, feels, and hardnesses. Non-woven fabrics are moisture-proof, breathable, flexible, thin, flame-retardant, non-toxic and tasteless, inexpensive, and recyclable, and are widely used in different industries. Non-woven fabrics are widely used in the medical and health fields, which brings certain requirements for their antibacterial properties.
[0003] Compared with finishing the prepared non-woven fabric to make it have antibacterial properties, adding an antibacterial agent to the spinning solution or melt in advance to prepare antibacterial fibers, and then weaving antibacterial non-woven fabrics with antibacterial fibers, the antibacterial properties of the antibacterial non-woven fabrics can be stable and lasting, but they face the problems of poor uniformity of the spinning solution and the selection of antibacterial agents. There are also some existing technologies that provide better antibacterial non-woven fabrics. For example, CN115012210A discloses a tear-resistant antibacterial non-woven fabric and its preparation method, first using modified polylactic acid, polyurethane and polyamic acid as raw materials to make composite fibers, then using silver ammonia solution to treat the surface to obtain silver-loaded fibers, opening, combing, laying into a fiber mesh, and needle punching to obtain a prefabricated non-woven fabric; finally, the prefabricated non-woven fabric is subjected to electron beam irradiation, and then grafted with tributyl methyl ammonium bis (trifluoromethanesulfonyl) imide salt. This non-woven fabric has good antibacterial properties and excellent tear resistance, and can be used for the preparation of medical protective equipment. However, silver particles are expensive as bactericides. CN116575191A discloses an antibacterial flash-steamed composite nonwoven fabric and a preparation method thereof, wherein the nonwoven fabric comprises polyethylene, antibacterial particles and a slow-release toughening agent, wherein the mass fraction of the antibacterial particles in the antibacterial flash-steamed composite nonwoven fabric is 2-5%, and the mass fraction of the slow-release toughening agent in the antibacterial flash-steamed composite nonwoven fabric is 3-3.5%; the antibacterial particles are composited by porous graphene micron flowers and magnesium oxide nanoparticles; the mass fraction of the magnesium oxide nanoparticles in the antibacterial particles is 20-30%. This nonwoven fabric has good antibacterial properties and good mechanical properties, but the porous graphene micron flowers are expensive and difficult to prepare. Summary of the invention
[0004] In order to solve the technical problems existing in the prior art, the present invention provides an antibacterial non-woven fabric, which includes 100 to 120 parts of polypropylene, 10 to 15 parts of antibacterial agent, and 2 to 10 parts of compatibilizer by weight;
[0005] Wherein, the antibacterial agent is selenium-modified zinc oxide or selenium-modified neodymium-doped zinc oxide.
[0006] The antibacterial activity of zinc oxide against gram-negative bacteria, such as Enterobacter aerogenes, Escherichia coli and Klebsiella pneumoniae, and positive bacteria, such as Micrococcus luteus and Staphylococcus aureus, has been reported. It is generally believed that zinc oxide can release zinc ions, which can interfere with the metabolic process in bacterial cells and block the normal metabolism and biosynthesis process of bacteria. In particular, nanostructured zinc oxide can be used as a highly effective antibacterial agent and catalyst. The morphology and particle size of zinc oxide have a great influence on the performance. At the same time, coupling, co-doping and single doping with other nanoparticles or other oxide metals can change the surface, structure formation, crystallinity, optics, electricity and properties of the nanoparticles to enhance their antibacterial properties. Selenium is generally considered to have anti-tumor and antioxidant properties. The present invention combines selenium nanoparticles on the surface of zinc oxide. The results show that selenium-modified zinc oxide can improve the antibacterial properties of non-woven fabrics.
[0007] However, direct modification of zinc oxide surface with selenium will cause serious agglomeration, which reduces the binding performance of zinc oxide with bacteria. Therefore, the present invention also introduces rare earth metal neodymium into the preparation of zinc oxide, improves the surface performance of zinc oxide, and inhibits the agglomeration phenomenon.
[0008] Furthermore, the preparation method of selenium-modified zinc oxide comprises, in parts by weight,
[0009] Mix 5 to 10 parts of a water-soluble zinc salt, 2 to 5 parts of a regulating agent, and 30 to 60 parts of a first solvent, and then heat and stir to react to obtain zinc oxide;
[0010] 5 to 10 parts of zinc oxide and 1 to 3 parts of selenium nanoparticles are dispersed in 50 to 100 parts of a second solvent, and the selenium nanoparticles are combined on the surface of the zinc oxide under stirring to obtain selenium-modified zinc oxide.
[0011] Furthermore, the preparation method of selenium-modified neodymium-doped zinc oxide comprises, in parts by weight,
[0012] 5 to 10 parts of a water-soluble zinc salt, 0.5 to 1.5 parts of a water-soluble neodymium salt, 2 to 5 parts of a regulating agent, and 30 to 60 parts of a first solvent are mixed, and then heated and stirred for reaction to obtain neodymium-doped zinc oxide;
[0013] 5-10 parts of neodymium-doped zinc oxide and 1-3 parts of selenium nanoparticles are dispersed in 50-100 parts of a second solvent, and the selenium nanoparticles are combined on the surface of zinc oxide under stirring to obtain selenium-modified zinc oxide.
[0014] Furthermore, the regulating agent is oxalic acid or hexamethylenetetramine.
[0015] Furthermore, the first solvent is at least one of ethanol, methanol, propanol, isopropanol, glycerol, and ethylene glycol;
[0016] The second solvent is an ethanol aqueous solution with a volume fraction of 50% to 70%;
[0017] The heating raises the temperature to 60-80°C.
[0018] Furthermore, the preparation method of the selenium nanoparticles comprises, in parts by weight,
[0019] The water-soluble selenite, the reducing agent and water are mixed and stirred for reaction, and selenium nanoparticles are collected.
[0020] Furthermore, the concentrations of the water-soluble selenite and reducing agent are 1-3 mmol / L and 0.5-1 mmol / L respectively.
[0021] Furthermore, the reducing agent is at least one of chlorogenic acid, L-ascorbic acid and gallic acid.
[0022] Furthermore, the compatibilizer is maleic anhydride grafted polypropylene.
[0023] The present invention also provides a method for preparing an antibacterial nonwoven fabric, which comprises, by weight,
[0024] Obtain 100-120 parts of polypropylene, 10-15 parts of antimicrobial agent, and 2-10 parts of compatibilizer;
[0025] The polypropylene, antimicrobial agent and compatibilizer are mixed and granulated to obtain a blended masterbatch;
[0026] The blended masterbatch is drawn, hot-pressed and shaped to obtain an antibacterial non-woven fabric.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] The present invention combines selenium nanoparticles on the surface of zinc oxide. The results show that selenium-modified zinc oxide can improve the antibacterial properties of non-woven fabrics. In addition, the present invention introduces rare earth metal neodymium into the preparation of zinc oxide, improves the surface properties of zinc oxide, and inhibits agglomeration. The present invention does not need to add any surfactant in the regulation of zinc oxide. The introduction of neodymium enhances the dispersion properties of zinc oxide, thereby allowing selenium to be better dispersed on the surface of zinc oxide. The results show that the non-woven fabric containing selenium-modified neodymium-doped zinc oxide can still maintain high antibacterial properties after multiple washings and frictions.
[0029] Instruction Manual
[0030] Figure 1 The transmission electron micrograph of the selenium-modified zinc oxide prepared in Example 1 is shown;
[0031] Figure 2 The transmission electron microscope image of selenium-modified neodymium-doped zinc oxide prepared in Example 2 is shown;
[0032] Figure 3 The transmission electron microscope image of zinc oxide prepared in Comparative Example 1 is shown;
[0033] Figure 4 The transmission electron microscope image of the neodymium-doped zinc oxide prepared in Comparative Example 2 is shown;
[0034] Figure 5 Transmission electron microscopy images of selenium nanoparticles are shown. DETAILED DESCRIPTION
[0035] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0036] Introduction of some raw materials used in the embodiments of the present invention:
[0037] Polypropylene, model MF650Y, was purchased from LyondellBasell Polyolefins (Shanghai) Co., Ltd.;
[0038] Maleic anhydride grafted polypropylene, model B1, was purchased from Dongguan Dingxin Plastic Raw Materials Co., Ltd.
[0039] Other raw materials not mentioned are common raw materials. The above content is only to help illustrate the present invention and shall not be construed as a strict limitation of the present invention. Those skilled in the art can directly purchase the same / similar raw materials from the market or prepare them by themselves. These contents will not be repeated in the examples.
[0040] The following will be combined with the specific embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] Example 1
[0042] A method for preparing an antibacterial nonwoven fabric, the steps in parts by weight are as follows:
[0043] Step 1, weigh 100 parts of polypropylene, 10 parts of selenium-modified zinc oxide, and 5 parts of maleic anhydride-grafted polypropylene;
[0044] Step 2, polypropylene, selenium-modified zinc oxide, and maleic anhydride-grafted polypropylene are uniformly mixed, and granulated through a twin-screw extruder at 170° C. to obtain a blended masterbatch;
[0045] Step 3: Add the blended masterbatch into a wire drawing machine to form a fiber mesh, and then heat press the fiber mesh for 15 seconds at a temperature of 180° C. and a pressure of 5 MPa to form a fabric structure, and finally cool it naturally to set it.
[0046] Wherein, the preparation method of selenium-modified zinc oxide is:
[0047] 8 parts of zinc nitrate hexahydrate, 3 parts of oxalic acid and 50 parts of ethanol were stirred at a stirring rate of 300 rpm for 15 minutes to mix evenly, and then the temperature was raised to 70°C while stirring to react for 90 minutes to obtain a gel-like substance, and the gel-like substance was placed in a constant temperature oven at 80°C to dry for 12 hours, and then the dried product was placed in a muffle furnace at 400°C to calcine for 2 hours to obtain zinc oxide;
[0048] Disperse 5 parts of zinc oxide and 2 parts of selenium nanoparticles in 80 parts of 60% ethanol aqueous solution, stir at a stirring rate of 500 rpm for 3 hours, bind the selenium nanoparticles to the surface of zinc oxide, then filter and wash three times with water and ethanol respectively, and then dry in a constant temperature oven at 120°C for 6 hours to obtain selenium-modified zinc oxide.
[0049] The preparation method of selenium nanoparticles is as follows:
[0050] Sodium selenite pentahydrate, gallic acid and 50 mL of water were stirred at a stirring rate of 300 rpm for 30 min to obtain a mixed solution, so that the concentrations of sodium selenite pentahydrate and gallic acid in the mixed solution were 2 mmol / L and 1 mmol / L, respectively. Then, the pH was adjusted to 5.5 with 1 mol / L hydrochloric acid. The mixture was stirred for 2 h and the insoluble matter was collected by centrifugation at 12000 rpm and washed three times with water and ethanol respectively, and then dried in a constant temperature oven at 120°C for 6 h to obtain selenium nanoparticles.
[0051] Example 2
[0052] A method for preparing an antibacterial nonwoven fabric, the steps in parts by weight are as follows:
[0053] Step 1, weigh 100 parts of polypropylene, 10 parts of selenium-modified neodymium-doped zinc oxide, and 5 parts of maleic anhydride-grafted polypropylene;
[0054] Step 2, polypropylene, selenium-modified neodymium-doped zinc oxide, and maleic anhydride-grafted polypropylene are uniformly mixed, and granulated through a twin-screw extruder at 170° C. to obtain a blended masterbatch;
[0055] Step 3: Add the blended masterbatch into a wire drawing machine to form a fiber mesh, and then heat press the fiber mesh for 15 seconds at a temperature of 180° C. and a pressure of 5 MPa to form a fabric structure, and finally cool it naturally to set it.
[0056] Wherein, the preparation method of selenium-modified neodymium-doped zinc oxide is:
[0057] 8 parts of zinc nitrate hexahydrate, 0.8 parts of neodymium acetate tetrahydrate, 3 parts of oxalic acid and 50 parts of ethanol were stirred at a stirring rate of 300 rpm for 15 minutes to mix evenly, and then the temperature was raised to 70°C while stirring to react for 90 minutes to obtain a gel-like substance, and the gel-like substance was placed in an 80°C constant temperature oven to dry for 12 hours, and then the dried product was placed in a 400°C muffle furnace for calcination for 2 hours to obtain neodymium-doped zinc oxide;
[0058] 5 parts of neodymium-doped zinc oxide and 2 parts of selenium nanoparticles were dispersed in 80 parts of 60% by volume ethanol aqueous solution, stirred at a stirring rate of 500 rpm for 3 hours, and the selenium nanoparticles were bound to the surface of the neodymium-doped zinc oxide. The mixture was then filtered and washed three times with water and ethanol each, and then dried in a constant temperature oven at 120°C for 6 hours to obtain selenium-modified neodymium-doped zinc oxide.
[0059] The preparation method of selenium nanoparticles is the same as that in Example 1.
[0060] Comparative Example 1
[0061] A method for preparing an antibacterial nonwoven fabric, the steps in parts by weight are as follows:
[0062] Step 1, weigh 100 parts of polypropylene, 10 parts of zinc oxide, and 5 parts of maleic anhydride grafted polypropylene;
[0063] Step 2, the polypropylene, zinc oxide, and maleic anhydride grafted polypropylene are uniformly mixed, and granulated through a twin-screw extruder at 170° C. to obtain a blended masterbatch;
[0064] Step 3: Add the blended masterbatch into a wire drawing machine to form a fiber mesh, and then heat press the fiber mesh for 15 seconds at a temperature of 180° C. and a pressure of 5 MPa to form a fabric structure, and finally cool it naturally to set it.
[0065] Wherein, the preparation method of zinc oxide is the same as that in Example 1.
[0066] Comparative Example 2
[0067] A method for preparing an antibacterial nonwoven fabric, the steps in parts by weight are as follows:
[0068] Step 1, weigh 100 parts of polypropylene, 10 parts of neodymium-doped zinc oxide, and 5 parts of maleic anhydride-grafted polypropylene;
[0069] Step 2, the polypropylene, the neodymium-doped zinc oxide, and the maleic anhydride-grafted polypropylene are uniformly mixed, and granulated through a twin-screw extruder at 170° C. to obtain a blended masterbatch;
[0070] Step 3: Add the blended masterbatch into a wire drawing machine to form a fiber mesh, and then heat press the fiber mesh for 15 seconds at a temperature of 180° C. and a pressure of 5 MPa to form a fabric structure, and finally cool it naturally to set it.
[0071] Wherein, the preparation method of neodymium-doped zinc oxide is the same as that in Example 2.
[0072] The morphologies of the selenium-modified zinc oxide of Example 1, the selenium-modified neodymium-doped zinc oxide of Example 2, the zinc oxide of Comparative Example 1, the neodymium-doped zinc oxide of Comparative Example 2, and the selenium nanoparticles were observed using a transmission electron microscope. The results are as follows: Figure 1 to Figure 5 As shown. Figure 3 It can be seen that the unmodified zinc oxide prepared by the sol-gel method of the present invention has a smaller particle size and more obvious agglomeration; Figure 4 It can be seen that the introduction of neodymium during preparation significantly enhances the dispersion performance of zinc oxide. Figure 3 to Figure 5 It can be seen that the particle size of selenium nanoparticles overlaps with that of zinc oxide and neodymium-doped zinc oxide. Figure 1 It can be seen that after modification of selenium nanoparticles, there is obvious agglomeration; Figure 2 It can be seen that the selenium nanoparticles are better dispersed on the surface of zinc oxide after neodymium improves zinc oxide.
[0073] The antibacterial nonwoven fabrics prepared in the examples and comparative examples were tested for antibacterial properties according to the standard GB / T20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method", and the antibacterial properties were tested again after 50 standard washes; at the same time, the nonwoven fabric samples were cut into circular samples with a diameter of 125 mm according to the standard GB / T 21196.2-2007 "Determination of abrasion resistance of textiles by Martindale method Part 3: Determination of mass loss", and a 250g weight was selected, the running speed was 60rpm, and the friction was performed for 2 minutes to test the antibacterial properties after friction. Among them, the tested bacteria species was Staphylococcus aureus, and the deposit number was ATCC6538. These results are shown in Table 1.
[0074] Table 1 Antibacterial performance results
[0075]
[0076] From the results in Table 1, it can be seen that the antibacterial nonwoven fabric of Example 2 of the present invention has significantly better antibacterial properties, water washing resistance and anti-friction properties. This is because the introduction of selenium nanoparticles wraps zinc oxide to make it more stable, and the introduction of selenium also increases the binding sites between zinc oxide and bacteria, making it easier for bacteria to be enriched and promoting contact with bacteria. At the same time, the introduction of neodymium improves the dispersibility of zinc oxide, so that selenium nanoparticles with similar particle sizes form fewer agglomeration structures on the surface of zinc oxide, which allows it to maintain a high antibacterial property after multiple washings and frictions.
[0077] The antibacterial nonwoven fabrics prepared in the examples and comparative examples were tested for their ultraviolet protection factor (UPF) in accordance with the standard GB / T18830-2009 "Evaluation of the ultraviolet protection performance of textiles". It is generally believed that the larger the UPF value, the better the anti-ultraviolet performance of the fabric. The UPF value results are shown in Table 2.
[0078] Table 2 UPF value results
[0079]
[0080]
[0081] From the test results in Table 2, it can be seen that the fabric of the embodiment has better anti-ultraviolet performance, which is due to the introduction of selenium nanoparticles. The improvement of Example 2 relative to Example 1 is derived from the enhanced dispersion performance of zinc oxide. Example 2 has the best anti-ultraviolet performance, which is because the introduction of neodymium enhances the dispersion of zinc oxide and better modifies the selenium nanoparticles, synergistically improving the anti-ultraviolet performance of the fabric.
[0082] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An antibacterial nonwoven fabric, characterized in that: The composition comprises 100 to 120 parts of polypropylene, 10 to 15 parts of antibacterial agent, and 2 to 10 parts of compatibilizer in parts by weight; Wherein, the antibacterial agent is selenium-modified zinc oxide or selenium-modified neodymium-doped zinc oxide; The preparation method of selenium-modified zinc oxide comprises, in parts by weight, Mix 5 to 10 parts of a water-soluble zinc salt, 2 to 5 parts of a regulating agent, and 30 to 60 parts of a first solvent, and then heat and stir to react to obtain zinc oxide; Dispersing 5 to 10 parts of zinc oxide and 1 to 3 parts of selenium nanoparticles in 50 to 100 parts of a second solvent, and combining the selenium nanoparticles on the surface of the zinc oxide under stirring to obtain selenium-modified zinc oxide; The preparation method of selenium-modified neodymium-doped zinc oxide comprises, in parts by weight, 5 to 10 parts of a water-soluble zinc salt, 0.5 to 1.5 parts of a water-soluble neodymium salt, 2 to 5 parts of a regulating agent, and 30 to 60 parts of a first solvent are mixed, and then heated and stirred to react to obtain neodymium-doped zinc oxide; Dispersing 5 to 10 parts of neodymium-doped zinc oxide and 1 to 3 parts of selenium nanoparticles in 50 to 100 parts of a second solvent, and combining the selenium nanoparticles on the surface of zinc oxide under stirring to obtain selenium-modified zinc oxide; The regulating agent is oxalic acid or hexamethylenetetramine.
2. The antibacterial nonwoven fabric according to claim 1, characterized in that: The first solvent is at least one of ethanol, methanol, propanol, isopropanol, glycerol, and ethylene glycol; The second solvent is an ethanol aqueous solution with a volume fraction of 50% to 70%; The heating raises the temperature to 60-80°C.
3. The antibacterial nonwoven fabric according to claim 1, characterized in that: The preparation method of the selenium nanoparticles comprises, in parts by weight, The water-soluble selenite, the reducing agent and water are mixed and stirred for reaction, and selenium nanoparticles are collected.
4. The antibacterial nonwoven fabric according to claim 3, characterized in that: The concentrations of the water-soluble selenite and the reducing agent are 1-3 mmol / L and 0.5-1 mmol / L respectively.
5. The antibacterial nonwoven fabric according to claim 3, characterized in that: The reducing agent is at least one of chlorogenic acid, L-ascorbic acid and gallic acid.
6. The antibacterial nonwoven fabric according to claim 1, characterized in that: The compatibilizer is maleic anhydride grafted polypropylene.
7. A method for preparing the antibacterial nonwoven fabric according to claim 1, characterized in that: In parts by mass, it includes: Obtain 100-120 parts of polypropylene, 10-15 parts of antimicrobial agent, and 2-10 parts of compatibilizer; The polypropylene, antimicrobial agent and compatibilizer are mixed and granulated to obtain a blended masterbatch; The blended masterbatch is drawn, hot-pressed and shaped to obtain an antibacterial non-woven fabric.