A polymer sheet and continuous production method thereof

By adopting composite core layer structure and continuous production method in PP self-reinforced materials, the problems of high equipment investment and discontinuity in the prior art are solved, and the efficient continuous production and bonding effect of polymer sheets is achieved, which is suitable for Large-scale application.

CN118269443BActive Publication Date: 2024-12-03CHANGZHOU CARBON FRONT COMPOSITE MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410582073.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-11
Publication Date
2024-12-03
Estimated Expiration
2044-05-11

AI Technical Summary

Technical Problem

The molding method of existing PP self-reinforced materials is not conducive to large-scale mass production, with high equipment investment, large maintenance costs, discontinuous production, physical bubbles and internal layers, which affects use.

Method used

The composite core layer structure is adopted, including alternate stacked unstretched polypropylene films and bidirectional tensile polypropylene films, combined with automatic unwinding and continuous rolling technology, and the fabric layer improves the notch impact performance through the concave airway exhaust, Realize the continuous production of polymer sheets.

Benefits of technology

It greatly improves production efficiency, reduces bubble formation, and ensures the bonding effect between the inner layers of the composite core layer, which is suitable for mass production and application expansion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118269443B_ABST
    Figure CN118269443B_ABST
Patent Text Reader

Abstract

The invention discloses a polymer sheet and a continuous production method thereof. The polymer sheet comprises a composite core layer, the composite core layer comprises multiple layers of unstretched polypropylene films, and biaxially stretched polypropylene films are arranged between adjacent unstretched polypropylene films to form an alternating laminated structure; a fabric layer can also be arranged to improve the extremely poor notched impact performance of polypropylene; the surface of the unstretched polypropylene film is rough or an inner concave air channel is opened; a horizontally sequentially arranged unwinding roller group is introduced for automatic unwinding, combined with preheating, spot welding, and continuous rolling equipment, to achieve continuous production of the polymer sheet, greatly improving production efficiency; and effective exhaust can be achieved during the molding process, and the bonding effect between the inner layers of the composite core layer is effectively guaranteed by setting the thickness of the unstretched polypropylene film and the biaxially stretched polypropylene film and combining temperature control, which is greatly beneficial to batch production and application expansion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a polymer sheet and a continuous production method thereof. Background Art

[0002] PP self-reinforced materials greatly improve the excellent properties of conventional PP such as strength and stiffness by blending and modifying PP. Usually, the PP resin is melted into a film, extruded and drawn into fibers, and the fibers are woven into fiber fabrics. The film and fiber fabrics are then stacked and hot-pressed to form a PP self-reinforced board.

[0003] In the prior art, a flat-plate tablet press is usually used to perform repeated hot pressing layer by layer to achieve a multi-layer structure of compounding and compounding. This is an intermittent production mode with many complex processes, high equipment investment, high maintenance costs, and a large proportion of labor costs.

[0004] The use of a tablet press flat-plate hot pressing molding is not conducive to product exhaust. Air will remain between the films when they are stacked, and it is difficult to exhaust during hot pressing. In particular, the films will stick to each other after being heated, cutting off the path for the air to exhaust laterally. In addition, the thicker the product and the larger its length and width, the more serious the physical bubbles in the product after hot pressing will be.

[0005] In the process of repeated hot pressing, due to discontinuous production, the temperature needs to be repeatedly raised and lowered, which takes a considerable amount of time; after molding, internal stratification will occur, affecting use.

[0006] Therefore, for existing PP self-reinforced materials, the current molding method is not conducive to large-scale mass production, and also limits its promotion and application in various fields. Summary of the invention

[0007] In order to solve the above problems, the present invention provides a polymer sheet with a reasonable structure and a continuous production method thereof, thereby realizing the continuous production of the polymer sheet, greatly improving the production efficiency, and effectively ensuring the bonding effect between the inner layers of the composite core layer, which is greatly beneficial to mass production and application expansion.

[0008] The technical solution adopted by the present invention is as follows:

[0009] A polymer sheet material comprises a composite core layer, wherein the composite core layer comprises multiple layers of unstretched polypropylene films, and biaxially stretched polypropylene films are arranged between adjacent unstretched polypropylene films to form an alternating laminated structure; and also comprises a fabric layer; the unstretched polypropylene films have a rough surface or are provided with concave air channels.

[0010] As a further improvement of the above technical solution:

[0011] The unstretched polypropylene film and the biaxially stretched polypropylene film are both single-layer structures; the unstretched polypropylene film adopts random copolymer polypropylene, and the biaxially stretched polypropylene film adopts isotactic polypropylene. The melting point of the unstretched polypropylene film is lower than that of the biaxially stretched polypropylene film.

[0012] The unstretched polypropylene film is formed by a casting machine, and the thickness of the unstretched polypropylene film is 0.01-0.02mm; the biaxially stretched polypropylene film is extruded by an extruder, and the thickness of the biaxially stretched polypropylene film is 0.02-0.03mm.

[0013] The unstretched polypropylene film has a melting point of 155-160°C, a molecular weight of 60,000-80,000, and a melt flow rate of 5-8g / 10min; the biaxially stretched polypropylene film has an isotacticity of 95-99%, a melting point of 168-172°C, a molecular weight of 80,000-100,000, and a melt flow rate of 1-4g / 10min.

[0014] The concave air channel penetrates along the length direction of the unstretched polypropylene film.

[0015] At least one fabric layer is provided in the composite core layer, and polypropylene film is laminated on both sides of the fabric layer; the fabric layer is one of polypropylene fiber fabric, polypropylene coated polyester fiber fabric, and polypropylene coated nylon fiber fabric, and the fabric layer adopts a plain or twill weave structure. The fiber structure of the fabric layer is round yarn, with a specification of 500-2000D and a draft ratio of 6-8 times.

[0016] The composite core layer is a laminated structure of more than 30 layers, with an adhesive layer and an outer layer one being arranged in sequence on one side of the composite core layer, and an outer layer two being arranged on the other side of the composite core layer; the outer layer one is a biaxially stretched polyester film or a biaxially stretched nylon film, and the outer layer two 5 is a polyester knitted fabric.

[0017] A continuous production method for polymer sheets, the continuous production method comprising the following steps: automatic unwinding, pre-pressing, spot welding, preheating, rolling, and cutting;

[0018] In the automatic unwinding process, each layer of film is placed on each unwinding roller in the order of the upper and lower layers of the plate. The upper and lower unwinding rollers are symmetrically arranged to form a group of unwinding rollers. Multiple groups of unwinding rollers are arranged horizontally and orderly along the production direction. The film on the unwinding roller group at the front end of the production direction constitutes the outermost layer of the upper and lower surfaces of the plate, and the film on the adjacent unwinding roller group at the rear constitutes the second outer layer. By analogy, the film on the unwinding roller group at the rear end of the production direction constitutes the middle layer of the plate.

[0019] The number of composite core layers in the plate is more than 30;

[0020] The pre-pressing adopts the pre-pressing laminating rollers which are arranged symmetrically up and down. During the pre-pressing laminating, the air is exhausted through the concave air channel between the layers.

[0021] As a further improvement of the above technical solution:

[0022] The structure of a single unwinding roller group is as follows: it includes a reel placed on the coil symmetrically arranged up and down, and the coil lead-out end is equipped with an electrostatic roller brush; the upper and lower groups of coils are led out facing forward and attached, and a tensioning traction device is provided at the attachment point;

[0023] The number of the unwinding roller groups used is determined by the number of layers constituting the plate.

[0024] In the spot welding process, the spot welding equipment makes spots at intervals on both sides of the pre-pressed plate stack in the length direction to form welding spots; the welding spots are 3-5 mm away from the edges.

[0025] There are two preheating processes before and after, including preheating by preheating oven 1 connected to the rear end of the unwinding roller group, and preheating by preheating oven 2 after spot welding;

[0026] The rolling process uses a continuous rolling equipment, which includes two sets of upper and lower steel belts linearly fitted along the length direction. Four temperature and heat control zones are set along the length direction of the continuous rolling equipment, namely: preheating and prepressing zone, heating and pressurizing zone, heat preservation and pressure holding zone, and cooling and pressure holding zone. The highest temperature is reached in the heat preservation and pressure holding zone and is controlled at 168±1℃.

[0027] The temperature of the preheating and prepressing section is controlled at 120-150°C and the pressure is 0.5-1Mpa; the temperature of the heating and pressurizing section is 150-168°C and the pressure is 1-2Mpa; the temperature of the insulation and pressure section is 168±1°C and the pressure is 1-2Mpa; the temperature of the cooling and pressure section is 60-90°C and the pressure is 1-2Mpa. The total time for the stacked film material to flow through the four sections is 3-15min.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The invention has a compact and reasonable structure. The composite core layer is formed by alternately stacking unstretched polypropylene films and biaxially stretched polypropylene films. The surface of the unstretched polypropylene film is roughened or an inward concave air channel is provided. A fabric layer can also be provided to improve the extremely poor notched impact performance of polypropylene. The invention is combined with automatic unwinding and continuous rolling to realize continuous production of polymer sheets. In addition, the invention can effectively realize exhaust during the molding process, reduce or even avoid the formation of bubbles, greatly improve production efficiency, and facilitate batch production and application expansion.

[0030] The present invention also includes the following advantages:

[0031] The introduction of unwinding roller groups arranged in a horizontal sequence realizes the automatic unwinding of coils, which is convenient for spatial layout and can quickly adjust the number of unwinding roller groups put into production according to the change of the number of plate layers. It is easy to replace, replace, switch, and spare. It can be controlled separately to ensure the adjustment and uniformity of the unwinding tension. The horizontally arranged production form is particularly suitable for the automatic unwinding of large-diameter coils, which effectively helps to realize the continuous production of plates.

[0032] By setting the thickness of the unstretched polypropylene film and the biaxially stretched polypropylene film, both of which are single-layer structures, combined with temperature control, the bonding effect between the inner layers of the composite core layer is effectively guaranteed, effectively solving the existing delamination and detachment phenomenon;

[0033] The unique warp and weft weaving structure of the fabric can greatly improve the extremely poor notched impact strength of polypropylene; the unique hole structure of the fabric also provides a better gas exhaust channel, which further improves the exhaust capacity and facilitates exhaust. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a schematic diagram of the structure of the polymer sheet of the present invention.

[0035] Figure 2 It is a schematic diagram of the structure of the concave air channel on the unstretched polypropylene film of the present invention.

[0036] Figure 3 Another schematic diagram of the structure of the concave air channel on the unstretched polypropylene film of the present invention.

[0037] Figure 4 This is a diagram of the connection layout of the equipment for continuous production of the present invention.

[0038] Figure 5 It is a structural schematic diagram of the unwinding roller group of the present invention.

[0039] Figure 6 The figure is a schematic diagram of the arrangement of welding points on the plate of the present invention.

[0040] Among them: 1. Outer layer one; 2. Adhesive layer; 3. Functional layer; 4. Composite core layer; 5. Outer layer two;

[0041] 4a, unstretched polypropylene film; 4b, biaxially stretched polypropylene film; 4c, fabric layer; 4a1, concave air channel;

[0042] 10. Unwinding roller group; 20. Preheating drying tunnel 1; 30. Pre-pressing laminating roller; 40. Spot welding equipment; 50. Preheating drying tunnel 2; 60. Rubber roller group; 70. Continuous rolling equipment; 80. Cutting machine; 90. Plate;

[0043] 11. Tensioning and pulling device; 12. Electrostatic roller brush; 13. Coil;

[0044] 91. Solder point. DETAILED DESCRIPTION

[0045] The specific implementation of the present invention will be described below in conjunction with the accompanying drawings.

[0046] like Figure 1 As shown, a polymer sheet material of this embodiment includes a composite core layer 4, which includes a plurality of layers of unstretched polypropylene films 4a, and biaxially stretched polypropylene films 4b are arranged between adjacent unstretched polypropylene films 4a to form an alternating laminated structure; it also includes a fabric layer 4c; the surface of the unstretched polypropylene film 4a is rough or has a concave air channel 4a1.

[0047] In this embodiment, the composite core layer 4 is composed of unstretched polypropylene films 4a and biaxially stretched polypropylene films 4b alternately stacked. The surface of the unstretched polypropylene film 4a is roughened or an inner concave air channel 4a1 is provided, which is convenient for continuous production, especially continuous rolling, and can effectively achieve exhaust, reduce or even avoid the formation of bubbles, and effectively ensure the molding quality in continuous production.

[0048] In one embodiment, the unstretched polypropylene film 4a and the biaxially stretched polypropylene film 4b are both single-layer structures; the unstretched polypropylene film 4a is made of random copolymer polypropylene, and the biaxially stretched polypropylene film 4b is made of isotactic polypropylene, and the melting point of the unstretched polypropylene film 4a is lower than the melting point of the biaxially stretched polypropylene film 4b.

[0049] In this embodiment, by setting the thickness of the unstretched polypropylene film 4a and the biaxially stretched polypropylene film 4b, both of which are single-layer structures, combined with temperature control, the bonding effect between the inner layers of the composite core layer 4 is effectively guaranteed, and the existing delamination and detachment phenomenon is effectively solved.

[0050] At the preset control temperature, the unstretched polypropylene film 4a is completely melted, while the biaxially stretched polypropylene film 4b is in a slightly melted state on the surface, thereby effectively ensuring the interlayer adhesion and still presenting a multi-layer overlapping effect after bonding and forming, thereby ensuring the excellent performance of the composite core layer 4.

[0051] The unstretched polypropylene film 4a is formed by casting with a casting machine. The thickness of the unstretched polypropylene film 4a is 0.01-0.02mm, the tensile strength is>25Mpa in the transverse direction,>35Mpa in the longitudinal direction, and the haze is <5%.

[0052] The biaxially oriented polypropylene film 4b is extruded by an extruder. The thickness of the biaxially oriented polypropylene film 4b is 0.02-0.03mm, the tensile strength is transversely>120Mpa, longitudinally>200Mpa, the elongation at break is transversely<200%, longitudinally<80%, the haze is<4%, and the thermal shrinkage is<5%.

[0053] In this embodiment, by setting the thickness of the unstretched polypropylene film 4a and the biaxially stretched polypropylene film 4b, combined with the difference in their melting points, the two can be bonded to each other when stacked and heated, and can still maintain the stacked state, thereby ensuring the effect after stacking and forming; and, it effectively helps to ensure the overall tensile strength of the plate after the two are stacked and formed.

[0054] The setting of haze is used to ensure the gloss of the film, and then to ensure the gloss of the sheet after lamination; the setting of heat shrinkage rate is used to reduce the appearance of wrinkles in the film material.

[0055] The melting point of the unstretched polypropylene film 4a is 155-160°C, the molecular weight is 60,000-80,000, and the melt flow rate is 5-8g / 10min; the isotacticity of the biaxially stretched polypropylene film 4b is between 95-99%, the melting point is 168-172°C, the molecular weight is 80,000-100,000, and the melt flow rate is 1-4g / 10min.

[0056] By setting the molecular weight, the viscosity and fluidity of the two films in their respective molten states are effectively guaranteed, and they can be smoothly formed into films respectively, ensuring their forming properties, especially the bonding between the unstretched polypropylene film 4a in a completely molten state and the biaxially stretched polypropylene film 4b.

[0057] The isotacticity of the biaxially oriented polypropylene film 4b is set to be above 95%, which effectively guarantees its melting point; if the isotacticity is lower than 95%, the melting point will drop significantly.

[0058] In actual production, the temperature can be controlled between the melting point of the unstretched polypropylene film 4a and the melting point of the biaxially stretched polypropylene film 4b. For example, the temperature is set between 160-168°C, preferably around 168°C, so that the unstretched polypropylene film 4a is completely melted, while the biaxially stretched polypropylene film 4b is in a slightly melted state on the surface, effectively ensuring their mutual bonding effect.

[0059] In this embodiment, the biaxially oriented polypropylene film 4b adopts isotactic polypropylene, which is a high melting point polypropylene with a melting point of 168-172°C, an isotacticity requirement of 95-99%, a molecular weight of 80,000-100,000, a melt flow rate of 1-4g / 10min, and a tensile strength of >25Mpa; the preferred brand is EP3T56F series, but not limited to this brand.

[0060] In this embodiment, the unstretched polypropylene film 4a adopts random copolymer polypropylene, which is a low-melting-point polypropylene with a melting point of 155-160°C, a molecular weight of 60,000-80,000, a melt flow rate of 5-8g / 10min, and a tensile strength of >20Mpa. The preferred brand is RP370M, but not limited to this brand.

[0061] The concave air channel 4a1 runs through the length direction of the unstretched polypropylene film 4a; according to actual conditions, such as the thickness of the unstretched polypropylene film 4a, exhaust requirements and other factors, the concave air channel 4a1 can be set on one side or both sides of the unstretched polypropylene film 4a.

[0062] like Figure 2 In the embodiment shown, a plurality of straight concave air channels 4a1 may be provided on the surface of the unstretched polypropylene film 4a along the length direction, and during the rolling process, the interlayer air may be discharged outward along the concave air channels 4a1.

[0063] like Figure 3 In the embodiment shown, a plurality of fold line-shaped concave air channels 4a1 can be opened along the length direction on the surface of the unstretched polypropylene film 4a. During the rolling process, the interlayer air is not affected from being discharged outward along the concave air channels 4a1, and the structural strength of the unstretched polypropylene film 4a can be ensured.

[0064] The concave air channel 4a1 in this embodiment can be formed by cast-casting along with the unstretched polypropylene film 4a. The thickness of the concave air channel 4a1 is at the μm level and can be set according to the actual thickness and performance of the film. For example, it can be 1 / 5-1 / 3 relative to the thickness of the film, which can facilitate exhaust. During stacking, the concave air channel 4a1 will be filled and disappear due to the melting of the unstretched polypropylene film 4a due to heat.

[0065] In another embodiment, the surface of the unstretched polypropylene film 4a may be provided with a certain degree of roughness, and the interlayer air may be discharged during rolling through the connecting air passages formed by the roughness setting.

[0066] At least one fabric layer 4c is provided in the composite core layer 4, and polypropylene film 4a is adhered to both sides of the fabric layer 4c; the fabric layer 4c is one of polypropylene fiber fabric, polypropylene coated polyester fiber fabric, and polypropylene coated nylon fiber fabric, and polypropylene fiber fabric is preferred, because the interface bonding force will be better; the fabric layer 4c adopts a plain or twill weaving structure, and the fiber structure of the fabric layer 4c is round yarn, with a specification of 500-2000D and a draft ratio of 6-8 times; the fabric cloth has a bird's eye-shaped structural pore to facilitate exhaust.

[0067] In this embodiment, the unique warp and weft weaving structure of the fabric layer 4c can greatly improve the extremely poor notched impact strength of polypropylene, and can provide a better pore discharge channel to facilitate exhaust.

[0068] A fabric layer 4c is provided between at least one group of adjacent unstretched polypropylene films 4a and biaxially stretched polypropylene films 4b in the composite core layer 4; by providing the fabric layer 4c in the inner layer of the composite core layer 4, the notched impact performance of the board is improved.

[0069] In this embodiment, the fabric layer 4 c may be disposed at the center of the composite core layer 4 ; or the fabric layers 4 c may be disposed in orderly intervals in the composite core layer 4 . The specific number of layers may be determined according to the notch performance requirements of the plate 90 .

[0070] The composite core layer 4 is a laminated structure of more than 30 layers, with an adhesive layer 2 and an outer layer 1 being arranged in sequence on one side of the composite core layer 4, and an outer layer 2 5 being arranged on the other side of the composite core layer 4; the outer layer 1 is a biaxially stretched polyester film or a biaxially stretched nylon film, which has the functions of oil resistance, barrier, friction resistance and impact resistance; the outer layer 2 5 is a polyester knitted fabric, which is used for special needs, is soft and elastic, has a buffering and protective function, can improve the notch impact strength, and also has a certain degree of effect on exhaust.

[0071] In this embodiment, the adhesive layer 2 can be made of ethylene-vinyl acetate copolymer to play a bonding role and bond the outer layer 1 and the composite core layer 4.

[0072] In this embodiment, the functional layer 3 can be stacked and laid on the surface of the composite core layer 4 for use as special needs, such as film layers of different colors, antibacterial film layers, flame retardant film layers, etc.

[0073] A continuous production method of a polymer sheet in this embodiment includes the following steps: automatic unwinding, pre-pressing, spot welding, preheating, rolling, and cutting.

[0074] like Figure 4 As shown, the front and rear connection equipment used for the continuous production of polymer sheets includes: an unwinding roller group 10, a preheating drying tunnel 1 20, a pre-pressing laminating roller 30, a spot welding device 40, a preheating drying tunnel 2 50, a rubber roller group 60, a continuous rolling device 70, and a cutting machine 80.

[0075] like Figure 5 As shown, in the automatic unwinding process, each layer of the film is placed on each unwinding roller in sequence according to the upper and lower layer order of the plate 90, and the upper and lower unwinding rollers are symmetrically arranged to form a group of unwinding roller groups 10, and multiple groups of unwinding roller groups 10 are horizontally and orderly arranged along the production direction; the film on the unwinding roller group 10 located at the front end of the production direction constitutes the outermost layer of the upper and lower surfaces of the plate 90, and the film on the adjacent unwinding roller group 10 at the rear constitutes the second outer layer, and so on, the film on the unwinding roller group 10 located at the rear end of the production direction constitutes the middle layer of the plate 90.

[0076] In actual production, the two layers of film unwound from the rear unwinding roller group 10 are respectively attached to the inner sides of the two layers of film unwound from the front unwinding roller group 10 and attached; the two layers of film unwound from the unwinding roller group 10 farthest from the preheating drying tunnel 20 are located at the center of the laminated sheet 90.

[0077] like Figure 5As shown, after the film is unwound by multiple groups of unwinding roller groups 10, the stacking order of the plate 90 from top to bottom is 1->i->N, and is arranged counterclockwise to form a plate 90 with an N-layer stacking structure; taking a plate 90 with 30 layers of stacking as an example, that is, when N is 30, 15 groups of unwinding roller groups 10 are compactly arranged to unwind 30 layers of film, and in the frontmost group of unwinding roller groups 10 close to the preheating drying tunnel 20, the film unwound by the upper unwinding roller constitutes the upper first layer of the plate 90, and the film unwound by the lower unwinding roller constitutes the lower last layer of the plate 90, that is, the 30th layer, and the films unwound by the upper unwinding rollers of each group of unwinding roller groups 10 are the 1st layer, the 2nd layer, the 3rd layer, ..., the 15th layer from front to back, and the films unwound by the lower unwinding rollers of each group of unwinding roller groups 10 are the 16th layer, the 17th layer, ..., the 30th layer from back to front.

[0078] The number of the composite core layers 4 in the plate 90 is more than 30, and the number of the unwinding roller groups 10 put into production corresponds to the number of the layers of the plate 90 .

[0079] The pre-pressing adopts the pre-pressing laminating rollers 30 which are arranged symmetrically up and down. During the pre-pressing laminating, the air between the layers is exhausted backwards through the concave air channel 4a1.

[0080] In actual production, the spacing between the pre-pressing and laminating rollers 30 and the roller speed are dynamically adjustable. The spacing and roller speed can be adjusted according to the thickness of the product, so that when the product is pre-laminated, the air can be exhausted and wrinkles will not occur due to overpressure. The pre-pressing and laminating rollers 30 can be set to have an adjustable spacing of 0-80mm and an adjustable roller speed of 0-30r / min.

[0081] In this embodiment, a horizontally arranged unwinding roller group 10 is introduced to realize automatic unwinding of the coil, which is convenient for spatial layout and can quickly adjust the number of unwinding roller groups 10 put into production according to the change of the number of layers of the plate 90. It is convenient for installation, replacement, substitution, switching, and standby. It can be controlled individually to ensure the adjustment and uniformity of the unwinding tension. The horizontally arranged production form is particularly suitable for the automatic unwinding of large-diameter coils, which effectively helps to realize the continuous production of the plate 90.

[0082] The structure of a single unwinding roller group 10 is as follows: it includes rollers symmetrically arranged up and down for placing coils 13, and the lead-out ends of the coils 13 are equipped with electrostatic roller brushes 12; the upper and lower groups of coils 13 are joined and led out toward each other forward, and a tensioning traction device 11 is set at the joining position, and the film is pulled backward by the tensioning traction device 11; the tension of the tensioning traction device 11 is set to 20-80N.

[0083] The number of unwinding roller sets 10 used is determined by the number of layers constituting the plate 90 .

[0084] In this embodiment, the electrostatic roller brush 12 can be an ion wind rod or an ion wind curtain, which is usually used in conjunction with a high-voltage generator. The static electricity elimination time is 1-5s. The static electricity removal effect is achieved by evenly blowing out strong ion wind to eliminate the electrostatic adsorption of impurities, foreign matter, and dust on the membrane surface, reduce the probability of dirt, and at the same time reduce the adsorption force between membranes, which is beneficial to the discharge of air.

[0085] In the spot welding process, the spot welding device 40 makes spots at intervals on both sides of the pre-pressed plate stack in the length direction to form welding spots 91, such as Figure 6 As shown; the welding point 91 is 3-5mm away from the edge; through the setting of the welding point 91, the stacking positioning of the multi-layer film is achieved to prevent slippage between the film layers in the subsequent process.

[0086] In this embodiment, ultrasonic spot welding equipment can be used to generate mechanical vibrations inside the polymer using high-frequency ultrasonic energy, generate heat at the joint, melt the material, and form welds 91 when cooled. Ultrasonic spot welding equipment usually has automatic positioning and automatic deviation correction functions, programmable intermittent spot welding functions, high spot welding accuracy, high spot welding efficiency, and can greatly improve the deviation and slip problems that occur during the production process; the welding time is preferably 0.5-1s, and the welding time interval is preferably 5-20s, and welds 91 are formed at intervals of 3-5mm from the edges of the left and right sides of the plate 90.

[0087] In actual production, the energy of the spot welding device 40 is adjusted to 0-2000J. The more layers of the plate 90, the higher the energy. The working amplitude is between 10%-100%. The more layers of the plate 90, the larger the amplitude.

[0088] There are two preheating processes, including preheating by the preheating drying tunnel 1 20 connected to the rear end of the unwinding roller group 10, and preheating by the preheating drying tunnel 2 50 after spot welding;

[0089] The rolling process uses a continuous rolling device 70, which can be a double-steel belt continuous rolling device, including two sets of upper and lower steel belts linearly fitted along the length direction; four temperature and heat control zones are set along the length direction of the continuous rolling device 70, namely: preheating and prepressing section, heating and pressurizing section, heat preservation and pressure holding section, cooling and pressure holding section, and the highest temperature is reached in the heat preservation and pressure holding section, which is controlled at 168±1°C.

[0090] In this embodiment, the continuous rolling equipment can control the temperature and pressure of each section through a program, and make differentiated process selections for different products.

[0091] In actual production, it is preferred that the temperature of the preheating and prepressing sections is controlled at 120-150°C and the pressure is 0.5-1Mpa; the temperature of the heating and pressurizing section is 150-168°C and the pressure is 1-2Mpa; the temperature of the insulation and pressure section is 168±1°C and the pressure is 1-2Mpa; the temperature of the cooling and pressure section is 60-90°C and the pressure is 1-2Mpa. The total time for the stacked membrane material to flow through the four sections is 3-15 minutes.

[0092] In this embodiment, by controlling the temperature and pressure of the four sections, namely the preheating and prepressing section, the heating and pressurizing section, the heat preservation and pressure maintaining section, and the cooling and pressure maintaining section, the laminated film material reaches a surface softening state in the preheating and prepressing section, and pressurizing in this state is conducive to the discharge of interlayer gas; in the heating and pressurizing section, the unstretched polypropylene film melts, and the biaxially stretched polypropylene film does not melt, and in this state, the air flow path on the surface of the unstretched polypropylene film disappears; in the heat preservation and pressure maintaining section, the surface of the biaxially stretched polypropylene film slightly melts and mixes with the completely melted unstretched polypropylene; in the cooling and pressure maintaining section, the melted molecular chains on the surface of the biaxially stretched polypropylene are cooled and crystallized together with the melted molecular chains of the unstretched polypropylene, and the molecular chains are entangled with each other to form a firm whole.

[0093] The heat preservation and pressure keeping section has high requirements on temperature accuracy, requiring the temperature of the heating roller to be controlled at 168±1°C, which is beneficial to the performance control of the product and improves and ensures the stability of the product. At this temperature, the surface of the biaxially oriented polypropylene film 4b is slightly melted, its biaxially oriented structure remains unchanged, and its mechanical properties are not affected. The unstretched polypropylene film 4a is completely melted, and after being cooled by the cooling section, the cooling temperature is between 60-90°C, and it can be firmly combined into a whole.

[0094] At the front end of continuous production, the cutting machine 80 can perform operations such as burr cutting, automatic winding, and fixed-point cutting, and can also cut the continuous sheet 90 into a specified size.

[0095] Embodiment 1:

[0096] A continuous production method for a polymer sheet is:

[0097] a. Place 15 rolls of biaxially oriented polypropylene film 4b, 17 rolls of unoriented polypropylene film 4a, 1 roll of polypropylene fabric (fabric layer 4c), 1 roll of biaxially oriented polyester film (outer layer 1), 1 roll of ethylene-vinyl acetate copolymer (adhesive layer 2), and 1 roll of polyester knitted fabric (outer layer 5) on each unwinding roller in order of laying. After each roll of film passes through an electrostatic removal device and is pulled by a tension roller, it is stacked and laid in order, and the tension roller is set to 30N.

[0098] b. After being preheated in an oven, the sheets are passed to a pre-pressing laminating roller 30, and the air between the layers is discharged through the pre-pressing laminating roller 30.

[0099] c. Through automatic ultrasonic spot welding equipment, through gap automatic welding, the spot welding time is 0.5s and the interval is 10s.

[0100] d. After passing through the preheating drying tunnel 250 and the rubber roller, it reaches the double steel belt continuous roller pressing equipment, and the temperature of the preheating and prepressing section is set to 130℃, and the pressure is 0.5Mpa; the temperature of the heating and pressurizing section is 160℃, and the pressure is 1Mpa; the temperature of the insulation and pressure holding section is 168±1℃, and the pressure is 1.5Mpa; the temperature of the cooling and pressure holding section is 60℃, and the pressure is 1.5Mpa; the total time for flowing through the four sections is 5min.

[0101] e. The bonded product is passed through an automatic cutting machine and cut into specific sizes.

[0102] Embodiment 2:

[0103] A continuous production method for a polymer sheet is:

[0104] a. Place 30 rolls of biaxially oriented polypropylene film 4b, 32 rolls of unoriented polypropylene film 4a, 1 roll of polypropylene fabric (fabric layer 4c), 1 roll of biaxially oriented polyester film (outer layer 1), 1 roll of ethylene-vinyl acetate copolymer (adhesive layer 2), and 1 roll of polyester knitted fabric (outer layer 5) on the unwinding roller in order of plying. After each roll of film passes through an electrostatic removal device and is pulled by a tension roller, it is stacked and laid in order.

[0105] b. After being preheated in an oven, the sheets are passed to a pre-pressing laminating roller 30, and the air between the layers is discharged through the pre-pressing laminating roller 30.

[0106] c. Through automatic ultrasonic spot welding equipment, through gap automatic welding, the spot welding time is 0.8s and the interval is 10s.

[0107] d. After passing through the preheating drying tunnel 250 and the rubber roller, it reaches the double steel belt continuous roller pressing equipment, and the temperature of the preheating and prepressing section is set to 130℃, and the pressure is 0.5Mpa; the temperature of the heating and pressurizing section is 160℃, and the pressure is 1Mpa; the temperature of the heat preservation and pressure holding section is 168±1℃, and the pressure is 1.5Mpa; the temperature of the cooling and pressure holding section is 60℃, and the pressure is 1.5Mpa; the total time for flowing through the four sections is 8min.

[0108] e. The bonded product is passed through an automatic cutting machine and cut into specific sizes.

[0109] Embodiment 3:

[0110] a. Place 45 rolls of biaxially oriented polypropylene film 4b, 47 rolls of unoriented polypropylene film 4a, 1 roll of polypropylene fabric (fabric layer 4c), 1 roll of biaxially oriented polyester film (outer layer 1), 1 roll of ethylene-vinyl acetate copolymer (adhesive layer 2), and 1 roll of polyester knitted fabric (outer layer 5) on the unwinding roller in order of plying. After each roll of film passes through an electrostatic removal device and is pulled by a tension roller, it is stacked and laid in order.

[0111] b. After being preheated in an oven, the sheets are passed to a pre-pressing laminating roller 30, and the air between the layers is discharged through the pre-pressing laminating roller 30.

[0112] c. Through automatic ultrasonic spot welding equipment, through gap automatic welding, the spot welding time is 1s and the interval is 10s.

[0113] d. After passing through the preheating drying tunnel 250 and the rubber roller, it reaches the double steel belt continuous roller pressing equipment, and the temperature of the preheating and prepressing section is set to 130℃, and the pressure is 0.5Mpa; the temperature of the heating and pressurizing section is 160℃, and the pressure is 1Mpa; the temperature of the heat preservation and pressure holding section is 168±1℃, and the pressure is 1.5Mpa; the temperature of the cooling and pressure holding section is 60℃, and the pressure is 1.5Mpa; the total time for flowing through the four sections is 10min.

[0114] e. The bonded product is passed through an automatic cutting machine and cut into specific sizes.

[0115] Comparative Example 1:

[0116] Different from Example 1, the composite core layer 4 body (i.e., 15 rolls of biaxially oriented polypropylene film 4b, 17 rolls of unoriented polypropylene film 4a, and 1 roll of polypropylene fabric) was replaced with a common homopolymer polypropylene film, and the other materials and processes remained unchanged to prepare the sample of Comparative Example 1. Because the product lost the reinforcement layer and fabric, its own strength decreased significantly.

[0117] Comparative Example 2:

[0118] Different from Example 1, the polypropylene fiber fabric (fabric layer 4c) was eliminated, and the other materials and processes remained unchanged, thereby obtaining a comparative example 2 sample.

[0119] Comparative Example 3:

[0120] Different from Example 1, the main body of the composite core layer 4 is replaced with a sheet of 30% glass fiber reinforced polypropylene, and the other materials and processes remain unchanged, thereby obtaining a sample of Comparative Example 3.

[0121] Comparative Example 4:

[0122] Different from Example 1, the tension roller is set to 5N, and the other conditions remain unchanged.

[0123] Comparative Example 5:

[0124] Different from Example 1, the tension roller is set to 200N, and the other conditions remain unchanged.

[0125] Comparative Example 6:

[0126] Different from Example 1, the time for removing electrostatic adsorption is adjusted to 0s, that is, no electrostatic adsorption is performed, and other conditions remain unchanged.

[0127] Comparative Example 7:

[0128] Different from Example 1, the spot welding time is adjusted to 0s, that is, no spot welding is performed, and other conditions remain unchanged.

[0129] Comparative Example 8:

[0130] Different from Example 1, the temperature of the heat preservation and pressure preservation section in the processing conditions of the double steel belt continuous rolling equipment is set to 175±1° C. and the pressure is set to 1.5 MPa; the other conditions remain unchanged.

[0131] Comparative Example 9:

[0132] Different from Example 1, the temperature of the heat preservation and pressure preservation section in the processing conditions of the double steel belt continuous rolling equipment is set to 130° C. and the pressure is set to 0.5 MPa; the other conditions remain unchanged.

[0133] The properties of the samples prepared by the above-mentioned Examples 1-3 and Comparative Examples 1-9 are as follows:

[0134]

[0135]

[0136] It can be seen that by adopting the structure of the composite core layer 4 in the present application, and preferably with a total number of layers of more than 30 layers, the transverse tensile strength and longitudinal tensile strength of the board can be effectively improved and guaranteed. Combined with the setting of the fabric layer, the notch impact strength can be effectively guaranteed. The continuous production method in the present application is adopted to effectively ensure the flatness, wrinkle-free and bubble-free of the board.

[0137] The present invention realizes the continuous production of polymer sheets and can effectively realize exhaust during the molding process, reduce or even avoid the formation of bubbles, greatly improves production efficiency, and is conducive to mass production and application expansion.

[0138] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0139] The above description is an explanation of the present invention, not a limitation of the present invention. The scope of the present invention is defined in the claims. Any form of modification may be made within the scope of protection of the present invention.

Claims

1. A continuous production method for a polymer sheet, characterized in that: The polymer sheet comprises a composite core layer (4), wherein the composite core layer (4) comprises a plurality of unstretched polypropylene films (4a), and biaxially stretched polypropylene films (4b) are arranged between adjacent unstretched polypropylene films (4a) to form an alternating laminated structure; and further comprises a fabric layer (4c); and a concave air channel (4a1) is provided on the surface of the unstretched polypropylene film (4a); The unstretched polypropylene film (4a) has a melting point of 155-160°C, a molecular weight of 60,000-80,000, and a melt flow rate of 5-8 g / 10 min; the biaxially stretched polypropylene film (4b) has an isotacticity of 95-99%, a melting point of 168-172°C, a molecular weight of 80,000-100,000, and a melt flow rate of 1-4 g / 10 min; The composite core layer (4) has a laminated structure of more than 30 layers, one side of the composite core layer (4) is provided with an adhesive layer (2) and an outer layer 1 (1) in sequence, and the other side of the composite core layer (4) is provided with an outer layer 2 (5); the outer layer 1 (1) is a biaxially stretched polyester film or a biaxially stretched nylon film, and the outer layer 2 (5) is a polyester knitted fabric; The concave air channel (4a1) penetrates along the length direction of the unstretched polypropylene film (4a); The continuous production method includes the following processes: automatic unwinding, pre-pressing, spot welding, preheating, rolling, and cutting; In the automatic unwinding process, each layer of film is placed on each unwinding roller in the order of the upper and lower layers of the plate (90), and the upper and lower unwinding rollers are symmetrically arranged to form a group of unwinding roller groups (10), and multiple groups of unwinding roller groups (10) are arranged horizontally and orderly along the production direction; the film on the unwinding roller group (10) located at the front end of the production direction constitutes the outermost layer of the upper and lower surfaces of the plate (90), and the film on the adjacent unwinding roller group (10) at the rear constitutes the second outer layer, and so on, the film on the unwinding roller group (10) located at the rear end of the production direction constitutes the middle layer of the plate (90); In the spot welding process, the spot welding device (40) performs spot welding at intervals on both edges of the pre-pressed plate stack in the length direction to form welding spots (91); the welding spots (91) are 3-5 mm away from the edge; Two preheating steps are arranged before and after, including preheating by a preheating drying tunnel 1 (20) connected to the rear end of the unwinding roller group (10), and preheating by a preheating drying tunnel 2 (50) after spot welding; The rolling process uses a continuous rolling device (70), which includes two sets of upper and lower steel strips linearly attached to each other along the length direction; four temperature and heat control zones are arranged along the length direction of the continuous rolling device (70), which are: a preheating and prepressing zone, a heating and pressurizing zone, a heat preservation and pressure holding zone, and a cooling and pressure holding zone, wherein the highest temperature is reached in the heat preservation and pressure holding zone and is controlled at 168±1°C; Pre-pressing uses pre-pressing laminating rollers (30) that are symmetrically arranged up and down, and during pre-pressing laminating, air is exhausted between the layers via the concave air passages (4a1).

2. The continuous production method of a polymer sheet according to claim 1, characterized in that: The unstretched polypropylene film (4a) and the biaxially stretched polypropylene film (4b) are both single-layer structures; the unstretched polypropylene film (4a) is made of random copolymer polypropylene, and the biaxially stretched polypropylene film (4b) is made of isotactic polypropylene.

3. The continuous production method of a polymer sheet according to claim 2, characterized in that: An unstretched polypropylene film (4a) is formed by casting with a casting machine, and the thickness of the unstretched polypropylene film (4a) is 0.01-0.02 mm; a biaxially stretched polypropylene film (4b) is formed by extrusion with an extruder, and the thickness of the biaxially stretched polypropylene film (4b) is 0.02-0.03 mm.

4. The continuous production method of a polymer sheet according to claim 1, characterized in that: At least one fabric layer (4c) is provided inside the composite core layer (4), and unstretched polypropylene films (4a) are laminated on both sides of the fabric layer (4c); the fabric layer (4c) is one of a polypropylene fiber fabric, a polypropylene-coated polyester fiber fabric, and a polypropylene-coated nylon fiber fabric; the fabric layer (4c) adopts a plain or twill weave structure; the fiber structure of the fabric layer (4c) is round yarn, with a specification of 500-2000D and a draft ratio of 6-8 times.

5. The continuous production method of a polymer sheet according to claim 1, characterized in that: The structure of a single unwinding roller group (10) is as follows: it comprises a reel arranged symmetrically up and down and on which a coil (13) is placed, and the lead-out end of the coil (13) is provided with an electrostatic roller brush (12); the upper and lower groups of coils (13) are joined together and led out in a forward direction, and a tensioning and pulling device (11) is provided at the joining position; The number of unwinding roller groups (10) used is determined by the number of layers constituting the plate (90).

6. The continuous production method of a polymer sheet according to claim 1, characterized in that: The temperature of the preheating and prepressing section is controlled at 120-150°C and the pressure is 0.5-1Mpa; the temperature of the heating and pressurizing section is 150-168°C and the pressure is 1-2Mpa; the temperature of the insulation and pressure section is 168±1°C and the pressure is 1-2Mpa; the temperature of the cooling and pressure section is 60-90°C and the pressure is 1-2Mpa. The total time for the stacked film material to flow through the four sections is 3-15min.