Itaconic acid and oxidized starch copolymer for scale and dispersible corrosion inhibitor and preparation method and application thereof

The copolymer generated by the copolymerization of itaconic acid and hydrogen peroxide oxidized starch solves the problem of environmental harm and insufficient performance of phosphorus-containing scale and dispersion corrosion inhibitors in industrial circulating cooling water systems, and achieves efficient scale inhibition, dispersion and corrosion inhibition. performance, suitable for environmentally friendly water treatment, reducing costs and pollution.

CN118307720BActive Publication Date: 2024-10-01ENERGY RESOURCES INST HEBEI ACADEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410705567.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2024-10-01
Estimated Expiration
2044-06-03

AI Technical Summary

Technical Problem

Phosphorus-containing scale and dispersion corrosion inhibitors used in existing industrial circulating cooling water systems are harmful to the environment, and the application of oxidized starch in copolymers has not been reported, resulting in insufficient performance and environmental pollution problems in circulating cooling water treatment. .

Method used

The copolymer generated by the copolymerization of itaconic acid and hydrogen peroxide oxidized starch is used as a scale and dispersion corrosion inhibitor. Through specific preparation methods and monomer ratio adjustment, its scale inhibition, dispersion and corrosion inhibition properties are improved, and production costs are reduced.

Benefits of technology

It achieves efficient scale inhibition, dispersed iron oxide and corrosion inhibition properties, and does not contain phosphorus and nitrogen elements. It is suitable for environmentally friendly water treatment agents, reduces the cost of industrial circulating water treatment, and is environmentally friendly to water bodies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_4
    Figure SMS_4
  • Figure SMS_5
    Figure SMS_5
Patent Text Reader

Abstract

The present invention relates to a copolymer of itaconic acid and oxidized starch for scale inhibition and dispersing corrosion inhibitor, and a preparation method and application thereof, wherein the copolymer is obtained by copolymerizing itaconic acid and hydrogen peroxide oxidized starch, and the mass ratio of the itaconic acid to the oxidized starch is 2.5-4.5: 1. The polymer provided by the present invention has excellent scale inhibition performance, iron oxide dispersing performance and corrosion inhibition performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of water treatment, and in particular to a copolymer of itaconic acid and oxidized starch used as a scale inhibitor, dispersant and corrosion inhibitor, and a preparation method and application thereof. Background Art

[0002] In industrial circulating cooling water systems, the most commonly used treatment method today is chemical treatment, that is, by adding scale inhibitors and corrosion inhibitors to treat scaling, corrosion and other problems in industrial circulating cooling water systems. The most widely used and successful scale inhibitors and corrosion inhibitors in domestic circulating cooling water treatment are phosphorus-containing scale inhibitors and corrosion inhibitors. Due to the well-known harm of phosphates to the environment, the use of phosphorus-containing scale inhibitors and corrosion inhibitors has been gradually restricted, and circulating cooling water treatment urgently needs to be "phosphate-free". The applicant has carried out a lot of research work around improving the performance and environmental friendliness of water treatment agents for industrial circulating cooling water systems.

[0003] The use of oxidized starch in water treatment scale inhibitors has been reported, but it appears in the form of a uniform composition, mixed with other ingredients for water treatment. For example, CN102452723A discloses a phosphorus-free composite scale inhibitor, which is made by mixing 10% to 13% polyaspartic acid, 25% to 28% sodium lignin sulfate, 10% to 13% oxidized starch, and 50% to 55% deionized water. CN110342654A discloses a new type of phosphorus-free corrosion inhibitor, characterized in that it is made of the following raw materials in mass percentage: 30-80% of a modified chitosan quaternary ammonium salt mixture, 10-50% of an oxidized starch mixture, and 10-25% of an alkylamine emulsion.

[0004] There are no reports on oxidized starch in copolymers. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects in the prior art, provide a copolymer of itaconic acid and oxidized starch for use as a scale inhibitor, dispersant and corrosion inhibitor, and also provide a preparation method and application thereof.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] The first aspect of the present invention provides an itaconic acid and oxidized starch copolymer for scale and dispersing corrosion inhibitor, which is obtained by copolymerizing itaconic acid and hydrogen peroxide oxidized starch, and the mass ratio of the itaconic acid to the hydrogen peroxide oxidized starch is 2.5-4.5:1.

[0008] As some preferred embodiments of the present invention, the mass ratio of the itaconic acid to the hydrogen peroxide oxidized starch is 3:1.

[0009] The second aspect of the present invention provides a method for preparing a copolymer of itaconic acid and oxidized starch for use as a scale-inhibiting and dispersing corrosion inhibitor, comprising the following steps:

[0010] Add hydrogen peroxide oxidized starch into distilled water and stir until it is in a suspension state. Pass nitrogen and heat to 68-75°C for gelatinization for 0.5-1h. Add ammonium persulfate solution and stir for a while. Add itaconic acid solution dropwise and polymerize at a constant temperature for 3-5h after the addition is completed. After the polymerization is completed, dry the product to obtain.

[0011] As some preferred embodiments of the present invention, the amount of ammonium persulfate added is 5-10% of the total mass of itaconic acid and hydrogen peroxide oxidized starch; and the mass concentration of the ammonium persulfate solution is 8-12%.

[0012] As some preferred embodiments of the present invention, the hydrogen peroxide oxidized starch is added to 6-10 times the mass of distilled water and stirred for dispersion, and the mass percentage of the itaconic acid aqueous solution is 8-15%.

[0013] As some preferred embodiments of the present invention, the ammonium persulfate solution is added and stirred for 8-12 minutes, and the itaconic acid solution is added dropwise for 24-48 minutes.

[0014] As some preferred embodiments of the present invention, the preparation of the hydrogen peroxide oxidized starch is as follows:

[0015] Add distilled water to soluble corn starch and stir until it becomes a paste. Use sodium hydroxide solution to adjust the pH value to 5-7, heat to 40-60°C, slowly add 30% hydrogen peroxide, react for 3-5 hours, filter the obtained solution, wash with distilled water, and dry to obtain hydrogen peroxide oxidized starch solid.

[0016] As some preferred embodiments of the present invention, the amount of the 30% hydrogen peroxide added is 20% of the mass of the soluble starch.

[0017] As some preferred embodiments of the present invention, the mass ratio of the soluble corn starch to distilled water is 1:10.

[0018] The third aspect of the present invention provides the use of the above-mentioned itaconic acid and oxidized starch copolymer for scale and corrosion inhibition as a water treatment agent in industrial circulating cooling water.

[0019] The beneficial effects of adopting the above technical solution are:

[0020] 1. The polymer provided by the present invention has excellent scale inhibition performance, iron oxide dispersion and corrosion inhibition performance.

[0021] 2. The polymer provided by the present invention has significantly improved scale inhibition, dispersibility and corrosion inhibition performance through monomer selection and ratio adjustment, and has a synergistic effect.

[0022] 3. The polymer provided by the present invention is low in cost, the initiator greatly promotes the polymerization of the monomer, and the preparation method has a high degree of polymerization, which can greatly reduce industrial costs and reduce the treatment cost of industrial circulating water.

[0023] 4. The monomers used and the synthesized copolymers do not contain phosphorus and nitrogen elements that may cause eutrophication of water bodies, and their application is friendly to the water environment and does not pollute the water body.

[0024] 5. The monomers used in the polymer are all environmentally friendly compounds, and the synthesis process is green and pollution-free, and the obtained product is an environmentally friendly green agent. DETAILED DESCRIPTION

[0025] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention is clearly and completely described below in conjunction with specific embodiments.

[0026] Preparation Example 1

[0027] A certain amount of soluble corn starch and distilled water equivalent to 10 times its mass were added to a four-necked flask and stirred until it became a paste. The pH value was adjusted to 6 with a sodium hydroxide solution with a mass concentration of 1%, and the water bath was heated to 50°C. 30% hydrogen peroxide was slowly added to the system by a syringe pump (the amount of hydrogen peroxide added was 20% of the mass of starch). The pH value was kept constant during this process. After the addition was completed, the solution in the system reacted for 4 hours, and the obtained solution was filtered, washed with distilled water and dried to finally obtain hydrogen peroxide oxidized starch (OS) solid.

[0028] Example 1

[0029] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system with a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the addition time was 0.5h. After the addition was completed, the reaction was continued for 4h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0030] Example 2

[0031] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 6 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 68°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, an 8% itaconic acid solution was slowly injected into the system with a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 4h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0032] Example 3

[0033] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 75°C. The starch was stirred and gelatinized for 1 hour. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the dropwise addition time was 0.5 hours. After the dropwise addition was completed, the reaction was continued for 4 hours. After the reaction was completed, the product was dried in an oven at 80°C for 24 hours to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0034] Example 4

[0035] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a 12% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 5% of the total mass of oxidized starch and itaconic acid. After 12 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the addition time was 0.5h. After the addition was completed, the reaction was continued for 4h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0036] Example 5

[0037] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, an ammonium persulfate solution with a mass concentration of 8% was added using a syringe pump, and the mass of ammonium persulfate was 10% of the total mass of oxidized starch and itaconic acid. After 8 minutes of initiation, a 10% mass percentage itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 4h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0038] Example 6

[0039] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 10 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 15% itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the dropwise addition time was 24 minutes. After the dropwise addition was completed, the reaction was continued for 4 hours. After the reaction was completed, the product was dried in an oven at 80°C for 24 hours to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0040] Example 7

[0041] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 4.5:1, and the dropwise addition time was 48 minutes. After the dropwise addition was completed, the reaction was continued for 4 hours. After the reaction was completed, the product was dried in an oven at 80°C for 24 hours to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0042] Example 8

[0043] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 2.5:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 3h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0044] Example 9

[0045] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 5h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0046] Comparative Example 1

[0047] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 50°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 4:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 4h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0048] Comparative Example 2

[0049] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 6h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0050] Comparative Example 3

[0051] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 30 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system with a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the addition time was 0.5h. After the addition was completed, the reaction was continued for 4h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0052] Comparative Example 4

[0053] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 3% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 2h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0054] Comparative Example 5

[0055] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 6:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 4h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0056] Comparative Example 6

[0057] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 80°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system with a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the addition time was 0.5h. After the addition was completed, the reaction was performed for 8h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0058] Comparative Example 7

[0059] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 15% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the addition time was 0.5h. After the addition was completed, the reaction was continued for 3h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0060] Comparative Example 8

[0061] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 50°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 2% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system with a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the addition time was 0.5h. After the addition was completed, the reaction was continued for 4h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0062] Comparative Example 9

[0063] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 1:3, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 4h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0064] Comparative Example 10

[0065] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 12% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 2:1, and the addition time was 0.5h. After the addition was completed, the reaction was continued for 4h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0066] Comparative Example 11

[0067] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask. In a suspension state, the temperature was raised to 70°C, and the starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 4h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0068] Comparative Example 12

[0069] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 10% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system with a syringe pump. The mass ratio of itaconic acid to oxidized starch was 1:2, and the dripping time was 0.5h. After the dripping was completed, the reaction was continued for 4h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0070] Comparative Example 13

[0071] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 1.5 hours. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the dropwise addition time was 0.5 hours. After the dropwise addition was completed, the reaction was continued for 4 hours. After the reaction was completed, the product was dried in an oven at 80°C for 24 hours to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0072] Comparative Example 14

[0073] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium persulfate solution was added with a syringe pump, and the mass of ammonium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was injected into the system within 5 minutes using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1. After the injection was completed, the reaction was carried out for 4 hours. After the reaction was completed, the product was dried in an oven at 80°C for 24 hours to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0074] Comparative Example 15

[0075] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a 10% ammonium cerium nitrate solution was added with a syringe pump, and the mass of ammonium cerium nitrate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 4h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0076] Comparative Example 16

[0077] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 8 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 70°C. The starch was stirred and gelatinized for 0.5h. Then, a potassium persulfate solution with a mass concentration of 10% was added with a syringe pump, and the mass of potassium persulfate was 6% of the total mass of oxidized starch and itaconic acid. After 10 minutes of initiation, a 10% mass percentage of itaconic acid solution was slowly injected into the system using a syringe pump. The mass ratio of itaconic acid to oxidized starch was 3:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 4h. After the reaction was completed, the product was dried in an oven at 80°C for 24h to obtain a solid product. The solid product was washed with ethanol and dried again to obtain the final product.

[0078] Comparative Example 17

[0079] Hydrogen peroxide oxidized starch was prepared according to the method of Preparation Example 1, and it was mechanically mixed with itaconic acid at a mass ratio of 3:1, and the product was obtained after mixing evenly.

[0080] Test Example 1

[0081] The scale inhibition performance and dispersibility performance of the polymers obtained in the examples and comparative examples were evaluated respectively.

[0082] The performance of the agent in inhibiting calcium carbonate scale and calcium phosphate scale was evaluated according to GB / T16632-2008 "Determination of scale inhibition performance of water treatment agents - Calcium carbonate deposition method" and GB / T22626-2008 "Determination of scale inhibition performance of water treatment agents - Calcium phosphate deposition method" respectively; the dispersion performance was evaluated by measuring the dispersion performance of the agent on iron oxide (with the transmittance of distilled water as 100% as the standard, the smaller the transmittance, the better the dispersion performance); the corrosion inhibition effect reached the national standard GB50050-2017 Industrial Circulating Cooling Water Treatment Design Code, and the corrosion rate of carbon steel was <0.075mm / a.

[0083] (1) Determination of scale inhibition performance of calcium carbonate

[0084] The experiment used prepared water and used non-evaporative concentration to determine the resistance to CaCO 3 Performance, Ca 2+ and HCO 3 - The concentrations were 600 mg / L and 1200 mg / L (in terms of CaCO 3 Calculate), add a certain amount of water treatment agent to 500ml water sample, put it into a constant temperature water bath at 80℃, and keep it at constant temperature for 10h. Then cool it to room temperature, take the upper clear layer, and determine the Ca in it by EDTA method 2+ The scale inhibition rate is calculated as shown in formula (1).

[0085] (1)

[0086] Where: C 0 The Ca content of the solution after the heating test without adding scale inhibitor and dispersant 2+ Content, mg / L;

[0087] C 1 The Ca content of the solution after the heating experiment when adding scale inhibitor and dispersant 2+ Content, mg / L;

[0088] C 2 Ca is the Ca content of the experimental water without adding scale inhibitor and dispersant and without heating 2+ Content, mg / L.

[0089] (2) Determination of scale inhibition performance of calcium phosphate

[0090] The experiment uses prepared water and non-evaporative concentration to determine the Ca resistance 3 (PO 4) 2 Performance, Ca 2+ The concentration is 250 mg / L (in terms of CaCO 3 ), PO 4 3- The concentration is 150mg / L. A certain amount of water treatment agent is added to 500ml of water sample. The pH value of the solution is 9 (adjusted with sodium tetraborate). It is placed in a constant temperature water bath at 80℃ and kept at constant temperature for 10 hours. Then it is cooled to room temperature, and the upper clear layer is taken and the PO in it is determined by a visible spectrophotometer. 4 3- The scale inhibition rate is calculated as shown in formula (2).

[0091] (2)

[0092] Where: C 0 The PO in the solution after the heating test without adding scale inhibitor and dispersant 4 3- Content, mg / L;

[0093] C 1 PO in the solution after heating test when adding scale inhibitor and dispersant 4 3- Content, mg / L;

[0094] C 2 PO 2 of the experimental water without adding scale inhibitor and dispersant and without heating 4 3- Content, mg / L.

[0095] (3) Dispersed Fe 2 O 3 Performance determination

[0096] Using analytically pure anhydrous calcium chloride and ammonium ferrous sulfate as reagents, the following experimental water samples were prepared: Ca 2+ The concentration is 150 mg / L (in terms of CaCO 3 , Fe 2+ The concentration is 10 mg / L. A certain amount of water treatment agent is added to 500 ml of water sample. The pH value of the solution is 9 (adjusted with sodium tetraborate). After strong stirring for 15 minutes, it is placed in a constant temperature water bath at 50°C for 5 hours. After cooling to room temperature, the upper layer of solution is taken and its transmittance T is measured at 450 nm with a visible spectrophotometer. The smaller the transmittance, the better the dispersion effect (taking distilled water as a reference, its transmittance is 100%).

[0097] (4) Determination of corrosion rate

[0098] The rotating coupon weight loss method was used, referring to the national standard GB / T 18175-2014, using a rotating coupon corrosion tester, A3 carbon steel sheet (50mm×25mm×2mm), test time: 72h; test temperature: 40℃; rotation speed: 75r / min, the corrosion rate X expressed in mm / a 1 The calculation formula is:

[0099]

[0100] Where: W is the weight of the specimen before testing, g; W 0 is the weight of the test piece after the test, g; A is the surface area of ​​the test piece, 28cm 2 ; D is the density of the test piece, carbon steel is 7.850g / cm 3 ; T is the test time of the specimen, 72h.

[0101] The following table shows the national standard for the corrosion rate of carbon steel. After adding the agent, the corrosion rate of the solution on carbon steel should be less than 0.075mm / a.

[0102] National Standard for Corrosion Rate of Carbon Steel

[0103]

[0104] The test results of various properties of the polymers obtained in the examples and comparative examples are shown in Table 1.

[0105] Table 1 Performance test results

[0106]

[0107] After testing, the copolymers of itaconic acid and oxidized starch obtained in Examples 1-9 have better scale inhibition, dispersion and corrosion inhibition properties than those in the comparative example, and have ideal comprehensive properties.

[0108] Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art may still modify the technical solutions described in the aforementioned embodiments, or make equivalent substitutions for some of the technical features therein; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A copolymer of itaconic acid and oxidized starch for use as a scale and corrosion inhibitor, characterized in that: The invention is obtained by copolymerizing itaconic acid and hydrogen peroxide oxidized starch, wherein the mass ratio of the itaconic acid to the hydrogen peroxide oxidized starch is 2.5-4.5:

1. The invention is prepared by the following steps: adding the hydrogen peroxide oxidized starch into distilled water and stirring it to form a suspension state, introducing nitrogen, heating it to 68-75°C, gelatinizing it for 0.5-1h, adding an ammonium persulfate solution, stirring it for a period of time, dripping itaconic acid solution, and polymerizing it at a constant temperature for 3-5h after the dripping is completed. After the polymerization is completed, the product is dried to obtain the product. The amount of the ammonium persulfate added is 5-10% of the total mass of the itaconic acid and the hydrogen peroxide oxidized starch. The mass concentration of the ammonium persulfate solution is 8-12%. After adding the ammonium persulfate solution, stirring is performed for 8-12min, and the dripping time of the itaconic acid solution is 24-48min.

2. The copolymer of itaconic acid and oxidized starch for scale and dispersing corrosion inhibitor according to claim 1, characterized in that: The mass ratio of the itaconic acid to the hydrogen peroxide oxidized starch is 3:

1.

3. The copolymer of itaconic acid and oxidized starch for scale and dispersing corrosion inhibitor according to claim 1, characterized in that: The hydrogen peroxide oxidized starch is added into 6-10 times the mass of distilled water and stirred for dispersion. The mass percentage of the itaconic acid aqueous solution is 8-15%.

4. The copolymer of itaconic acid and oxidized starch for scale and dispersing corrosion inhibitor according to claim 1, characterized in that: The preparation of the hydrogen peroxide oxidized starch is as follows: Add distilled water to soluble corn starch, stir to form a paste, adjust the pH value to 5-7 with sodium hydroxide solution, heat to 40-60°C, slowly add 30% hydrogen peroxide, react for 3-5 hours, filter the obtained solution, wash with distilled water, and dry to obtain hydrogen peroxide oxidized starch solid.

5. The copolymer of itaconic acid and oxidized starch for scale and dispersing corrosion inhibitor according to claim 4, characterized in that: The added amount of the 30% hydrogen peroxide is 20% of the mass of the soluble starch.

6. The copolymer of itaconic acid and oxidized starch for scale and dispersing corrosion inhibitor according to claim 4, characterized in that: The mass ratio of the soluble corn starch to distilled water is 1:

10.

7. Use of the copolymer of itaconic acid and oxidized starch for scale and dispersibility corrosion inhibitor as claimed in any one of claims 1 to 6 as a water treatment agent in industrial circulating cooling water.