Flexible graphite bipolar plate and preparation method thereof
By applying ultrasonic vibration during the molding process, the problem of low conductivity of flexible graphite bipolar plates is solved, and higher density and conductivity are achieved, improving the overall performance of the fuel cell.
Patent Information
- Application Number
- CN202410413008.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-08
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-04-08
AI Technical Summary
The flexible graphite bipolar plate has a low conductive performance due to the loose texture and softness of the expanded graphite, and there are many voids that affect its performance.
Ultrasonic vibration is applied during the molding process to discharge bubbles in the base material, improving the compactness and conductivity of the bipolar plate.
By reducing the gaps in the bipolar plate, its conductivity and density are significantly improved, and the overall performance of the fuel cell is enhanced.
Smart Images

Figure BDA0004779848760000041 
Figure BDA0004779848760000051 
Figure BDA0004779848760000052
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of fuel cell bipolar plates, and in particular to flexible graphite bipolar plates and a preparation method thereof. Background Art
[0002] Flexible graphite bipolar plate is an important component used in hydrogen fuel cells. It connects single cells, distributes reaction gases, collects current, dissipates heat and seals. The surface of the bipolar plate has flow channels, which are not only channels for water and gas in the fuel cell, but also the skeleton supporting the proton exchange membrane fuel cell. Its performance and cost directly affect the performance and cost of the fuel cell.
[0003] At present, the materials of fuel cell bipolar plates mainly include metal, graphite and composite materials. Among them, metal bipolar plates have the advantages of good conductivity, high strength and low cost, but also have disadvantages such as easy corrosion, poor air tightness and heavy weight. Graphite bipolar plates have the advantages of corrosion resistance, good air tightness and light weight, but also have disadvantages such as low strength, difficult molding and high cost. Composite bipolar plates are made by adding other materials to metal or graphite to improve its performance, but it also increases complexity and cost.
[0004] Flexible graphite bipolar plate is a special graphite bipolar plate, which is formed by mixing expanded graphite and resin and other materials and then molding. Flexible graphite, also known as worm graphite, is a graphite material that has been chemically oxidized and expanded at high temperature. It has the characteristics of loose texture, softness and toughness. Compared with traditional graphite bipolar plates, flexible graphite bipolar plates have the advantages of light weight, low cost and good air tightness. It is an ideal choice for fuel cell bipolar plates. However, it is precisely because of the loose texture and softness of expanded graphite that there are more gaps in the bipolar plate formed by it and the resin, which affects the conductivity of the bipolar plate. Summary of the invention
[0005] The technical solution of the present application mainly provides a flexible graphite bipolar plate and a preparation method thereof. Taking into account that the bipolar plate has many gaps due to the special material of expanded graphite, which affects the conductivity of the bipolar plate, ultrasonic vibration is applied during the molding and pressure relief curing stages to expel bubbles in the base material and the resin, thereby improving the conductivity of the bipolar plate.
[0006] To achieve the above objectives, this application provides the following technical solutions:
[0007] A method for preparing a flexible graphite bipolar plate comprises the following steps:
[0008] Mixing a main conductive filler, a first auxiliary conductive filler and a first thermoplastic resin to form a first preform;
[0009] The main conductive filler, the second auxiliary conductive filler and the second thermoplastic resin are mixed to form a second prefabricated material; wherein the ratio (mass ratio) of each component in the first / second prefabricated material is:
[0010] Main conductive filler 44-62 parts
[0011] 4 to 7 parts of the first / second auxiliary conductive filler
[0012] 30-48 parts of the first / second thermoplastic resin
[0013] Laying the first prefabricated material in the mold to form a first base layer; laying the second prefabricated material on the first base layer to form a second base layer; laying the first prefabricated material on the second base layer to form a third base layer;
[0014] The mold is heated and pressurized for molding, and ultrasonic vibration is applied to the mold during the molding process.
[0015] Preferably, the first auxiliary conductive filler is at least one of graphite particles, carbon black, carbon fibers and carbon nanotubes;
[0016] The first thermoplastic resin is (fluorinated) polyetheretherketone.
[0017] Preferably, the first auxiliary conductive filler is at least one of graphite particles and carbon black.
[0018] Preferably, the second auxiliary conductive filler is carbon fiber grafted with acrylamide;
[0019] The second thermoplastic resin is polyetheretherketone.
[0020] Preferably, the main conductive filler is expanded graphite.
[0021] Preferably, the mold is heated to 60-86° C. before laying the first base layer;
[0022] Among them, the ratio (mass ratio) of the first base layer, the second base layer and the third base layer is:
[0023] (0.8~1.2):(2.2~2.7):(0.8~1.2).
[0024] Preferably, the compression molding process comprises:
[0025] In the first stage, the applied pressure is 0.4-0.8MPa, and the ultrasonic vibration amplitude is 22-34μm (temperature, time); (exhaust + formation of transition layer)
[0026] In the second stage, a pressure of 2 to 2.7 MPa is applied, and the amplitude of ultrasonic vibration is 7 to 12 μm;
[0027] In the third stage, the applied pressure is 10-24 MPa and the ultrasonic vibration amplitude is 7-12 μm. (Ultrasound can reduce the viscosity of the resin and improve fluidity)
[0028] Preferably, the first prefabricated material is laid in a powder form in a mold and is scraped flat to form a first base layer;
[0029] The second prefabricated material is laid on the first base layer in powder form and is scraped flat to form a second base layer;
[0030] The first prefabricated material is laid on the second base layer in powder form and is scraped flat to form a third base layer.
[0031] Preferably, the first prefabricated material is cold pressed into a sheet and then laid in a mold to form a first base layer;
[0032] The second prefabricated material is cold pressed into a sheet and laid on the first base layer to form a second base layer;
[0033] The first prefabricated material is cold pressed into a sheet and then laid on the second base layer to form a third base layer.
[0034] Preferably, after the molding, the pressure is released;
[0035] The temperature rises to 350-420°C and is maintained for 30-50 minutes, while ultrasonic vibration is continuously applied to the mold. (Ultrasonic cavitation causes bubbles in the liquid to burst)
[0036] Another aspect of the present application further provides a flexible graphite bipolar plate, which is prepared based on the above-described method for preparing the flexible graphite bipolar plate.
[0037] Compared with the known public technologies, the technical solution provided by this application has the following beneficial effects:
[0038] In the technical solution of the present application, during the preparation process of the flexible bipolar plate, ultrasonic vibration is applied to the mold while heating and pressurizing during the compression molding stage, so that the gas in the base material in the mold can be discharged in time. At the same time, the increase in ultrasonic vibration is beneficial to improving the density of the base material; the gaps in the prepared bipolar plate are reduced, which is beneficial to improving the conductive performance of the bipolar plate. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in combination with the specific embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0040] The technical solution of the embodiment of the present application records a method for preparing a flexible graphite bipolar plate, which includes the following steps:
[0041] S10, mixing a main conductive filler, a first auxiliary conductive filler and a first thermoplastic resin to form a first preform.
[0042] Among them, the main conductive filler is expanded graphite, which is obtained by intercalation, water washing, drying and high-temperature expansion of natural flake graphite. The natural flake graphite used is purchased from Qingdao Baixing Graphite Co., Ltd.
[0043] The first auxiliary conductive filler is at least one of graphite particles, carbon black, carbon fibers and carbon nanotubes. More preferably, the first auxiliary conductive filler is at least one of graphite particles and carbon black.
[0044] The first thermoplastic resin is a fluorinated polyetheretherketone. In the embodiment of the present application, the fluorinated polyetheretherketone is obtained by modifying the polyetheretherketone resin before polymerization. Specifically:
[0045] Fluorinated polyetheretherketone is prepared by nucleophilic substitution using 4,4'-difluorobenzophenone and hexafluorobisphenol A as raw materials, cyclopentane as solvent, and anhydrous potassium carbonate as catalyst. The reaction equation is as follows:
[0046]
[0047] The product obtained above is washed and filtered with methanol and deionized water to obtain the first thermoplastic resin, which is then dried into powder for later use.
[0048] Then, 44 to 62 parts of expanded graphite, 4 to 7 parts of the first auxiliary conductive filler and 30 to 48 parts of the fluorinated polyetheretherketone prepared above are placed in a high-speed disperser for premixing; after sufficient mixing, the first prefabricated material is obtained.
[0049] S20, mixing the main conductive filler, the second auxiliary conductive filler and the second thermoplastic resin to form a second preform.
[0050] The preparation method of the main conductive filler has been explained above. In this application, the second auxiliary conductive filler is carbon fiber grafted with acrylamide, and the preparation method thereof is as follows:
[0051] Take p-phenylenediamine and place it in dichloromethane solvent; put 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) and 4-dimethylaminopyridine (DMAP) and stir and dissolve; finally add methacrylic acid and stir under nitrogen protection; after the reaction is completed, evaporate the dichloromethane solvent, then separate the product by column chromatography and dry it to obtain N-(4-amino-phenyl)-2-methyl-acrylamide. The reaction equation is as follows:
[0052]
[0053] Afterwards, the synthesized N-(4-amino-phenyl)-2-methyl-acrylamide (APMA) is grafted onto the carbon fiber surface; the reaction mode is as follows:
[0054]
[0055] Among them, CFs is carbon fiber washed with acetone;
[0056] COOH-CFs are carbon fibers that are functionalized by treating CFs with mixed acid and grafting carboxyl groups;
[0057] APMA-CFs are carbon fibers grafted with N-(4-amino-phenyl)-2-methyl-acrylamide.
[0058] The ratio of each powder (mass ratio) in the above preparation process is:
[0059] p-Phenylenediamine (4-6): EDC (9-11): DMAP (1-1.2): Methacrylic acid (4-5).
[0060] The p-phenylenediamine, EDC, DMAP, methacrylic acid and auxiliary reagents used above were purchased from Beijing Chemical Plant and were of chemically pure quality.
[0061] The surface of the carbon fiber grafted with N-(4-amino-phenyl)-2-methyl-acrylamide contains a large number of branched functional groups, so that the interface bonding strength is higher during the bonding process with the second thermoplastic resin.
[0062] The product obtained above is washed with deionized water and filtered to obtain the second auxiliary conductive filler, which is dried and set aside.
[0063] The second thermoplastic resin is polyetheretherketone, and its chemical structure is:
[0064]
[0065] Then, 44 to 62 parts of expanded graphite, 4 to 7 parts of the second auxiliary conductive filler and 30 to 48 parts of polyetheretherketone are taken and placed in a high-speed disperser for premixing; after sufficient mixing, the second prefabricated material is obtained.
[0066] S30, laying the prepared first prefabricated material and the second prefabricated material in a mold for compression molding.
[0067] This step is specifically performed in the following manner:
[0068] S32, laying the first prefabricated material in the mold to form a first base layer; wherein, the first prefabricated material can be the powdered mixture prepared in step S10. When the first prefabricated material is a powdered mixture, a metal scraper is required to flatten the top of the mixture after laying it in the mold; in some embodiments, the first prefabricated material is cold-pressed into a sheet and placed directly in the mold to form the first base layer.
[0069] S34, laying the second prefabricated material on top of the first base layer to form a second base layer; wherein, the second prefabricated material can be the powdered mixture prepared in step S20. When the second prefabricated material is a powdered mixture, after laying the mixture on the first base layer, it is necessary to use a metal scraper to scrape the top thereof flat; in some embodiments, the second prefabricated material is cold-pressed into a sheet and placed directly on the first base layer to form the second base layer.
[0070] S36, laying the first prefabricated material on top of the second base layer to form a third base layer; wherein the first prefabricated material in this step is the same as the first prefabricated material in step S32, and the first base material used in this step can also be in powder form or in sheet form after cold pressing. When it is in powder form, it is necessary to scrape the top end thereof flat to form the third base layer; when it is in sheet form, it can be directly placed on the second base layer to form the third base layer.
[0071] S38, applying temperature and pressure to the mold to shape the base material therein, and applying ultrasonic vibration to the mold during the molding process. The application of ultrasonic vibration allows the gas in the mold to be discharged in time, effectively reducing the porosity of the obtained graphite bipolar plate and improving its electrical conductivity; at the same time, the application of ultrasonic vibration can also effectively compact the base material in the mold and improve the density of the bipolar plate.
[0072] The bipolar plate prepared by the above method is a "sandwich" structure in which the surface is mainly the first prefabricated material and the middle is mainly the second prefabricated material. In the first prefabricated material and the second prefabricated material, expanded graphite is used as the main conductive filler, and is filled with corresponding first / second auxiliary conductive fillers. The first / second auxiliary conductive fillers are different in size and shape from the expanded graphite, and are mixed in the expanded graphite to increase the conductive path, thereby improving the conductive performance of the bipolar plate.
[0073] During actual use, in addition to being conductive, the bipolar plate also needs to promptly discharge the water generated during the operation of the fuel cell, and this process is mainly based on the channels on the surface of the bipolar plate. If water penetrates into the bipolar plate while flowing through the bipolar plate, it will affect the performance of the bipolar plate. Therefore, in an embodiment of the present application, the resin in the first prefabricated material on the surface of the bipolar plate is fluorinated polyetheretherketone, and hydrophobic fluorine atoms are introduced into the polyetheretherketone, so that its hydrophobic performance is better than that of polyetheretherketone, thereby ensuring the drainage performance of the bipolar plate.
[0074] In some embodiments, before laying the first base layer in step S32, the method further includes:
[0075] Step S31, heating the mold to 60-86° C. before laying the first base layer.
[0076] The purpose of preheating the mold is to improve the filling property and fluidity of the first substrate and / or the third substrate during the molding process so that they can better fit the shape of the mold to form channels on the surface of the bipolar plate.
[0077] During the bipolar plate compression molding process in step S30, the mass ratio of each base material is: first base material (0.8-1.2): second base material (2.2-2.7): third base material (0.8-1.2).
[0078] That is, in the embodiment of the present application, the mass of the second base layer located in the middle is approximately 1 / 2 of the mass of the entire base material. Since the auxiliary conductive filler in the second base layer is carbon fiber grafted with acrylamide, it has a strong bonding ability with the resin, thereby ensuring the overall strength of the bipolar plate.
[0079] In a better solution, the compression molding process of step S38 includes the following stages:
[0080] Step S381, the first stage, the applied pressure is 0.4-0.8MPa, the ultrasonic vibration amplitude is 22-34μm, and the duration is 30min. The temperature of the mold in this stage can be the same as the mold temperature in the preheating stage, that is, the temperature can be maintained at 60-86℃.
[0081] During this stage, an ultrasonic vibration with a large amplitude is applied, mainly to expel the gas between the base layers, effectively reduce the porosity of the molded product, and ensure the conductivity of the bipolar plate; at the same time, during this stage, the pressure is relatively small, and under the ultrasonic vibration, the powder particles between the base layers are mixed, so that the base material can be compacted while the molded product will not be stratified due to different raw materials; in addition, it can ensure that the powder will not be violently mixed, that is, the powder close to the molds on both sides is basically the first prefabricated powder, which can ensure the hydrophobicity of the surface of the bipolar plate.
[0082] Step S382, the second stage, the applied pressure is 2 to 2.7 MPa, the ultrasonic vibration amplitude is 7 to 12 μm, and the duration is about 15 minutes. Compared with the first stage, the pressure in this stage is slightly increased, and the amplitude of the ultrasonic vibration is reduced. This stage is no longer mainly for mixing raw materials. The purpose of ultrasonic vibration is mainly to exhaust gas to reduce porosity.
[0083] Step S383, the third stage, the applied pressure is 10-24 MPa, the ultrasonic vibration amplitude is 7-12 μm, and the duration is 2 hours. This stage is the main molding stage, the temperature rises to 220-260°C, and the purpose of applying ultrasound in this stage is to reduce the viscosity of the resin to ensure that the resin fully flows, so that it can better infiltrate the expanded graphite and reduce the formation of agglomerates during the molding process.
[0084] After the bipolar plate is molded, it is necessary to release the pressure for curing. In the embodiment of the present application, the temperature rises to 350-420° C. during the curing process and is maintained for 30-50 minutes, and ultrasonic vibration is continuously applied to the mold.
[0085] During this stage, the effect of ultrasound can, on the one hand, increase the fluidity of the resin, allowing the resin to better enter the voids of the expanded graphite; on the other hand, the application of ultrasound can cause the bubbles enclosed in the flowing resin to burst through its cavitation effect, further reducing the bubbles in the final product and ensuring the conductivity of the bipolar plate.
[0086] The frequency of the ultrasonic vibration involved in the above steps is 20 to 22 kHz.
[0087] The bipolar plate prepared through the above steps has good integrity, and has good electrical conductivity and drainage performance.
[0088] In the present application, a bipolar plate is prepared by the above method, and the density, planar conductivity, bending strength, gas tightness (gas permeability) and surface wetting angle of the prepared bipolar plate are measured.
[0089] Among them, the plane conductivity is measured by a four-probe resistance meter; the surface wetting angle is detected by a water drop using a contact angle meter, and the measurement methods of other properties are measured using the corresponding measurement methods in GBT 20042.6-2011.
[0090] Example 1
[0091] In this embodiment, in the first preformed powder, the main conductive filler is expanded graphite, the first auxiliary conductive filler is carbon black and graphite particles of equal mass, the carbon black is 774 mesh, the graphite particles are 800 mesh, and the first thermoplastic resin is fluorinated polyetheretherketone; wherein the number of parts (mass parts) of the main conductive filler is 44, the number of parts of the first auxiliary conductive filler is 4, and the number of parts of the first thermoplastic resin is 48.
[0092] In the second preformed powder, the main conductive filler is expanded graphite, the second auxiliary conductive filler is acrylamide grafted carbon fiber, and the second thermoplastic resin is polyetheretherketone; wherein the number of parts (mass parts) of the main conductive filler is 45, the number of parts of the second auxiliary conductive filler is 4, and the number of parts of the second thermoplastic resin is 42.
[0093] Lay each base layer in the mold according to the following mass ratio:
[0094] First base layer 1: second base layer 3: third base layer 1.
[0095] Then, compression molding, pressure relief curing, and demolding are performed in the manner described in step S30 above.
[0096] Example 2
[0097] In this embodiment, in the first preformed powder, the main conductive filler is expanded graphite, the first auxiliary conductive filler is carbon black and graphite particles of equal mass, the carbon black is 774 mesh, the graphite particles are 800 mesh, and the first thermoplastic resin is fluorinated polyetheretherketone; wherein the number of parts (mass parts) of the main conductive filler is 50 parts, the number of parts of the first auxiliary conductive filler is 6 parts, and the number of parts of the first thermoplastic resin is 30 parts.
[0098] In the second preformed powder, the main conductive filler is expanded graphite, the second auxiliary conductive filler is acrylamide grafted carbon fiber, and the second thermoplastic resin is polyetheretherketone; wherein the number of parts (mass parts) of the main conductive filler is 60 parts, the number of parts of the second auxiliary conductive filler is 7 parts, and the number of parts of the second thermoplastic resin is 30 parts.
[0099] Lay each base layer in the mold according to the following mass ratio:
[0100] First base layer 1: second base layer 3: third base layer 1.
[0101] Example 3
[0102] In this embodiment, in the first preformed powder, the main conductive filler is expanded graphite, the first auxiliary conductive filler is carbon black and graphite particles of equal mass, the carbon black is 774 mesh, the graphite particles are 800 mesh, and the first thermoplastic resin is fluorinated polyetheretherketone; wherein the number of parts (mass parts) of the main conductive filler is 62 parts, the number of parts of the first auxiliary conductive filler is 5 parts, and the number of parts of the first thermoplastic resin is 30 parts.
[0103] In the second preformed powder, the main conductive filler is expanded graphite, the second auxiliary conductive filler is acrylamide grafted carbon fiber, and the second thermoplastic resin is polyetheretherketone; wherein the number of parts (mass parts) of the main conductive filler is 60 parts, the number of parts of the second auxiliary conductive filler is 7 parts, and the number of parts of the second thermoplastic resin is 30 parts.
[0104] Lay each base layer in the mold according to the following mass ratio:
[0105] First base layer 1: second base layer 3: third base layer 1.
[0106] Example 4
[0107] The difference between this embodiment and embodiment 3 is that the first auxiliary conductive filler is different. In the embodiment of the present application, the first auxiliary conductive filler is selected from carbon fiber, carbon nanotube and carbon black of equal quality.
[0108] Comparative Example 1
[0109] The difference between this example and Example 3 is that in this example, ultrasonic vibration is not applied in each molding stage and pressure relief and curing stage.
[0110] Comparative Example 2
[0111] The difference between this example and Example 3 is that in this example, ultrasound is not applied in each compression molding stage, but ultrasound is applied in the pressure release and curing stage.
[0112] Comparative Example 3
[0113] The difference between this example and Example 3 is that, in this example, the first preformed powder is a mixture of a main conductive filler and a first thermoplastic resin, the main conductive filler is expanded graphite, the first thermoplastic resin is fluorinated polyetheretherketone, the number of parts (mass parts) of the main conductive filler is 67 parts, and the number of parts of the first thermoplastic resin is 30 parts; the second preformed powder is a mixture of a main conductive filler and a second thermoplastic resin, the main conductive filler is expanded graphite, the second thermoplastic resin is polyetheretherketone, the number of parts (mass parts) of the main conductive filler is 67 parts, and the number of parts of the second thermoplastic resin is 30 parts.
[0114] Comparative Example 4
[0115] The difference between this embodiment and Example 3 is that, in this embodiment, a second preformed powder is laid in a mold for compression molding.
[0116] The density, planar conductivity, flexural strength, gas tightness and surface wetting angle data of the bipolar plates prepared in the above-mentioned Examples 1-4 and Comparative Examples 1-4 are listed in the following table.
[0117] (In each case, 5 samples were prepared for data measurement, 3 valid samples were taken as a group, and the average value was calculated as the experimental result)
[0118]
[0119] From the above data, we can know that:
[0120] As for the density of the bipolar plate, analysis of Examples 1 to 4 shows that when the resin content in the bipolar plate is high, the density of the corresponding bipolar plate is relatively large, and the density of the bipolar plate also tends to increase with the increase of the resin content; analysis of Example 3 and Comparative Examples 1-2 shows that the application of ultrasonic vibration in the compression molding stage and the pressure relief and curing stage is beneficial to the increase of the density of the bipolar plate.
[0121] As for the planar conductivity of the bipolar plate, analysis of Examples 1 to 4 shows that when the content of expanded graphite and the corresponding auxiliary conductive filler in the bipolar plate is high, the planar conductivity of the corresponding bipolar plate is large, and the planar conductivity of the bipolar plate also shows an upward trend with the increase of expanded graphite and the corresponding auxiliary conductive filler; analysis of Example 3 and Comparative Examples 1-2 shows that the application of ultrasonic vibration in the compression molding stage and the pressure relief curing stage is beneficial to the increase of the planar conductivity of the bipolar plate; analysis of Example 3 and Comparative Example 3 shows that in the preparation process of the bipolar plate, the planar conductivity of the bipolar plate with the corresponding auxiliary conductive filler is better than the planar conductivity of the bipolar plate with only the main conductive filler, indicating that the increase of the corresponding auxiliary filler is beneficial to increase the conductive channel in the corresponding bipolar plate, thereby improving its conductivity.
[0122] As for the bending strength of the bipolar plate, analysis of Examples 1 to 4 shows that when the resin content in the bipolar plate is higher, the bending strength of the corresponding bipolar plate is larger, and the density of the bipolar plate also tends to increase with the increase of the resin content; analysis of Example 3 and Comparative Examples 1-2 shows that the application of ultrasonic vibration in the compression molding stage and the pressure relief curing stage is beneficial to the increase of the bending strength of the bipolar plate.
[0123] As for the gas permeability of the bipolar plate, analysis of Examples 1 to 4 shows that when the content of expanded graphite and the corresponding auxiliary conductive filler in the bipolar plate is high, the gas permeability of the corresponding bipolar plate increases, and the gas permeability of the bipolar plate also shows an upward trend with the increase of expanded graphite and the corresponding auxiliary conductive filler; analysis of Example 3 and Comparative Examples 1-2 shows that the application of ultrasonic vibration in the compression molding stage and the pressure relief curing stage is beneficial to reducing the gas permeability of the bipolar plate; analysis of Example 3 and Comparative Example 3 shows that the bipolar plate with expanded graphite as the conductive medium has a higher gas permeability than the bipolar plate with expanded graphite and the corresponding auxiliary conductive filler as the conductive medium, indicating that the presence of expanded graphite is conducive to the permeation of gas.
[0124] As for the surface wetting angle of the bipolar plate, analysis of Examples 1 to 4 shows that the increase in the resin content in the bipolar plate is beneficial to improving the wetting properties of the bipolar plate surface; analysis of Example 3 and Comparative Examples 1-2 shows that the application of ultrasonic vibration during the compression molding stage and the pressure relief curing stage is beneficial to improving the wetting properties of the bipolar plate surface, but this improvement effect is not obvious. Analysis of Example 3 and Comparative Example 4 shows that the surface wetting properties of the thermoplastic resin using fluorinated polyetheretherketone as the bipolar plate surface are better than those of the thermoplastic resin using polyetheretherketone as the bipolar plate surface.
[0125] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the protection scope of the technical solutions of the embodiments of the present application.
Claims
1. Preparation method of flexible graphite bipolar plate, It is characterized in that The steps include: Mixing a main conductive filler, a first auxiliary conductive filler and a first thermoplastic resin to form a first preform; The main conductive filler, the second auxiliary conductive filler and the second thermoplastic resin are mixed to form a second prefabricated material; wherein the ratio (mass ratio) of each component in the first / second prefabricated material is: Main conductive filler 44~62 parts; 4-7 parts of the first / second auxiliary conductive filler; 30-48 parts of the first / second thermoplastic resin; Laying the first prefabricated material in the mold to form a first base layer; laying the second prefabricated material on the first base layer to form a second base layer; laying the first prefabricated material on the second base layer to form a third base layer; The mold is heated and pressurized to form the product, and ultrasonic vibration is applied to the mold during the forming process; After the molding process, the pressure is released, the temperature is raised to 350-420°C, maintained for 30-50 minutes, and ultrasonic vibration is continuously applied to the mold; Wherein, the main conductive filler is expanded graphite; the first auxiliary conductive filler is at least one of graphite particles, carbon black, carbon fiber and carbon nanotubes; the first thermoplastic resin is fluorinated polyetheretherketone; the second auxiliary conductive filler is carbon fiber grafted with acrylamide; the second thermoplastic resin is polyetheretherketone; The compression molding process includes: In the first stage, the applied pressure was 0.4-0.8 MPa and the ultrasonic vibration amplitude was 22-34 μm; In the second stage, a pressure of 2 to 2.7 MPa was applied, and the ultrasonic vibration amplitude was 7 to 12 μm; In the third stage, the applied pressure is 10~24MPa and the ultrasonic vibration amplitude is 7~12μm.
2. The method for preparing the flexible graphite bipolar plate according to claim 1, It is characterized in that Heat the mold to 60~86℃ before laying the first base layer; Among them, the ratio (mass ratio) of the first base layer, the second base layer and the third base layer is: (0.8~1.2):(2.2~2.7):(0.8~1.2)。 3. The method for preparing the flexible graphite bipolar plate according to claim 1, It is characterized in that The first prefabricated material is laid in a powder form in a mold and is scraped flat to form a first base layer; The second prefabricated material is laid on the first base layer in powder form and is scraped flat to form a second base layer; The first prefabricated material is laid on the second base layer in powder form and is scraped flat to form a third base layer.
4. The method for preparing the flexible graphite bipolar plate according to claim 1, It is characterized in that The first prefabricated material is cold pressed into a sheet and then laid in a mold to form a first base layer; The second prefabricated material is cold pressed into a sheet and laid on the first base layer to form a second base layer; The first prefabricated material is cold pressed into a sheet and then laid on the second base layer to form a third base layer.
5. A flexible graphite bipolar plate prepared by the preparation method according to any one of claims 1 to 4.
Citation Information
Patent Citations
Resin filling type integrated bipolar plate and preparation method thereof
CN113540487A
Bipolar plate, method for production and use thereof
CN114730891A
Fuel cell bipolar plate with corrosion-resistant film layer and preparation method of fuel cell bipolar plate
CN115224295A
Preparation method of asymmetric hydrophilic and hydrophobic composite bipolar plate on surfaces of integrally formed cathode and anode plates
CN115692755A
Bipolar plate, fuel cell and method for producing bipolar plate
CN116057738A