A method for producing silver from copper anode mud gold separation slag

By simplifying the copper anode mud treatment process, canceling the silver electrolysis process, and using sodium sub-silver separation and silver oxide conversion technology to directly prepare high-purity silver powder, the problems of low silver qualification rate and large wastewater volume in the existing process have been solved, and the process has been simplified. and environmentally friendly production results.

CN118272664BActive Publication Date: 2024-10-01JIANGXI COPPER GUOXING (YANTAI) COPPER CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410711282.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-01
Estimated Expiration
2044-06-04

AI Technical Summary

Technical Problem

The extraction, separation and electrolytic refining process of silver in the existing copper anode slime treatment process is difficult to meet the complex composition requirements, resulting in a low silver qualification rate, long process flow, and large amounts of industrial sewage. In addition, the traditional process requires high-energy-consuming converter equipment and hazardous chemicals. products, leading to environmental pollution and high production costs.

Method used

The method of preparing silver from copper anode mud and gold slag eliminates the silver electrolysis process and uses sodium sub-sodium to separate silver, acidification treatment, silver oxide conversion, nitric acid dissolution and hydrochloric acid to generate silver chloride precipitate, which is then reduced with reduction under alkaline conditions. React with the reagent to directly obtain high-purity silver powder, simplify the process and recycle the nitric acid solution.

Benefits of technology

It realizes the direct preparation of first-grade silver ingots, improves the silver qualification rate, shortens the process flow, reduces the amount of waste water and energy consumption, avoids the use of high-energy-consuming equipment, reduces production costs, and reduces environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118272664B_ABST
    Figure CN118272664B_ABST
Patent Text Reader

Abstract

The invention discloses a method for producing silver from copper anode mud gold separation slag, wherein the gold separation slag is the gold separation slag obtained by filtering the copper anode mud after acid leaching for copper separation and chlorination for gold separation, and comprises the following steps: step 1, preparation of silver chloride precipitate: sodium sulfite silver separation is performed on the gold separation slag to obtain silver separation slag and silver separation liquid, and the silver separation liquid is acidified to obtain silver chloride precipitate; step 2, conversion and purification of silver chloride: silver chloride is used to prepare silver oxide under alkaline conditions, silver oxide is dissolved in nitric acid to obtain a dissolving liquid, and hydrochloric acid is added to the dissolving liquid to obtain silver chloride precipitate; step 3, preparation of silver: silver chloride is subjected to reduction reaction with a reducing agent under alkaline conditions to obtain elemental silver. Beneficial effects: the process is simple, the reaction conditions are mild, the silver electrolysis process is eliminated, the treatment process flow is shortened, the cost is saved, the qualified rate of silver meeting the national standard No. 1 is improved, and the sodium sulfite solution and nitric acid solution generated in the process can also be returned to the process flow for recycling, thereby reducing the amount of wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper anode mud smelting, and in particular to a method for producing silver from copper anode mud gold separation slag. Background Art

[0002] Most domestic enterprises use the Kaldo furnace process or rotary kiln process to process copper anode mud. The main process of the Kaldo furnace process is copper anode mud → pretreatment copper removal → Kaldo furnace smelting → gold-silver alloy → gold-silver refining; the rotary kiln process is mostly combined with the wet process, and the main process is copper anode mud → rotary kiln roasting and selenium evaporation → wet copper removal → wet gold separation and gold precipitation → wet silver separation and silver precipitation → gold-silver electrolytic refining. Although this semi-wet process can recover a variety of valuable metals in anode mud, the disadvantage is that the extraction and separation of silver and the electrolytic refining process are difficult to meet the treatment requirements of copper anode mud with increasingly complex components, resulting in a low pass rate of silver reaching the national standard No. 1 silver, a long process flow, and a large amount of industrial wastewater.

[0003] At present, in the production practice of using rotary kiln technology to treat copper anode mud, the wet silver separation process first adopted the method of sodium silver separation + formaldehyde reduction + silver electrolysis + casting. The impurity content of the crude silver powder obtained is relatively high, resulting in a low silver grade. It is directly cast into silver anode plates for electrolytic refining, which cannot meet the first-grade silver powder index, and even the second-grade silver ingots cannot be produced stably. Therefore, it is necessary to add a silver converter process to remove impurities from the crude silver powder and then cast it into silver anode plates for electrolytic refining. However, the converter is a high-energy consumption equipment and has serious environmental pollution. In addition to the above process, some companies use the process of sodium silver separation + acid precipitation of silver + oxidation removal of impurities + formaldehyde reduction + silver electrolysis + casting to produce first-grade silver ingots. Although it avoids adding a converter process, it needs to add an oxidizing impurity remover. Some companies even need to use expensive organic reagents such as EDTA for purification, which not only increases production costs, but also introduces new substances, resulting in difficult treatment of organic matter in wastewater, complex process flow, and the use of many types of hazardous chemicals. In addition, traditional silver separation technology cannot be separated from the silver electrolysis process, which also results in long-term occupation of precious metals and high energy consumption. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for producing silver from copper anode mud gold separation slag, which has simple process, mild reaction conditions, eliminates the silver electrolysis process, shortens the treatment process flow, saves costs, and improves the qualified rate of national standard No. 1 silver. At the same time, the sodium sulfite solution and nitric acid solution generated in the process can be returned to the process flow for recycling, thereby reducing the amount of waste water.

[0005] The object of the present invention is achieved by the following technical measures: a method for producing silver from copper anode mud gold separation slag, wherein the gold separation slag is the gold separation slag obtained by filtering the copper anode mud after acid leaching for copper separation and chlorination for gold separation, and the method comprises the following steps:

[0006] Step 1, preparation of silver chloride precipitate: separating gold-separating slag with sodium sulfate to obtain silver-separating slag and silver-separating liquid, and acidifying the silver-separating liquid to obtain silver chloride precipitate;

[0007] Step 2, conversion and purification of silver chloride: silver chloride is used to prepare silver oxide under alkaline conditions, nitric acid is used to dissolve the silver oxide to obtain a solution, and hydrochloric acid is added to the solution to obtain a silver chloride precipitate;

[0008] Step 3, preparation of silver: silver chloride is subjected to reduction reaction with a reducing agent under alkaline conditions to obtain elemental silver.

[0009] Furthermore, the sodium sulfite separation process in step 1 includes: adding 200-300 g / L of sodium sulfite solution to the gold separation slag, with a liquid-to-solid ratio of 8-12:1, a reaction temperature of 20-40°C, and stirring for 2-6 hours.

[0010] Furthermore, the acidification process in step 1 includes: adding sulfuric acid to the silver separation solution until the pH reaches 2-5 and then stopping the addition, the reaction temperature is 20-40° C., and stirring is performed for 0.5-1 h.

[0011] Furthermore, after the acidification treatment, the solid-liquid separation is performed to obtain a silver chloride precipitate and a silver chloride solution, and the pH of the silver chloride solution is adjusted to 7-8.5.

[0012] Furthermore, the process of preparing silver oxide from silver chloride under alkaline conditions in step 2 includes: mixing silver chloride and water to form a slurry, stirring and adding sodium hydroxide, and stopping the addition of sodium hydroxide when the molar amount of the added sodium hydroxide reaches 2-4 times the molar amount required for the reaction with the silver chloride.

[0013] Furthermore, the liquid-to-solid ratio of the slurry is 2-4:1.

[0014] Furthermore, the reaction temperature is 80-95°C, and the reaction time is 2-4h.

[0015] Furthermore, the process of dissolving silver oxide with nitric acid in step 2 includes: preparing silver oxide and water into a slurry, stirring and adding nitric acid, and stopping adding nitric acid when the pH reaches 3-6.

[0016] Furthermore, the liquid-solid ratio of the slurry is 2-4:1, the reaction temperature is room temperature, and the reaction time is 1-3h.

[0017] Furthermore, in step 3, silver chloride reacts with sodium hydroxide and formaldehyde to obtain elemental silver.

[0018] Compared with the prior art, the beneficial effects of the present invention are as follows: the present application proposes a method for producing silver from copper anode mud gold separation slag, cancels the silver electrolytic refining process, and directly prepares first-grade silver ingots in a full wet method short process, thereby solving the problems of poor raw material adaptability, low first-grade silver rate, high energy consumption of silver electrolysis process, long production cycle, and environmental pollution in the existing traditional copper anode mud treatment process. The present application converts silver chloride into silver oxide, dissolves the silver oxide with nitric acid, purifies silver, and then uses hydrochloric acid to generate silver chloride precipitation after the purified silver nitrate, thereby purifying silver chloride, and then directly reducing the silver chloride to obtain high-purity silver powder, thereby meeting the standard requirements of national standard No. 1 silver, and improving the qualified rate of national standard No. 1 silver. At the same time, the obtained nitric acid solution can be returned to the process for recycling, and the amount of wastewater is small.

[0019] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a processing process flow chart of the present invention. DETAILED DESCRIPTION

[0021] like Figure 1 As shown, a method for producing silver from copper anode mud gold separation slag, wherein the gold separation slag is obtained by filtering the copper anode mud after acid leaching and gold separation, and the silver mainly exists in the form of silver chloride in the gold separation slag. The method comprises the following steps:

[0022] Step 1, preparation of silver chloride precipitate: prepare a sodium sulfite solution with a concentration of 200-300g / L, add it to the gold separation slag according to a liquid-solid ratio of 8-12:1, control the reaction temperature to 20-40℃, stir for 2-6h, perform solid-liquid separation after the reaction is completed, perform sodium sulfite silver separation on the gold separation slag to obtain silver separation slag and silver separation liquid. The silver separation slag can be returned to the copper smelting system to enrich precious metals again. Add sulfuric acid to the silver separation liquid to react and generate silver chloride precipitate. When the pH reaches 2-5, stop adding sulfuric acid, the reaction temperature is 20-40℃, stir for 0.5-1h, acidify the silver separation liquid, perform solid-liquid separation after the reaction is completed, obtain silver chloride precipitate and precipitated silver chloride liquid, and adjust the pH of the precipitated silver chloride liquid to 7-8.5 and return to the sodium sulfite silver separation process for reuse. The main chemical reactions that occur are as follows:

[0023]

[0024] Step 2, conversion and purification of silver chloride: silver chloride is mixed with water to form a slurry, the liquid-solid ratio of the slurry is 2-4:1, sodium hydroxide is slowly added after stirring, and the addition of sodium hydroxide is stopped when the molar amount of sodium hydroxide added reaches 2-4 times the molar amount required for the reaction with silver chloride, the reaction temperature is 80-95°C, the reaction time is 2-4h, silver chloride reacts under alkaline conditions to generate silver oxide, and after the reaction is completed, the solid-liquid separation is performed to obtain silver oxide precipitate and silver oxide precipitation liquid, which can be used for ring collection flue gas treatment. The silver oxide precipitate and water are configured into a slurry, the liquid-solid ratio of the slurry is 2-4:1, nitric acid solution is slowly added after stirring, and the addition of nitric acid is stopped when the pH reaches 3-6, the reaction temperature is maintained at room temperature, the reaction time is 1-3h, nitric acid is used to dissolve the silver oxide, and after the reaction is completed, the solid-liquid separation is performed to obtain a dissolved solution and tailings, which can be returned to the copper smelting system. At room temperature, stir and slowly add hydrochloric acid to the solution until no white precipitate is precipitated, then stop adding hydrochloric acid. After the reaction is completed, perform solid-liquid separation to obtain purified silver chloride precipitate and nitric acid solution. The nitric acid solution can be returned to the process to dissolve silver oxide. The main chemical reactions that occur are as follows:

[0025]

[0026] Step 3, preparation of silver: silver chloride reacts with a reducing agent under alkaline conditions to obtain elemental silver. Specifically, silver chloride and water are prepared into a slurry with a liquid-solid ratio of 1-3:1, sodium hydroxide is added to the slurry to make the pH ≥ 13, and formaldehyde is slowly added. At room temperature, the reaction is carried out for 1-3 hours to detect the end point, that is, an appropriate amount of solution is taken as a sample, and an excess of formaldehyde is added to the sample. If no silver powder is generated, it is the end point. After the reaction reaches the end point, solid-liquid separation is carried out to obtain silver powder, which can be melted and cast into silver ingots. The silver ingots can meet the requirements of the national standard GB / T 4135-2002 and have a purity of 99.99%. The reducing liquid after solid-liquid separation can be sent to the sewage treatment process. The main chemical reactions that occur are as follows:

[0027]

[0028] Example 1

[0029] A batch of gold separation slag from the wet smelting process of copper anode mud was selected. After testing, its main components were as follows: Au 42g / t, Ag 180.7kg / t, Pb 25.4%.

[0030] The reagents used in the experiment are as follows: sodium sulfite, sulfuric acid, sodium hydroxide, nitric acid, hydrochloric acid and formaldehyde are industrial pure reagents, the mass percentage of sodium sulfite is not less than 93%, the mass percentage of sulfuric acid is not less than 98%, the mass percentage of sodium hydroxide is not less than 98%, the mass percentage of nitric acid is not less than 60%, the mass percentage of hydrochloric acid is not less than 31%, and the mass percentage of formaldehyde is not less than 37%.

[0031] Weigh 1000g (dry basis) of the above gold separation slag, add it into a sodium sulfite solution with a concentration of 250g / L at a liquid-solid ratio of 10:1, control the temperature at 30±5°C, stir for 4 hours, and perform solid-liquid separation to obtain silver separation slag and silver separation liquid, wherein the weight of the silver separation slag is 758g (dry basis). After testing, its main components include Au 51g / t, Ag 4.5kg / t, and Pb33.2%.

[0032] Sulfuric acid is added to the silver separation solution, and the temperature is controlled at 30±5°C. When the pH value is 3.5, the addition of sulfuric acid is stopped, and the stirring time is 1 hour. After the reaction is completed, the solid-liquid separation is performed to obtain a silver chloride precipitate and a precipitated silver chloride solution. NaOH is added to the precipitated silver chloride solution until the pH value is 7.5, and the sodium sulfite content is detected, and its concentration is adjusted so that it can be used as a sodium sulfite solution and returned to the sodium sulfite silver separation process.

[0033] Add industrial water to the silver chloride precipitate to a liquid-solid ratio of 2:1, stir to form a slurry, add 200g of NaOH, maintain the temperature at 90°C, react for 3 hours, separate the solid and the liquid, and obtain silver oxide and silver oxide precipitation solution, wherein the silver oxide precipitation solution is about 500mL and contains 0.015g / L of silver.

[0034] Silver oxide was added to industrial water to a liquid-solid ratio of 2:1, stirred to form a slurry, and nitric acid was slowly added at room temperature. When pH = 5, the addition of nitric acid was stopped. The reaction time was 2 hours, and the reaction was completed. Solid-liquid separation was performed to obtain tailings and silver nitrate solution, of which the tailings weighed 45g (dry basis). After testing, Ag was 335kg / t and gold was traced.

[0035] The silver nitrate solution was kept at room temperature, stirred and hydrochloric acid was slowly added until no white precipitate was precipitated from the solution, which was the end point of the reaction. The solid-liquid separation gave pure silver chloride and nitric acid solution, which was returned to the silver oxide dissolution process for continued use. Pure silver chloride was added to industrial water to a liquid-solid ratio of 1:1, stirred, and NaOH was added to a pH of ≥13, kept at room temperature, and formaldehyde was slowly added until no silver powder was precipitated, which was the end point of the reaction. Silver powder was obtained, and 161.6 g of silver sample was dried, slag-formed and cast.

[0036] Embodiment 2:

[0037] A batch of gold separation slag from the wet smelting process of copper anode mud was selected. After testing, its main components were as follows: Au 61g / t, Ag 123.6kg / t, Pb 24.3%.

[0038] The reagents used in the experiment are as follows: sodium sulfite, sulfuric acid, sodium hydroxide, nitric acid, hydrochloric acid and formaldehyde are industrial pure reagents, the mass percentage of sodium sulfite is not less than 93%, the mass percentage of sulfuric acid is not less than 98%, the mass percentage of sodium hydroxide is not less than 98%, the mass percentage of nitric acid is not less than 60%, the mass percentage of hydrochloric acid is not less than 31%, and the mass percentage of formaldehyde is not less than 37%.

[0039] Weigh 1000g (dry basis) of the above gold separation slag, add it into a sodium sulfite solution with a concentration of 210g / L at a liquid-solid ratio of 10:1, control the temperature at 25±5°C, stir for 2 hours, and perform solid-liquid separation to obtain silver separation slag and silver separation liquid, wherein the weight of the silver separation slag is 805.8g (dry basis). After testing, its main components include Au 71g / t, Ag 6.3kg / t, and Pb 30.1%.

[0040] Sulfuric acid is added to the silver separation solution, and the temperature is controlled at 25±5°C. When pH=2.5, the addition of sulfuric acid is stopped, and the stirring time is 0.5h. After the reaction is completed, the solid-liquid separation is performed to obtain silver chloride precipitate and precipitated silver chloride solution. NaOH is added to the precipitated silver chloride solution until pH=8, and the sodium sulfite content is detected, and its concentration is adjusted so that it can be used as a sodium sulfite solution and returned to the sodium sulfite silver separation process.

[0041] Add industrial water to the silver chloride precipitate to a liquid-to-solid ratio of 4:1, stir to form a slurry, add 180 g of NaOH, maintain the temperature at 95°C, react for 4 hours, separate the solid and the liquid, and obtain silver oxide and a silver oxide precipitation solution, wherein the silver oxide precipitation solution is about 1000 mL and contains 0.09 g / L of silver.

[0042] Silver oxide was added to industrial water to a liquid-solid ratio of 4:1, stirred to form a slurry, and nitric acid was slowly added at room temperature. When pH = 3, the addition of nitric acid was stopped. The reaction time was 3 hours, and the reaction was completed. The tailings and silver nitrate solution were obtained by solid-liquid separation. The tailings weighed 37g (dry basis). After testing, Ag was 284kg / t and gold was traced.

[0043] The silver nitrate solution was kept at room temperature, stirred and hydrochloric acid was slowly added until no white precipitate was precipitated from the solution, which was the end point of the reaction. The solid-liquid separation gave pure silver chloride and nitric acid solution, which was returned to the silver oxide dissolution process for continued use. Pure silver chloride was added to industrial water to a liquid-solid ratio of 3:1, stirred, and NaOH was added to a pH of ≥13, kept at room temperature, and formaldehyde was slowly added until silver powder no longer precipitated, which was the end point of the reaction. Silver powder was obtained, and 102.7 g of silver sample was dried, slag-formed and cast.

[0044] The chemical compositions of the silver samples of Example 1 and Example 2 are shown in the following table:

[0045]

[0046] Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for producing silver from copper anode mud gold separation slag, characterized in that: The gold separation slag is the gold separation slag obtained by filtering the copper anode mud after acid leaching for copper separation and chlorination for gold separation. The method comprises the following steps: Step 1, preparation of silver chloride precipitate: separating gold-separating slag with sodium sulfate to obtain silver-separating slag and silver-separating liquid, and acidifying the silver-separating liquid to obtain silver chloride precipitate; Step 2, conversion and purification of silver chloride: at a temperature of 80-95° C., silver chloride is mixed with water to form a slurry, stirred and silver oxide is prepared under alkaline conditions, nitric acid is used to dissolve the silver oxide to obtain a solution, hydrochloric acid is added to the solution to obtain a silver chloride precipitate and a nitric acid solution, and the nitric acid solution is returned to the process to dissolve the silver oxide; Step 3, preparation of silver: silver chloride reacts with a reducing agent under alkaline conditions to obtain elemental silver.

2. The method for producing silver from copper anode mud gold separation slag according to claim 1, characterized in that: The sodium sulfite separation process in step 1 comprises: adding 200-300 g / L of sodium sulfite solution to the gold separation slag, with a liquid-to-solid ratio of 8-12:1, a reaction temperature of 20-40° C., and stirring for 2-6 hours.

3. The method for producing silver from copper anode mud gold separation slag according to claim 1, characterized in that: The acidification process in step 1 includes: adding sulfuric acid to the silver separation solution until the pH reaches 2-5, stopping the addition, the reaction temperature is 20-40° C., and stirring for 0.5-1 h.

4. The method for producing silver from copper anode mud gold separation slag according to claim 3, characterized in that: After the acidification treatment, the solid-liquid separation is performed to obtain a silver chloride precipitate and a silver chloride solution, and the pH of the silver chloride solution is adjusted to 7-8.

5.

5. The method for producing silver from copper anode mud gold separation slag according to claim 1, characterized in that: The process of preparing silver oxide from silver chloride under alkaline conditions in step 2 comprises: mixing silver chloride and water to form a slurry, stirring and adding sodium hydroxide, and stopping adding sodium hydroxide when the molar amount of the added sodium hydroxide reaches 2-4 times the molar amount required for the reaction with the silver chloride.

6. The method for producing silver from copper anode mud gold separation slag according to claim 5, characterized in that: The liquid-to-solid ratio of the slurry is 2-4:

1.

7. The method for producing silver from copper anode mud gold separation slag according to claim 5, characterized in that: The reaction time is 2-4h.

8. The method for producing silver from copper anode mud gold separation slag according to claim 1, characterized in that: The process of dissolving silver oxide with nitric acid in step 2 includes: preparing silver oxide and water into slurry, stirring and adding nitric acid, and stopping adding nitric acid when the pH reaches 3-6.

9. The method for producing silver from copper anode mud gold separation slag according to claim 8, characterized in that: The liquid-to-solid ratio of the slurry is 2-4:1, the reaction temperature is room temperature, and the reaction time is 1-3 hours.

10. The method for producing silver from copper anode mud gold separation slag according to claim 1, characterized in that: In the step 3, silver chloride reacts with sodium hydroxide and formaldehyde to obtain elemental silver.

Citation Information

Patent Citations

  • Method for extracting silver from gold separating residues

    CN113528840A

  • Preparation of super pure metal silver

    CN1301874A

  • Process for treating liquid effluents containing chloride ions

    FR3124503A1

  • Method of recovering silver

    KR1020020094482A

  • Process for refining silver bullion with gold separation

    US20030154821A1