A method for preparing mineralized collagen based on dynamic cross-linking and the obtained mineralized collagen

By simulating the nonlinear process of natural bone through a dynamic cross-linking scheme, we successfully prepared biomimetic mineralized collagen with high mineralization that is close to the structure and properties of natural bone, solving the problem of inconsistent mechanical strength and multi-scale mineralized structure in the existing technology. , significantly improving the mechanical properties and enzymatic performance of bionic mineralized collagen.

CN118286511BActive Publication Date: 2024-10-15BEIJING UNIV OF TECH +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410520542.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-28
Publication Date
2024-10-15
Estimated Expiration
2044-04-28

AI Technical Summary

Technical Problem

It is difficult to achieve the preparation of biomimetic mineralized collagen composite materials in vitro that is consistent with the mechanical strength and multi-scale mineralization structure of natural bone, and the dynamic cross-linking process has not been effectively simulated.

Method used

A dynamic cross-linking scheme is adopted, by sequentially adding EDC, NHS and calcium chloride solution to the collagen solution to adjust the pH, and on this basis, adding diammonium hydrogen phosphate solution for cross-linking and mineralization, and simultaneously performing freezing treatment and vacuum freeze-drying. , simulating the nonlinear process of natural bone to prepare biomimetic mineralized collagen with high mineralization and high mechanical properties.

Benefits of technology

The microstructure of the prepared multi-scale mineralized collagen is highly coincident with that of natural bone, and its mechanical properties and enzymatic hydrolysis properties are significantly improved. The mechanical properties are closer to human bone tissue, which improves the development prospects of bionic mineralized collagen.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118286511B_ABST
    Figure CN118286511B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing mineralized collagen based on dynamic cross-linking and the obtained mineralized collagen, belonging to the technical field of biomedical materials. The method for preparing mineralized collagen based on dynamic cross-linking of the present invention comprises the following steps: adding EDC solution, NHS solution and calcium chloride solution to a collagen solution in sequence, stirring, adjusting pH, reacting for 6 to 9 hours, obtaining a reaction mixture one, adding diammonium hydrogen phosphate solution thereto, cross-linking and mineralizing, obtaining a reaction mixture two, freezing treatment, and then vacuum freeze drying to obtain mineralized collagen. The present invention uses a dynamic cross-linking scheme and simulates the nonlinear process of natural bone mineralization to make collagen combine with more inorganic minerals. On a micron scale, a biomimetic mineralized collagen with a higher degree of mineralization and a higher similarity to the body's mineralized collagen is prepared; on a macro scale, the biomimetic mineralized collagen has better mechanical properties and enzymatic hydrolysis properties; and provides technical support for the preparation of multi-scale biomimetic bone matrix materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomedical materials, and in particular relates to a method for preparing mineralized collagen based on dynamic cross-linking and the obtained mineralized collagen. Background Art

[0002] Bone tissue, as a typical hard tissue in the human body, is a composite structure composed of organic and inorganic substances, among which organic substances are mainly collagen and inorganic substances are mainly hydroxyapatite. Mineralized collagen composed of collagen and hydroxyapatite is the basic structural unit of bone tissue. Therefore, preparing biomimetic mineralized collagen by in vitro biomimetic mineralization is an important research method for developing clinical bone repair materials. However, the mechanical strength of biomimetic mineralized collagen composites is insufficient. Reasonable regulation of mineralization and formation of mineralized collagen in vitro that is consistent with the mechanical strength and multi-scale mineralized structure of natural bone is the focus and difficulty of current research.

[0003] In in vitro bionic mineralization, cross-linking is crucial for the in vitro formation of mineralized collagen that is consistent with the mechanical strength and multi-scale mineralized structure of natural bone. Studies have used different physical and chemical cross-linking methods to prepare collagen with a high degree of cross-linking for mineralization research. Studies have shown that the increase in the degree of collagen cross-linking can provide better mechanical and structural conditions for the deposition of hydroxyapatite, ultimately improving the mineralization capacity of collagen. However, these studies all cross-linked first and then mineralized, and cross-linking and mineralization were carried out separately. In the process of natural bone formation, the process of forming collagen fibrils and the process of collagen fiber mineralization are continuous and synchronous, that is, the dynamic cross-linking mineralization process. As a necessary factor in the process of bone formation, dynamic cross-linking can also affect the structure of bone and thus improve the mechanical properties. However, to date, in vitro bionic self-assembled mineralized collagen under the regulation of dynamic cross-linking has not been prepared. Summary of the invention

[0004] In order to solve the above technical problems, the present invention proposes a method for preparing mineralized collagen based on dynamic cross-linking and the obtained mineralized collagen. Through the dynamic cross-linking scheme and the simulation of the nonlinear process of natural bone mineralization, collagen is combined with more inorganic minerals. At the micron scale, a bionic mineralized collagen with a higher degree of mineralization and a higher similarity to the body's mineralized collagen is prepared; at the macroscopic scale, the bionic mineralized collagen has better mechanical properties and enzymatic hydrolysis properties; and technical support is provided for the preparation of multi-scale bionic bone matrix materials.

[0005] To achieve the above object, the present invention provides a method for preparing mineralized collagen based on dynamic cross-linking, comprising the following steps:

[0006] (1) Adding EDC solution, NHS solution and calcium chloride solution to the collagen solution in sequence, stirring, adjusting the pH, and reacting for 6 to 9 hours to obtain a reaction mixture 1;

[0007] (2) adding diammonium hydrogen phosphate solution to the reaction mixture 1 obtained in step (1), and crosslinking and mineralizing for 10 to 24 hours to obtain a reaction mixture 2;

[0008] (3) The reaction mixture obtained in step (2) is subjected to second freezing treatment and then vacuum freeze-dried to obtain mineralized collagen.

[0009] Preferably, the collagen solution in step (1) is a type I collagen solution, and the mass concentration of the type I collagen solution is 0.7-0.9%.

[0010] Preferably, in step (1), the mass concentration of the EDC solution is 1.2-5.2%, the mass concentration of the NHS solution is 0.3-1.3%, and the concentration of the calcium chloride solution is 8.78-8.98M.

[0011] Preferably, in step (1), the volume ratio of the collagen solution, EDC solution, NHS solution and calcium chloride solution is 1 to 3:1:1:1.

[0012] Preferably, the stirring speed in step (1) is 50 to 80 r / min.

[0013] Preferably, the solution for adjusting pH in step (1) is sodium hydroxide solution and / or potassium hydroxide solution.

[0014] Preferably, the concentration of the diammonium hydrogen phosphate solution in step (2) is 4.67-4.87 M, and the volume ratio of the diammonium hydrogen phosphate solution to the calcium chloride solution is 1:1.

[0015] Preferably, the temperature of the freezing treatment in step (3) is -15 to -25°C, and the time of the freezing treatment is 20 to 28 hours.

[0016] Preferably, the vacuum degree of the vacuum freeze-drying in step (3) is less than 6 Pa, the temperature of the vacuum freeze-drying is -55 to -85°C, and the time of the vacuum freeze-drying is 20 to 28 hours.

[0017] The invention also provides the mineralized collagen prepared by the preparation method.

[0018] Compared with the prior art, the present invention has the following advantages and technical effects:

[0019] The present invention prepares a hydrogel composite collagen scaffold, combines dynamic cross-linking during the mineralization process of the composite collagen scaffold, affects the transport and deposition of minerals to adjust the mechanical properties of mineralized collagen and optimize the internal structure of mineralized collagen. According to the nonlinear characteristics of natural bone growth trend, the natural bone cross-linking process and mineralization process are simulated, and the time for adding mineralizing liquid during dynamic cross-linking is determined to achieve cross-linking and mineralization at the same time, thereby achieving the effect of dynamic cross-linking. The multi-scale mineralized collagen prepared by the present invention has a microstructure that is highly consistent with natural bone, and has significantly improved mineral content and mechanical properties compared to mineralized collagen under non-dynamic cross-linking.

[0020] Compared with the traditional method of self-assembly collagen mineralization, the present invention fully considers the influence of dynamic cross-linking, mineral transport process and natural bone mineralization process in mineralization, constructs a bionic mineralization system regulated by dynamic cross-linking factors, better simulates the complex bone matrix mineralization process in natural bone, and prepares a bone matrix material that is more in line with the real bone structure. Dynamic cross-linking promotes collagen mineralization by promoting the infiltration of minerals into collagen and changing the mineral morphology on the surface of collagen, completing multi-scale and multi-level mineralization, and has stronger mechanical properties than traditional mineralized collagen materials, and the prepared structure and mechanical properties have a very high degree of matching with human bone tissue, greatly improving the development prospects of bionic mineralized collagen. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 This is a flow chart for preparing mineralized collagen of the present invention;

[0023] Figure 2 A scheme diagram for realizing dynamic cross-linking to regulate the in vitro biomimetic mineralization of bone matrix, wherein A is the dynamic cross-linking scheme of Example 1, B is the cross-linking without mineralization scheme of Comparative Example 1, C is the cross-linking before mineralization scheme of Comparative Example 2, and D is the mineralization without cross-linking scheme of Comparative Example 3;

[0024] Figure 3The cross-sectional SEM images of the mineralized collagen scaffolds mineralized under different cross-linking conditions, wherein A1 is the SEM electron microscopic structure diagram of comparative example 1 at a scale of 1 mm, A2 is the SEM electron microscopic structure diagram of comparative example 1 at a scale of 200 μm, A3 is the SEM electron microscopic structure diagram of comparative example 1 at a scale of 50 μm, B1 is the SEM electron microscopic structure diagram of comparative example 2 at a scale of 1 mm, B2 is the SEM electron microscopic structure diagram of comparative example 2 at a scale of 200 μm, B3 is the SEM electron microscopic structure diagram of comparative example 2 at a scale of 50 μm, B4 is the EDS energy spectrum analysis diagram of calcium element at a scale of 500 μm of comparative example 2, B5 is the EDS energy spectrum analysis diagram of phosphorus element at a scale of 500 μm of comparative example 2, and C1 is the SEM electron microscopic structure diagram of comparative example 3 at a scale of 1 mm. Structural diagram, C2 is the structural diagram of comparative example 3 observed by SEM electron microscope at a scale of 200μm, C3 is the structural diagram of comparative example 3 observed by SEM electron microscope at a scale of 50μm, C4 is the energy dispersion x-ray spectrum analysis diagram of calcium element at a scale of 500μm of comparative example 3, C5 is the energy dispersion x-ray spectrum analysis diagram of phosphorus element at a scale of 500μm of comparative example 3, D1 is the structural diagram of Example 1 observed by SEM electron microscope at a scale of 1mm, D2 is the structural diagram of Example 1 observed by SEM electron microscope at a scale of 200μm, D3 is the structural diagram of Example 1 observed by SEM electron microscope at a scale of 50μm, D4 is the energy dispersion x-ray spectrum analysis diagram of calcium element at a scale of 500μm of Example 1, and D5 is the energy dispersion x-ray spectrum analysis diagram of phosphorus element at a scale of 500μm of Example 1;

[0025] Figure 4 The results of the enzymatic hydrolysis rate of collagen prepared by different methods;

[0026] Figure 5 These are the results of mechanical testing of collagen prepared by different methods. DETAILED DESCRIPTION

[0027] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0028] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0029] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0030] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0031] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0032] Instrument used in the present invention: scanning electron microscope (FEI, Quanta 650 FEG, USA).

[0033] The type I collagen solution used in the present invention is prepared by using bovine Achilles tendon type I collagen with a mass concentration of 1-3% purchased from Chengdu Kele Biological Products Co., Ltd. as the collagen stock solution and diluting the concentration to the required concentration with deionized water.

[0034] The EDC solution (1-ethyl-3-(3-dimethylaminopropyl)-carbodiimide solution), NHS solution (N-hydroxysuccinimide solution), calcium chloride solution, diammonium hydrogen phosphate solution, sodium hydroxide solution and potassium hydroxide solution used in the present invention are all prepared with water as solvent.

[0035] Example 1

[0036] (1) Take 2 mL of type I collagen solution with a mass concentration of 0.8%, add 1 mL of EDC solution with a mass concentration of 3.2%, 1 mL of NHS solution with a mass concentration of 0.8%, and 1 mL of 8.88 M calcium chloride solution in sequence, stir well at a speed of 65 r / min, adjust the pH to 7.4 with a 1 M sodium hydroxide solution, and react for 8 hours to obtain a reaction mixture 1;

[0037] (2) adding 1 mL of 4.77 M diammonium hydrogen phosphate solution to the reaction mixture 1, and crosslinking and mineralizing for 12 h to obtain the reaction mixture 2;

[0038] (3) The reaction mixture 2 was placed in a -20°C environment for freezing treatment for 24 hours, and then vacuum freeze-dried at a vacuum degree of <6 Pa and a temperature of -70°C for 24 hours to obtain mineralized collagen. Figure 1 The preparation process is shown.

[0039] Example 2

[0040] (1) Take 3 mL of type I collagen solution with a mass concentration of 0.7%, add 1 mL of EDC solution with a mass concentration of 1.2%, 1 mL of NHS solution with a mass concentration of 0.3%, and 1 mL of calcium chloride solution with a concentration of 8.78 M, respectively, stir well at a speed of 50 r / min, adjust the pH to 7.4 with a potassium hydroxide solution with a concentration of 1 M, and react for 6 hours to obtain a reaction mixture 1;

[0041] (2) adding 1 mL of 4.67 M diammonium hydrogen phosphate solution to the reaction mixture 1, and crosslinking and mineralizing for 10 h to obtain the reaction mixture 2;

[0042] (3) The reaction mixture 2 was placed in a -15°C environment for freezing treatment for 28 hours, and then vacuum freeze-dried for 28 hours at a vacuum degree of <6 Pa and a temperature of -55°C to obtain mineralized collagen.

[0043] Example 3

[0044] (1) Take 1 mL of 0.9% type I collagen solution, add 1 mL of 5.2% EDC solution, 1 mL of 1.3% NHS solution and 1 mL of 8.98M calcium chloride solution in sequence, stir well at 80 r / min, adjust pH to 7.4 with 1M sodium hydroxide solution, react for 9 h, and obtain reaction mixture 1;

[0045] (2) adding 1 mL of 4.87 M diammonium hydrogen phosphate solution to the reaction mixture 1, and crosslinking and mineralizing for 24 h to obtain the reaction mixture 2;

[0046] (3) The reaction mixture 2 was placed in a -25°C environment for freezing treatment for 20 h, and then vacuum freeze-dried for 20 h at a vacuum degree of <6 Pa and a temperature of -85°C to obtain mineralized collagen.

[0047] Comparative Example 1

[0048] Take 2 mL of type I collagen solution with a mass concentration of 0.8%, add 1 mL of EDC solution with a mass concentration of 3.2%, 1 mL of NHS solution with a mass concentration of 0.8% and 1 mL of calcium chloride solution with a concentration of 8.88 M in sequence, stir thoroughly at a speed of 65 r / min, adjust the pH to 7.4 with a 1 M sodium hydroxide solution, react for 12 hours, put it in a -20°C environment for freezing treatment for 24 hours, and then vacuum freeze-dry it at a vacuum degree of <6 Pa and a temperature of -70°C for 24 hours to obtain mineralized collagen.

[0049] Comparative Example 2

[0050] (1) Take 2 mL of type I collagen solution with a mass concentration of 0.8%, add 1 mL of EDC solution with a mass concentration of 3.2%, 1 mL of NHS solution with a mass concentration of 0.8%, and 1 mL of calcium chloride solution with a concentration of 8.88 M, respectively, stir the mixture at a speed of 65 r / min, adjust the pH to 7.4 with a sodium hydroxide solution with a concentration of 1 M, and react for 12 hours to obtain a reaction mixture 1;

[0051] (2) adding 1 mL of 4.77 M diammonium hydrogen phosphate solution to the reaction mixture 1, and crosslinking and mineralizing for 12 h to obtain the reaction mixture 2;

[0052] (3) The reaction mixture 2 was placed in a -20°C environment for freezing treatment for 24 hours, and then vacuum freeze-dried at a vacuum degree of <6 Pa and a temperature of -70°C for 24 hours to obtain mineralized collagen.

[0053] Comparative Example 3

[0054] Take 2 mL of type I collagen solution with a mass concentration of 0.8%, add 1 mL of 8.88 M calcium chloride solution and 1 mL of 4.77 M diammonium phosphate solution thereto in sequence, stir thoroughly at a speed of 65 r / min, adjust the pH to 7.4 with 1 M sodium hydroxide solution, react for 12 hours, freeze it in an environment of -20°C for 24 hours, and then vacuum freeze-dry it at a vacuum degree of <6 Pa and a temperature of -70°C for 24 hours to obtain mineralized collagen.

[0055] Experimental Example 1

[0056] The mineralized collagen prepared in Example 1, Comparative Example 1, Comparative Example 2 and Comparative Example 3 was subjected to electron microscope scanning.

[0057] The above scanning electron microscope (SEM) micro-scale and energy dispersive x-ray spectroscopy (EDS) were analyzed and compared, and the results are as follows: Figure 3 As shown. Figure 3From A1, A2 and A3, it can be seen that the cross-linked, unmineralized cross-linked collagen prepared in Comparative Example 1 has many interconnected and entangled microfibrils on its surface, with denser pores and a high degree of cross-linking. The cross-linked collagen fibers transition from filaments to sheets, and protruding holes are formed due to entanglement and extrusion. Figure 3 From B1, B2, B3, B4 and B5, we can see that the mineralized collagen prepared in Comparative Example 2, which was first cross-linked and then mineralized, has relatively loose pores, and the surface of the mineralized collagen is wrapped by minerals, forming flaky hydroxyapatite. Calcium ions and phosphorus ions are evenly and widely distributed on the surface of the mineralized collagen, indicating that mineralization destroys the cross-linked structure, causing the minerals to adhere to the surface of the collagen layer and not penetrate into the collagen fibers. Figure 3 From C1, C2, C3, C4, and C5, it can be seen that the mineralized collagen prepared in Comparative Example 3 can be observed to have obvious collagen fibers, and the content of attached minerals is relatively small. The flake-shaped minerals are attached to the surface of the collagen, and the spherical minerals are attached to the collagen fibers. Calcium and phosphorus are evenly distributed on the surface of the mineralized collagen. Since there is no cross-linking in this example, there is no connection between the collagen molecules, which cannot provide better structural conditions for the deposition of minerals, so the mineralization effect is not good. Figure 3 It can be seen from D1, D2, D3, D4 and D5 that the pores of the cross-linked and mineralized mineralized collagen prepared in Example 1 are relatively loose, and clear entangled cross-linked collagen can be observed, and minerals are attached inside the collagen fibers. The distribution of calcium ions and phosphorus ions is consistent with that of collagen, indicating that mineralization and cross-linking occur simultaneously, resulting in the growth of minerals on the collagen and the minerals penetrating into the collagen fibers to form uniformly mineralized mineralized collagen.

[0058] Among them, Figure 3 As shown in the figure, dynamic cross-linking is the key to promoting the entry of minerals into the collagen scaffold, and dynamic cross-linking is also the key to adjusting the aggregation morphology of minerals. Without dynamic cross-linking, minerals are only distributed on the surface, and less enter the collagen scaffold. If dynamic cross-linking is performed, minerals can penetrate deep into the collagen fibers, and cross-linking and collagen entanglement occur at the same time, thereby increasing the uniformity and amount of minerals, which may play a powerful role in the preparation of artificial bone substitute materials.

[0059] Experimental Example 2

[0060] The enzymatic hydrolysis performance evaluation experiment is performed as follows:

[0061] The enzymatic hydrolysis experiments were conducted to analyze the enzymatic hydrolysis rates of the collagen matrices in different cross-linked states, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Example 1. The collagen samples of Comparative Example 1 (cross-linked only but not mineralized), Comparative Example 2 (cross-linked first and then mineralized), Comparative Example 3 (mineralized only) and Example 1 (cross-linked and mineralized simultaneously) were cut into 1 mm*1 mm cylinders, and the samples were immersed in 1 M PBS solution. After 1 hour, the sample mass was measured to be m 0 Then, the sample was immersed in a 0.25% trypsin solution for 24 hours. To simulate the enzymatic hydrolysis environment in vivo, the sample was placed in a 37°C water bath. After 24 hours, the sample mass was measured to be m 1 , enzymatic hydrolysis rate calculation formula (m 0 -m 1 ) / m 0 *100%, the enzymatic hydrolysis rate bar graph is measured and analyzed.

[0062] The results are as follows Figure 4 As shown, there is a significant difference between the enzymatic hydrolysis rate of the mineralized collagen in Example 1 and the enzymatic hydrolysis rates of the mineralized collagen in Comparative Examples 2 and 3. Among them, the enzymatic hydrolysis rate of the mineralized collagen in Example 1 is the lowest, which confirms that the inorganic content of the mineralized collagen in Example 1 is higher than that in Comparative Examples 1, 2 and 3, indicating that dynamic crosslinking can promote the entry of inorganic minerals into the interior of the collagen, thereby increasing the mineral content of the mineralized collagen, thereby affecting the enzymatic hydrolysis performance. Dynamic crosslinking to regulate the biomimetic mineralization of collagen in vitro is conducive to the preparation of bone repair materials with good enzymatic hydrolysis performance and a mineralized morphology close to the natural structure, which can be used for subsequent bone repair of load-bearing parts in the body.

[0063] Experimental Example 3

[0064] The mechanical properties evaluation experiment is performed as follows:

[0065] Through compression test, the elastic modulus of the collagen matrix under different cross-linking and mineralization conditions, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Example 1 were analyzed. The collagen samples of Comparative Example 1 (cross-linked only but not mineralized), Comparative Example 2 (cross-linked first and then mineralized), Comparative Example 3 (mineralized only) and Example 1 (cross-linked and mineralized at the same time) were cut into cylinders with a diameter of 5.6 mm and a height of 2.5 mm, and tested using a universal material testing machine (purchased from INSTRON, USA) at a speed of 0.05 mm / s and a compression force of 20 N to obtain a force-displacement curve. The elastic modulus bar graph was calculated and analyzed based on the measured results as shown in the figure. Figure 5 shown.

[0066] The results are as follows Figure 5As shown, there is a significant difference between the elastic modulus of the mineralized collagen of Example 1 and the elastic modulus of the mineralized collagen of Comparative Examples 2 and 3. Among them, the elastic modulus of the mineralized collagen of Example 1 is the highest, which proves that the mineralized collagen of Example 1 is more sensitive to force, has stronger resilience and rigidity, and is less prone to deformation. It shows that dynamic crosslinking can improve the mechanical properties of mineralized collagen, has higher strength, and is closer to the properties of natural bone, which may have a strong significance for improving the mechanical properties of artificial bone.

[0067] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing mineralized collagen based on dynamic cross-linking, characterized in that: The following steps are involved: (1) Add EDC solution, NHS solution and calcium chloride solution to the collagen solution in sequence, stir, adjust the pH, and react for 6 to 9 hours to obtain reaction mixture 1; (2) adding diammonium hydrogen phosphate solution to the reaction mixture 1 obtained in step (1), and crosslinking and mineralizing for 10 to 24 hours to obtain a reaction mixture 2; (3) freezing the reaction mixture obtained in step (2) and then freeze-drying it in a vacuum to obtain mineralized collagen; The collagen solution in step (1) is a type I collagen solution, and the mass concentration of the type I collagen solution is 0.7-0.9%; The mass concentration of the EDC solution in step (1) is 1.2-5.2%, the mass concentration of the NHS solution is 0.3-1.3%, and the concentration of the calcium chloride solution is 8.78-8.98M; In step (1), the volume ratio of the collagen solution, EDC solution, NHS solution and calcium chloride solution is 1 to 3:1:1:

1.

2. The preparation method according to claim 1, characterized in that The stirring speed in step (1) is 50 to 80 r / min.

3. The preparation method according to claim 1, characterized in that: The solution for adjusting pH in step (1) is sodium hydroxide solution and / or potassium hydroxide solution.

4. The preparation method according to claim 1, characterized in that The concentration of the diammonium hydrogen phosphate solution in step (2) is 4.67-4.87 M, and the volume ratio of the diammonium hydrogen phosphate solution to the calcium chloride solution is 1:

1.

5. The preparation method according to claim 1, characterized in that: The temperature of the freezing treatment in step (3) is -15 to -25°C, and the time of the freezing treatment is 20 to 28 hours.

6. The preparation method according to claim 1, characterized in that: The vacuum degree of the vacuum freeze drying in step (3) is less than 6 Pa, the temperature of the vacuum freeze drying is -55 to -85°C, and the time of the vacuum freeze drying is 20 to 28 hours.

7. The mineralized collagen prepared by the method according to any one of claims 1 to 6.

Citation Information

Cited By

  • Preparation method of gas-jet mineralized collagen-hydrogel microspheres

    CN120617620A