Formaldehyde-free adhesive for artificial board and preparation method thereof

By adding glycidyl ether modified silicone oil and modified acrylic resin to the magnesium oxychloride adhesive, a chemical curing crosslinking network is formed, which solves the problems of low compressive strength and water absorption of oxychloride adhesive, and improves the bonding Strength and water resistance achieve higher compressive strength and wet bond strength.

CN118272016BActive Publication Date: 2024-11-19GUANGZHOU KOXIFEI E-COMMERCE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410630626.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-21
Publication Date
2024-11-19
Estimated Expiration
2044-05-21

AI Technical Summary

Technical Problem

Magnesium oxychloride adhesive has poor compressive strength in artificial boards, has a large water absorption rate, low bonding strength with wooden veneer substrates, and poor water resistance, resulting in limited practical application.

Method used

Using an aldehyde-free adhesive composed of magnesium oxide, magnesium chloride, glycidyl ether modified silicone oil and modified acrylic resin, a stable chemical curing crosslinking network is formed in magnesium oxychloride specimens to improve compressive strength and interface bonding. performance and reduce water absorption.

Benefits of technology

The compressive strength and interface bonding performance of oxy-chloride adhesive are significantly improved, the water absorption rate is reduced, the water resistance of the adhesive is enhanced, and the wet bonding strength is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
  • Figure SMS_5
    Figure SMS_5
Patent Text Reader

Abstract

The invention discloses a formaldehyde-free adhesive for artificial boards and a preparation method thereof, wherein the formaldehyde-free adhesive is composed of component A and component B; component A includes 100 parts by weight of magnesium oxide, 47-48 parts by weight of magnesium chloride, 0.6-1.4 parts by weight of water reducer, and 5-20 parts by weight of glycidyl ether modified silicone oil; component B is 15-50 parts by weight of modified acrylic resin; epoxy groups of the glycidyl ether modified silicone oil and multiple amino groups of the modified acrylic resin undergo cross-linking reaction, and a stable chemically cured cross-linked network is formed in the pores of the magnesium oxychloride specimen, which improves the compressive strength of the magnesium oxychloride adhesive and reduces water absorption. The glycidyl ether modified silicone oil and the emulsion of the modified acrylic resin react, and a chemically cured cross-linked network occurs at the interface of the wooden board, which significantly improves the interface bonding performance and bonding strength between the adhesive and the template.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesives, in particular to a formaldehyde-free adhesive for artificial boards and a preparation method thereof. Background Art

[0002] At present, almost all the board products sold in the artificial board market contain adhesives such as urea-formaldehyde resin and phenol-formaldehyde resin, which will release formaldehyde during long-term use. Formaldehyde is a colorless toxic gas, which is not easy to detect at low concentrations and can be easily masked by other odors; at high concentrations, it has a strong irritating and suffocating odor, which is irritating to the eyes and nose, seriously endangering human health. Therefore, the development of new formaldehyde-free adhesives and artificial boards is a research trend.

[0003] At present, the formaldehyde-free adhesives for panels mainly include magnesium oxychloride adhesive, water glass adhesive, mineral stone adhesive, etc. Among them, magnesium oxychloride adhesive does not contain formaldehyde and has the advantages of high strength, good fire resistance, and high wear resistance. It is widely used in the use of artificial panels. However, there is a large difference in polarity between inorganic adhesives such as magnesium oxychloride adhesive and wood veneer substrates, the interface bonding force is not good, and the bonding strength is low; and the water resistance of magnesium oxychloride adhesive is not good, and problems such as halogen frosting will occur, which significantly limits the practical application of magnesium oxychloride adhesive. Summary of the invention

[0004] The invention solves the problems that the magnesium oxychloride adhesive has poor compressive strength, high water absorption rate and low bonding strength with a wood substrate.

[0005] Technical solution: A formaldehyde-free adhesive consisting of component A and component B.

[0006] Component A includes 100 parts by weight of magnesium oxide, 47-48 parts by weight of magnesium chloride, 0.6-1.4 parts by weight of a water reducing agent, and 5-20 parts by weight of glycidyl ether modified silicone oil.

[0007] Component B is 15-50 parts by weight of modified acrylic resin.

[0008] The preparation method of the modified acrylic resin is as follows: add butyl acrylate, methyl methacrylate, polyamine polymerization monomer, and emulsifier into distilled water, stir and mix, then heat to 70-85° C., add initiator, stir and react for 20-60 minutes; then add butyl acrylate, methyl methacrylate, polyamine polymerization monomer, and initiator, continue to react for 2-3 hours, cool, and obtain the modified acrylic resin.

[0009] The structural formula of polyamine polymer monomer is: .

[0010] Furthermore, the ratio of the total mass of butyl acrylate, the total mass of methyl methacrylate, and the total mass of the polyamine polymerization monomer is 1:(0.3-0.4):(0.1-0.25).

[0011] Furthermore, the initiator is potassium persulfate and the emulsifier is OP-10.

[0012] Furthermore, the preparation method of the polyamine polymerization monomer is as follows: add 2,4-dichloro-6-allyloxy-1,3,5-triazine, 1,7-bis-BOC-1,4,7-triazaheptane, and N,N-diisopropylethylamine to any one of tetrahydrofuran and 1,4-dioxane solvents, heat to 45-55° C., react for 18-24 hours, distill the solution under reduced pressure, wash, add to dichloromethane, then add trifluoroacetic acid, react at room temperature for 3-4 hours, distill the solution under reduced pressure, wash, and dry to obtain the polyamine polymerization monomer.

[0013] Furthermore, the mass ratio of 2,4-dichloro-6-allyloxy-1,3,5-triazine, 1,7-bis-BOC-1,4,7-triazaheptane, and N,N-diisopropylethylamine is 1:(3.2-3.6):(1.2-1.7).

[0014] Furthermore, the preparation method of the glycidyl ether-modified silicone oil is: mix the glycidyl ether-modified silicone oil and the hydrogen-containing silicone oil in a mass ratio of (0.04-0.15):1, then add an isopropanol solution of chloroplatinic acid, heat to 85-90°C in a nitrogen atmosphere, react for 4-6 hours, and remove low-boiling substances by reduced pressure distillation to obtain the glycidyl ether-modified silicone oil.

[0015] Furthermore, the preparation method of the formaldehyde-free adhesive is as follows: the formaldehyde-free adhesive consists of component A and component B; modified acrylic resin is used as component B.

[0016] Add magnesium chloride into distilled water, stir to dissolve, then add magnesium oxide, water reducing agent, and glycidyl ether modified silicone oil, mix well, and obtain component A.

[0017] Furthermore, formaldehyde-free adhesives are used in artificial boards.

[0018] Technical effects of the present invention:

[0019] The present invention uses 2,4-dichloro-6-allyloxy-1,3,5-triazine and 1,7-bis-BOC-1,4,7-triazaheptane as reaction raw materials to prepare polyamine polymerization monomers, which are then mixed with butyl acrylate and methyl methacrylate to obtain modified acrylic resin.

[0020] The present invention uses magnesium chloride, magnesium oxide, water reducer, glycidyl ether modified silicone oil, and modified acrylic resin as the main formula of magnesium oxychloride formaldehyde-free adhesive, which does not contain formaldehyde and is nontoxic and environmentally friendly. The emulsion of glycidyl ether modified silicone oil and modified acrylic resin can be well penetrated into the pores of the magnesium oxychloride specimen, and the epoxy group of glycidyl ether modified silicone oil and multiple amino groups of modified acrylic resin undergo cross-linking reaction, and in the pores of the magnesium oxychloride specimen, a stable chemical curing cross-linking network is formed, which is conducive to reducing the pore structure of the magnesium oxychloride adhesive specimen, and when subjected to external force, the stable chemical curing cross-linking network can absorb and consume stress, and the specimen is prevented from producing microcracks, thereby improving the compressive strength of the magnesium oxychloride adhesive. And the chemical curing cross-linking network contains hydrophobic polysiloxane segments, which can improve the hydrophobicity inside the magnesium oxychloride specimen and further reduce water absorption.

[0021] The glycidyl ether modified silicone oil and the emulsion of modified acrylic resin added to the magnesium oxychloride formaldehyde-free adhesive of the present invention react to form a chemically cured cross-linked network at the interface of the wood board, thereby significantly improving the interface bonding performance and bonding strength between the adhesive and the template. In addition, the adhesive has good water resistance and exhibits high wet bonding strength. DETAILED DESCRIPTION

[0022] In order to make the contents of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.

[0023] Add 1.85g of cyanuric chloride to dichloromethane, stir to dissolve, add 15mL of 0.58g of allyl alcohol, 10mL of 50% sodium hydroxide solution, and 0.32g of tetrabutylammonium bromide, react at 10°C for 15min, add 20mL of distilled water, extract and separate, add anhydrous sodium sulfate to the dichloromethane organic phase to dry and remove water, filter and distill the filtrate under reduced pressure to obtain 2,4-dichloro-6-allyloxy-1,3,5-triazine. The structural formula is: .

[0024] Example 1.

[0025] Add 0.5 g 2,4-dichloro-6-allyloxy-1,3,5-triazine, 1.6 g 1,7-bis-BOC-1,4,7-triazaheptane (CAS registration number 117499-16-8), and 0.6 g N,N-diisopropylethylamine in a mass ratio to 15 mL tetrahydrofuran, heat to 55°C, react for 18 hours, distill the solution under reduced pressure, wash the product with methanol, add it to 15 mL dichloromethane, then add 5 mL trifluoroacetic acid, react at room temperature for 3 hours, distill the solution under reduced pressure, wash with saturated sodium bicarbonate solution and methanol in turn, and dry to obtain a polyamine polymerization monomer. The reaction formula is as follows:

[0026]

[0027] Add 3g of butyl acrylate, 0.8g of methyl methacrylate, 0.3g of polyamine polymerization monomer, and 0.03g of emulsifier OP-10 to 30mL of distilled water, stir and mix, then heat to 85°C, add 0.04g of initiator, and stir to react for 20min; then add 7g of butyl acrylate, 2.2g of methyl methacrylate, 0.7g of polyamine polymerization monomer, and 0.11g of initiator potassium persulfate, continue to react for 2h, cool, and obtain a modified acrylic resin.

[0028] Mix 2.4 g of glycidyl ether-modified silicone oil and 60 g of hydrogenated silicone oil (brand SM801), then add an isopropanol solution (0.15 mL) containing 2 mg of chloroplatinic acid, heat to 85 ° C in a nitrogen atmosphere, react for 5 hours, and remove low-boiling substances by reduced pressure distillation to obtain glycidyl ether-modified silicone oil.

[0029] The formaldehyde-free adhesive consists of component A and component B. 48 g of magnesium chloride is added to 115 mL of distilled water, stirred to dissolve, and then 100 g of magnesium oxide, 1.4 g of calcium lignin sulfonate, a water reducer, and 5 g of glycidyl ether-modified silicone oil are added and mixed to obtain component A. 15 g of modified acrylic resin is used as component B.

[0030] Example 2.

[0031] To 20 mL of tetrahydrofuran were added 0.5 g of 2,4-dichloro-6-allyloxy-1,3,5-triazine, 1.8 g of 1,7-bis-BOC-1,4,7-triazaheptane and 0.6 g of N,N-diisopropylethylamine in a mass ratio, heated to 50° C., reacted for 18 hours, and the solution was distilled under reduced pressure. The product was washed with methanol and added to 15 mL of dichloromethane, and then 6 mL of trifluoroacetic acid was added. The reaction was carried out at room temperature for 3 hours, and the solution was distilled under reduced pressure. The product was washed with saturated sodium bicarbonate solution and methanol in turn, and dried to obtain a polyamine polymerization monomer.

[0032] Add 3g butyl acrylate, 1g methyl methacrylate, 0.4g polyamine polymerization monomer, and 0.03g emulsifier OP-10 to 40mL distilled water, stir and mix, then heat to 70°C, add 0.04g initiator, and stir to react for 60min; then add 7g butyl acrylate, 2.5g methyl methacrylate, 1.4g polyamine polymerization monomer, and 0.12g initiator potassium persulfate, continue to react for 3h, cool, and obtain a modified acrylic resin.

[0033] Mix 6.3 g of glycidyl ether-modified silicone oil and 60 g of hydrogen-containing silicone oil, then add an isopropanol solution (0.15 mL) containing 2.6 mg of chloroplatinic acid, heat to 85°C in a nitrogen atmosphere, react for 6 hours, and remove low-boiling substances by reduced pressure distillation to obtain glycidyl ether-modified silicone oil.

[0034] The formaldehyde-free adhesive consists of component A and component B. 47 g of magnesium chloride is added to 115 mL of distilled water, stirred to dissolve, and then 100 g of magnesium oxide, 1 g of water reducer calcium lignin sulfonate, and 12 g of glycidyl ether modified silicone oil are added and mixed to obtain component A. 30 g of modified acrylic resin is used as component B.

[0035] Example 3.

[0036] To 10 mL of tetrahydrofuran were added 0.5 g of 2,4-dichloro-6-allyloxy-1,3,5-triazine, 1.6 g of 1,7-bis-BOC-1,4,7-triazaheptane and 0.85 g of N,N-diisopropylethylamine in a mass ratio, heated to 45°C, reacted for 24 hours, and the solution was distilled under reduced pressure. The product was washed with methanol and added to 15 mL of dichloromethane, and then 5 mL of trifluoroacetic acid was added. The reaction was carried out at room temperature for 5 hours, and the solution was distilled under reduced pressure. The product was washed with saturated sodium bicarbonate solution and methanol in turn, and dried to obtain a polyamine polymerization monomer.

[0037] Mix 9 g of glycidyl ether-modified silicone oil and 60 g of hydrogen-containing silicone oil, then add an isopropanol solution (0.15 mL) containing 2 mg of chloroplatinic acid, heat to 90°C in a nitrogen atmosphere, react for 4 hours, and remove low-boiling substances by reduced pressure distillation to obtain glycidyl ether-modified silicone oil.

[0038] Add 3g butyl acrylate, 1g methyl methacrylate, 0.6g polyamine polymerization monomer, and 0.05g emulsifier OP-10 to 40mL distilled water, stir and mix, then heat to 75°C, add 0.04g initiator, and stir to react for 60min; then add 7g butyl acrylate, 3g methyl methacrylate, 1.9g polyamine polymerization monomer, and 0.14g initiator potassium persulfate, continue to react for 3h, cool, and obtain a modified acrylic resin.

[0039] The formaldehyde-free adhesive consists of component A and component B. 48 g of magnesium chloride is added to 115 mL of distilled water, stirred to dissolve, and then 100 g of magnesium oxide, 1.4 g of calcium lignin sulfonate, a water reducer, and 20 g of glycidyl ether-modified silicone oil are added and mixed to obtain component A. 50 g of modified acrylic resin is used as component B.

[0040] Comparative example 1.

[0041] The difference between this comparative example and Example 1 is that the formaldehyde-free adhesive consists of component A, and component B modified acrylic resin is not added.

[0042] Comparative example 2.

[0043] The difference between this comparative example and Example 1 is that no glycidyl ether-modified silicone oil is added to component A of the formaldehyde-free adhesive.

[0044] The formaldehyde-free adhesive consists of component A and component B. 48 g of magnesium chloride is added to 115 mL of distilled water, stirred to dissolve, and then 100 g of magnesium oxide and 1.4 g of calcium lignin sulfonate, a water reducer, are added and mixed to obtain component A. 15 g of modified acrylic resin is used as component B.

[0045] Comparative example 3.

[0046] The difference between this comparative example and Example 1 is that glycidyl ether-modified silicone oil is not added to component A of the formaldehyde-free adhesive, but hydrogen-containing silicone oil is added.

[0047] The formaldehyde-free adhesive consists of component A and component B. 48 g of magnesium chloride is added to 115 mL of distilled water, stirred to dissolve, and then 100 g of magnesium oxide, 1.4 g of calcium lignin sulfonate, a water reducer, and 5 g of hydrogenated silicone oil are added and mixed to obtain component A. 15 g of modified acrylic resin is used as component B.

[0048] Pour component A and component B into the mold, stir and mix, mold at 50°C for 24 hours, demould, and then place in a constant temperature and humidity incubator with a humidity of 60% and room temperature for 28 days to make a magnesium oxychloride specimen.

[0049] According to the GB / T 17671-2021 method, the compressive strength of the magnesium oxychloride specimen was tested, and the loading rate of the tester was 5mm / min. The test was performed 5 times and the average value was taken.

[0050] The porosity of magnesium oxychloride specimens was tested using a high-performance fully automatic mercury intrusion instrument.

[0051] The compressive strength and porosity test results are shown in Table 1.

[0052] Table 1 Compressive strength and porosity test of magnesium oxychloride specimens.

[0053]

[0054] The compressive strength of the magnesium oxychloride specimens of Examples 1 to 3 reaches 74.69-94.24MPa. The porosity is 9.8-12.3%, which is because the emulsion of glycidyl ether-modified silicone oil and modified acrylic resin is added, which can penetrate into the pores of the magnesium oxychloride specimen well, and the epoxy groups of the glycidyl ether-modified silicone oil and the multiple amino groups of the modified acrylic resin undergo cross-linking reactions, forming a stable chemically cured cross-linked network in the pores of the magnesium oxychloride specimen, which is conducive to reducing the pore structure of the magnesium oxychloride specimen. At the same time, when subjected to external force, the stable chemically cured cross-linked network can absorb and consume stress, avoiding microcracks in the specimen, thereby improving the compressive strength of the magnesium oxychloride specimen.

[0055] The formaldehyde-free adhesive of Comparative Example 1 is composed of component A, and the modified acrylic resin of component B is not added. A stable chemically cured cross-linked network cannot be formed in the pores of the magnesium oxychloride specimen. The porosity of the specimen is large, and the compressive strength is low.

[0056] No glycidyl ether-modified silicone oil was added to component A of the formaldehyde-free adhesive of Comparative Example 2. A stable chemically cured cross-linked network could not be formed in the pores of the magnesium oxychloride specimen. The specimen had a large porosity and low compressive strength.

[0057] The hydrogenated silicone oil added to component A of the formaldehyde-free adhesive of comparative example 3 does not contain epoxy groups, and cannot undergo crosslinking reaction with the amino groups of the modified acrylic resin, and does not form a stable chemically cured crosslinking network in the pores of the magnesium oxychloride specimen. The specimen has a large porosity and low compressive strength.

[0058] Dry and weigh the magnesium oxychloride specimen, soak it in distilled water for 1-7 days, take out the magnesium oxychloride specimen, wipe off the surface moisture, weigh it, and calculate the water absorption rate. Water absorption rate = (m-m0) / m0×100%. m is the mass of the specimen after absorbing water, and m0 is the mass before absorbing water.

[0059] The water absorption test results are shown in Table 2.

[0060] Table 2 Water absorption test of magnesium oxychloride specimens.

[0061]

[0062] The 7-day water absorption of the magnesium oxychloride specimens of Examples 1 to 3 is only 0.865-1.540%. This is because the added glycidyl ether-modified silicone oil and the emulsion of modified acrylic resin can penetrate into the pores of the magnesium oxychloride specimen well to form a chemically cured cross-linked network, which is conducive to reducing the pore structure of the magnesium oxychloride specimen, and the chemically cured cross-linked network contains hydrophobic polysiloxane segments, which can improve the hydrophobicity inside the magnesium oxychloride specimen and further reduce the water absorption.

[0063] Pour component A and component B into the mold, stir and mix, and apply them on the surface of the poplar veneer. The amount of glue applied is 500g / m 3 , treated at 50℃ for 24h; assembled the poplar veneer, cold pressed at room temperature for 24h, with a pressure of 0.8MPa, and the obtained artificial board was cured at room temperature for 28 days. The dry and wet bonding strength of the artificial board was tested according to GB / T 17657-2013 method.

[0064] The test results of dry and wet bonding strength are shown in Table 3.

[0065] Table 3 Dry and wet bonding strength test of artificial boards.

[0066]

[0067] The dry bonding strength of the boards of Examples 1 to 3 reached 2.91-3.62MPa, and the wet bonding strength reached 2.02-2.59MPa. This is because the emulsion of glycidyl ether-modified silicone oil and modified acrylic resin added to the adhesive reacts to form a chemically cured cross-linked network at the interface of the wood board, which significantly improves the interface bonding performance and bonding strength between the adhesive and the template. In addition, the adhesive has good water resistance and exhibits high wet bonding strength.

[0068] The above general description of the invention involved in this application and the description of its specific embodiments should not be understood as limiting the technical solutions of the invention. Based on the disclosure of this application, those skilled in the art can add, reduce or combine the disclosed technical features in the above general description or / and embodiments without violating the constituent elements of the invention involved, to form other technical solutions within the protection scope of this application.

Claims

1. A formaldehyde-free adhesive, characterized in that: The formaldehyde-free adhesive consists of component A and component B; Component A includes 100 parts by weight of magnesium oxide, 47-48 parts by weight of magnesium chloride, 0.6-1.4 parts by weight of water reducer, and 5-20 parts by weight of glycidyl ether modified silicone oil; Component B is 15-50 parts by weight of modified acrylic resin; The preparation method of the modified acrylic resin is as follows: add butyl acrylate, methyl methacrylate, polyamine polymerization monomer, and emulsifier into distilled water, stir and mix, then heat to 70-85° C., add initiator, stir and react for 20-60 minutes; then add butyl acrylate, methyl methacrylate, polyamine polymerization monomer, and initiator, continue to react for 2-3 hours, cool, and obtain the modified acrylic resin; The structural formula of the polyamine polymerization monomer is: ; The ratio of the total mass of butyl acrylate, the total mass of methyl methacrylate, and the total mass of polyamine polymerization monomers is 1:(0.3-0.4):(0.1-0.25); The preparation method of the polyamine polymerization monomer is as follows: 2,4-dichloro-6-allyloxy-1,3,5-triazine, 1,7-bis-BOC-1,4,7-triazaheptane and N,N-diisopropylethylamine are added to a solvent, heated to 45-55° C., reacted for 18-24 hours, distilled the solution under reduced pressure, washed, added to dichloromethane, then added with trifluoroacetic acid, reacted at room temperature for 3-4 hours, distilled the solution under reduced pressure, washed, and dried to obtain the polyamine polymerization monomer.

2. The formaldehyde-free adhesive according to claim 1, characterized in that: The initiator is potassium persulfate and the emulsifier is OP-10.

3. The formaldehyde-free adhesive according to claim 1, characterized in that: The mass ratio of the 2,4-dichloro-6-allyloxy-1,3,5-triazine, 1,7-bis-BOC-1,4,7-triazaheptane and N,N-diisopropylethylamine is 1:(3.2-3.6):(1.2-1.7).

4. The formaldehyde-free adhesive according to claim 1, characterized in that: In the method for preparing the polyamine polymerization monomer, the solvent is any one of tetrahydrofuran and 1,4-dioxane.

5. A method for preparing the formaldehyde-free adhesive according to any one of claims 1 to 4, characterized in that: The formaldehyde-free adhesive consists of component A and component B; Using modified acrylic resin as component B; Add magnesium chloride into distilled water, stir to dissolve, then add magnesium oxide, water reducing agent, and glycidyl ether modified silicone oil, mix well, and obtain component A.

6. Use of the formaldehyde-free adhesive obtained by the preparation method as claimed in claim 5 in artificial boards.