A method for preparing modified epoxy resin adhesive

By organically modifying nano-silica, mercapto-modified silica was prepared and blended with epoxy resin to form a composite three-dimensional network structure. This solved the problem of easy agglomeration of inorganic particles in epoxy resin, improved the bonding performance and heat resistance, and enhanced the toughness and water resistance of the adhesive.

CN118308053BActive Publication Date: 2024-11-15CHUNG SHUN CENTURY ELECTRONIC MATERIAL (SHIXING) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410384860.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-01
Publication Date
2024-11-15
Estimated Expiration
2044-04-01

AI Technical Summary

Technical Problem

Existing inorganic particles tend to agglomerate in epoxy resins, leading to a decrease in adhesive properties.

Method used

By organically modifying nano-silica by grafting functional groups such as amino and carboxyl groups, mercapto-modified silica is prepared and then blended and cured with epoxy resin to form a composite three-dimensional network structure, achieving an effective combination of inorganic and organic particles.

Benefits of technology

It improves the bonding performance, heat resistance, and toughness of epoxy resin, enhances the mechanical properties and water resistance of adhesives, reduces shrinkage, and has self-healing properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a method for preparing a modified epoxy resin adhesive, and relates to the technical field of adhesives. The invention discloses a method for preparing a modified epoxy resin adhesive, comprising the following steps: using nano silicon dioxide as a raw material, after being organically treated with a silane coupling agent, and then sequentially through succinic anhydride ring-opening carboxylation, aminomethylboronic acid pinacol ester hydrochloride grafting, to obtain modified silicon dioxide; then using modified silicon dioxide and 1-thioglycerol as raw materials to prepare mercapto silicon dioxide; mercapto silicon dioxide, 1,8-diazabicycloundecane-7-ene, epoxy resin are blended and cured to obtain an adhesive. The adhesive prepared by the present application has excellent mechanical properties and flexibility, and good water resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesives, and in particular to a method for preparing a modified epoxy resin adhesive. Background Art

[0002] Epoxy resin, as one of the most commonly used thermosetting resins, is a polymer prepolymer composed of two or more groups of epoxy groups with aromatic or aliphatic as the main chain. Epoxy resin is widely used in aviation, vehicles, construction and other fields due to its strong bonding properties, good chemical corrosion resistance, good mechanical properties and excellent insulation properties. Epoxy resin adhesives have the advantages of being able to cure at room temperature, the curing pressure is only the contact pressure, and have high bonding strength, wide mechanical strength and wide bonding surface. However, after curing, the unmodified epoxy resin has a high cross-linking density and a three-dimensional network structure. It has the disadvantages of large internal stress, brittleness, poor heat resistance and impact resistance, which seriously limits its scope of use.

[0003] Commonly used methods for toughening epoxy resins are: (1) adding rubber elastomers to epoxy resins to form a dispersed phase, such as carboxyl-terminated nitrile rubber as a toughening agent, so that the mechanical and thermal properties of the adhesive are improved; (2) thermotropic liquid crystal polymer toughening resin alloying; (3) adding thermoplastic resins to the epoxy resin system to form an interpenetrating or semi-interpenetrating network structure, such as polyethersulfone resin; (4) introducing flexible segments into the cross-linked network of the system when the epoxy resin system is cured. However, although rubber or thermoplastic elastomers can greatly improve the impact strength of epoxy resins, it is at the expense of a decrease in tensile strength; reinforcing fibers can greatly improve the tensile strength of epoxy resins, but the impact strength and elongation at break are reduced; liquid crystal polymer in-situ composite reinforcement technology can improve the tensile strength and impact strength of epoxy resins, but the elongation at break is reduced. In contrast, epoxy resin modified by inorganic nanoparticles can effectively combine the rigidity, dimensional stability and thermal stability of inorganic materials with the toughness, processability and dielectric properties of polymers. Therefore, the research on epoxy resin modified by inorganic nanoparticles has become a research focus. However, nanoparticles have a large surface area, a high surface atomic occupancy rate, and a special structure with unsaturated bonds or dangling bonds on the surface, which makes the nanoparticles have very large surface activity, easy to agglomerate, and difficult to achieve uniform dispersion of nanometer size in the epoxy resin matrix, which leads to a decrease in bonding performance. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a modified epoxy resin adhesive to solve the following technical problems:

[0005] When existing inorganic particles are added to epoxy resin, as the amount of added particles increases, the inorganic particles tend to agglomerate, thereby causing the bonding performance of the epoxy resin to decrease.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing a modified epoxy resin adhesive comprises the following steps:

[0008] A1: Add modified silica, 1-thioglycerol, tetrahydrofuran and deionized water into a reaction kettle and disperse them evenly, add magnesium sulfate, react at room temperature for 24-30 hours under stirring conditions, filter and rotary evaporate to obtain mercapto silica;

[0009] A2: Add mercapto silicon dioxide, 1,8-diazabicycloundec-7-ene and epoxy resin into a reaction bottle, place it in a vacuum drying oven for degassing, and then perform curing treatment in the drying oven to obtain an adhesive.

[0010] As a further embodiment of the present invention: the addition ratio of modified silicon dioxide, 1-thioglycerol, tetrahydrofuran, deionized water and magnesium sulfate in A1 is 10 g: 2-4 g: 100-200 mL: 0.5-1 mL: 3-7 g.

[0011] As a further embodiment of the present invention: the mass ratio of mercapto silicon dioxide, 1,8-diazabicycloundec-7-ene and epoxy resin in A2 is 1-10:0.5-2:100.

[0012] As a further solution of the present invention: The specific steps of the curing treatment in A2 are: controlling the temperature to 70-90°C for insulation treatment for 1-3 hours, and controlling the temperature to 120-150°C for insulation treatment for 0.5-1 hour.

[0013] As a further embodiment of the present invention: the preparation method of modified silicon dioxide comprises the following steps:

[0014] S1: Add γ-aminopropyltriethoxysilane and deionized water component 1 to a reaction bottle, adjust the pH to 3-4, and obtain solution A; disperse nano-silicon dioxide, deionized water component 2, and anhydrous ethanol evenly to obtain solution B; add solution B to solution A, control the temperature to 50-60°C, keep warm for 3-6 hours under stirring conditions, centrifuge, filter, wash, and dry to obtain component 1;

[0015] S2: Add component 1 and N,N-dimethylformamide into a reaction kettle and disperse them evenly, add succinic anhydride, react at room temperature for 6-9 hours under stirring, wash with water, and dry to obtain component 2;

[0016] S3: In a nitrogen atmosphere, aminomethylboronic acid pinacol ester hydrochloride (CAS: 298689-75-5), component 2, 2-(1H-benzotriazol L-1-yl)-1,1,3,3-tetramethyluronium tetrafluoroborate (CAS: 125700-67-6), and N,N-dimethylformamide are added to a reaction bottle, the temperature is controlled at -20 to 0°C, the reaction is kept warm for 1-3 hours, N,N-diisopropylamine is added, the reaction is kept warm for 1-3 hours, the solvent is removed in vacuo, the mixture is washed, and the mixture is dried to obtain modified silica.

[0017] As a further solution of the present invention: the addition ratio of γ-aminopropyltriethoxysilane, deionized water component one, nano silicon dioxide, deionized water component two, and anhydrous ethanol in S1 is 0.1-0.5g:2-5mL:1g:10-50mL:10-50mL.

[0018] As a further solution of the present invention: the addition ratio of component 1, N,N-dimethylformamide and succinic anhydride in S2 is 1g:30-50mL:0.1-0.3g.

[0019] As a further scheme of the present invention: the addition ratio of aminomethylboronic acid pinacol ester hydrochloride, component two, 2-(1H-benzotriazo L-1-yl)-1,1,3,3-tetramethyluronium tetrafluoroborate, N,N-dimethylformamide, and N,N-diisopropylamine in S3 is 0.4-1g:10g:0.5-1g:10-100mL:0.5-1g.

[0020] Beneficial effects of the present invention:

[0021] (1) The present application first uses γ-aminopropyltriethoxysilane to organically modify the surface of nano-silica, grafts amino groups on the surface of silica, and obtains component one; and uses the amino groups of component one to open the ring carboxylation with succinic anhydride to graft a large number of carboxyl groups on the surface of silica, and obtains component two; finally, the amino groups of aminomethylboronic acid pinacol ester hydrochloride react with the carboxyl groups of component two to obtain modified silica. The surface of the modified silica prepared in the present application has functional groups such as boric acid groups, amino groups, and carboxyl groups grafted by organic silicon segments. The present application uses modified silica and 1-thioglycerol as raw materials to carry out chemical reaction to prepare mercapto-silica, and uses mercapto-silica as a toughening agent, 1,8-diazabicycloundec-7-ene as a curing agent accelerator, and epoxy resin as a base material to blend and degas and then cure to obtain a modified epoxy resin adhesive. The adhesive prepared in the present application has the advantages of excellent mechanical properties, good water resistance, and good heat resistance.

[0022] The modified silica added in the present application has unsaturated residual bonds and organic functional bonds in different bonding states on its surface, and its molecular state presents a three-dimensional network structure. Its surface has strong surface energy and chemical reaction activity, and has elastic mechanical properties similar to polymer chains. It forms chemical crosslinking points by chemical bonding with epoxy resin. The organic functional groups on the surface molecular chains of silica are entangled and adsorbed with epoxy polymer chains to form a composite three-dimensional network structure, so that the particle network and the epoxy polymer network are mutually extended and intertwined, effectively eliminating the interface energy difference between the two. Realize the composite of organic and inorganic particles; silicon dioxide, as an inorganic substance, introduces rigid particles into epoxy resin to form physical cross-linking points with polymer chains; modified silicon dioxide actually plays the role of physical and chemical cross-linking points in the adhesive. The high rigidity of the inorganic structure can reduce the adverse effects on the mechanical strength, modulus or thermal properties of the cured product, while the organic structure can give the epoxy cured product good toughness and good compatibility with epoxy resin. The groups on the surface of modified silicon dioxide that can react with epoxy resin are beneficial to the improvement of cross-linking density, and can achieve the effect of simultaneous toughening and strengthening.

[0023] (2) The present application first uses organosiloxane to organically modify silica, then uses succinic anhydride to perform ring-opening carboxylation, aminomethylboronic acid pinacol ester hydrochloride grafting, and 1-thioglycerol to perform mercapto modification, and then chemically copolymerizes the prepared mercapto silica with epoxy resin to improve the compatibility of silicone and epoxy resin, thereby solving the problem in the prior art that silicone and epoxy resin have large solubility parameter differences, which makes it difficult for silicone to be effectively dispersed in epoxy resin. With the addition of mercapto silica, not only is a flexible and stable silicon-oxygen chain introduced into the curing system to improve the heat resistance of the epoxy resin system and the toughness of the curing system, but the surface energy of silicone is lower than that of epoxy resin, giving the adhesive water resistance and oil resistance; and the cross-linking density increases, the movement of the polymer chain segments is spatially restricted, the shrinkage of the adhesive layer is reduced, and the heat-resistant dimensional stability of epoxy resin curing is further improved, which can effectively improve the thermal properties of the adhesive.

[0024] (3) This application uses modified silica and 1-thioglycerol as raw materials to react and prepare thiolated silica. The thiol on the interface of silica is mixed with epoxy resin and then enters the cured epoxy resin structure, giving the cross-linked epoxy resin good flexibility, high shear strength and peel strength. This application uses γ-aminopropyltriethoxysilane to graft amino groups on the surface of silica, and uses the amino group of component one to open the ring carboxylation with succinic anhydride, and uses the amino group of aminomethylboronic acid pinacol ester hydrochloride to react with the carboxyl group of component two; a large number of carbamate groups are generated on the surface of silica, which are highly polar and active and have high adhesion to a variety of materials. In addition, the borate bonds generated during the reaction have the ability to give the adhesive a bonding property similar to "self-healing". DETAILED DESCRIPTION

[0025] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Example 1 The preparation method of modified silicon dioxide comprises the following steps:

[0027] S1: Add 5g of γ-aminopropyltriethoxysilane and 20mL of deionized water component 1 into a reaction bottle, add glacial acetic acid to adjust the pH to 3, and obtain solution A; evenly disperse 10g of nano-silicon dioxide, 100mL of deionized water component 2, and 100mL of anhydrous ethanol to obtain solution B; add solution B to solution A, control the temperature to 50°C, keep warm for 3h under stirring, centrifuge, filter, wash, and dry to obtain component 1;

[0028] S2: 10 g of component 1 and 300 mL of N,N-dimethylformamide were added to a reaction kettle and dispersed evenly, 1 g of succinic anhydride was added, and the mixture was reacted at room temperature for 6 h under stirring conditions, and then washed with water and dried to obtain component 2;

[0029] S3: In a nitrogen atmosphere, 1 g of aminomethylboronic acid pinacol ester hydrochloride (CAS: 298689-75-5), 10 g of component 2, 1 g of 2-(1H-benzotriazol L-1-yl)-1,1,3,3-tetramethyluronium tetrafluoroborate (CAS: 125700-67-6), and 100 mL of N,N-dimethylformamide were added to a reaction bottle, the temperature was controlled at -20°C, and the reaction was kept warm for 3 hours. 0.5 g of N,N-diisopropylamine was added, and the reaction was kept warm for 1 hour. The solvent was removed in vacuo, washed, and dried to obtain modified silica.

[0030] Example 2 The preparation method of modified silicon dioxide comprises the following steps:

[0031] S1: Add 5g of γ-aminopropyltriethoxysilane and 40mL of deionized water component 1 into a reaction bottle, add glacial acetic acid to adjust the pH to 3, and obtain solution A; evenly disperse 10g of nano-silicon dioxide, 100mL of deionized water component 2, and 100mL of anhydrous ethanol to obtain solution B; add solution B to solution A, control the temperature to 55°C, keep warm for 3h under stirring, centrifuge, filter, wash, and dry to obtain component 1;

[0032] S2: 10 g of component 1 and 300 mL of N,N-dimethylformamide were added to a reaction kettle and dispersed evenly, 2 g of succinic anhydride was added, and the mixture was reacted at room temperature for 6 h under stirring conditions, and then washed with water and dried to obtain component 2;

[0033] S3: In a nitrogen atmosphere, 1 g of aminomethylboronic acid pinacol ester hydrochloride (CAS: 298689-75-5), 10 g of component 2, 1 g of 2-(1H-benzotriazol L-1-yl)-1,1,3,3-tetramethyluronium tetrafluoroborate (CAS: 125700-67-6), and 100 mL of N,N-dimethylformamide were added to a reaction bottle, the temperature was controlled at -10°C, the reaction was kept warm for 1 hour, 1 g of N,N-diisopropylamine was added, the reaction was kept warm for 1 hour, the solvent was removed in vacuo, the mixture was washed, and the mixture was dried to obtain modified silica.

[0034] Example 3 The preparation method of modified silicon dioxide comprises the following steps:

[0035] S1: Add 5g of γ-aminopropyltriethoxysilane and 50mL of deionized water component 1 into a reaction bottle, add glacial acetic acid to adjust the pH to 3, and obtain solution A; evenly disperse 10g of nano-silicon dioxide, 100mL of deionized water component 2, and 100mL of anhydrous ethanol to obtain solution B; add solution B to solution A, control the temperature to 50°C, keep warm for 3h under stirring, centrifuge, filter, wash, and dry to obtain component 1;

[0036] S2: 10 g of component 1 and 300 mL of N,N-dimethylformamide were added to a reaction kettle and dispersed evenly, 3 g of succinic anhydride was added, and the mixture was reacted at room temperature for 9 h under stirring, and then washed with water and dried to obtain component 2;

[0037] S3: In a nitrogen atmosphere, 1 g of aminomethylboronic acid pinacol ester hydrochloride (CAS: 298689-75-5), 10 g of component 2, 1 g of 2-(1H-benzotriazol L-1-yl)-1,1,3,3-tetramethyluronium tetrafluoroborate (CAS: 125700-67-6), and 100 mL of N,N-dimethylformamide were added to a reaction bottle, the temperature was controlled at 0°C, and the reaction was kept warm for 3 hours. 1 g of N,N-diisopropylamine was added, and the reaction was kept warm for 1-3 hours. The solvent was removed in vacuo, washed, and dried to obtain modified silica.

[0038] Example 4 A method for preparing a modified epoxy resin adhesive comprises the following steps:

[0039] A1: 10 g of the modified silicon dioxide prepared in Example 1, 2 g of 1-thioglycerol, 100 mL of tetrahydrofuran, and 1 mL of deionized water were added to a reaction kettle and dispersed evenly, 3 g of magnesium sulfate was added, and the mixture was reacted at room temperature for 24 h under stirring, filtered, and rotary evaporated to obtain mercapto silicon dioxide;

[0040] A2: Add 5 g of mercaptosilicon dioxide, 2 g of 1,8-diazabicycloundec-7-ene, and 100 g of bisphenol A epoxy resin (epoxy resin with the brand name CYD-127 produced by Baling Petrochemical Branch of Sinopec Asset Management Company) into a reaction bottle, place it in a vacuum drying oven for degassing, and then control the temperature in the drying oven to 70°C for 3 h and control the temperature to 150°C for 1 h to obtain an adhesive.

[0041] Example 5 A method for preparing a modified epoxy resin adhesive comprises the following steps:

[0042] A1: 10 g of the modified silicon dioxide prepared in Example 2, 2 g of 1-thioglycerol, 100 mL of tetrahydrofuran, and 1 mL of deionized water were added to a reaction kettle and dispersed evenly, 3 g of magnesium sulfate was added, and the mixture was reacted at room temperature for 24 h under stirring, filtered, and rotary evaporated to obtain mercapto silicon dioxide;

[0043] A2: Add 5 g of mercaptosilicon dioxide, 2 g of 1,8-diazabicycloundec-7-ene, and 100 g of bisphenol A epoxy resin (epoxy resin with the brand name CYD-127 produced by Baling Petrochemical Branch of Sinopec Asset Management Company) into a reaction bottle, place it in a vacuum drying oven for degassing, and then control the temperature in the drying oven to 70°C for 3 h and control the temperature to 150°C for 1 h to obtain an adhesive.

[0044] Example 6 A method for preparing a modified epoxy resin adhesive comprises the following steps:

[0045] A1: 10 g of the modified silica prepared in Example 3, 2 g of 1-thioglycerol, 100 mL of tetrahydrofuran, and 1 mL of deionized water were added to a reaction kettle and dispersed evenly, 3 g of magnesium sulfate was added, and the mixture was reacted at room temperature for 24 h under stirring, filtered, and rotary evaporated to obtain thiolated silica;

[0046] A2: Add 5 g of mercaptosilicon dioxide, 2 g of 1,8-diazabicycloundec-7-ene, and 100 g of bisphenol A epoxy resin (epoxy resin with the brand name CYD-127 produced by Baling Petrochemical Branch of Sinopec Asset Management Company) into a reaction bottle, place it in a vacuum drying oven for degassing, and then control the temperature in the drying oven to 70°C for 3 h and control the temperature to 150°C for 1 h to obtain an adhesive.

[0047] Comparative Example 1 The preparation method of modified silicon dioxide comprises the following steps:

[0048] 5 g of γ-aminopropyltriethoxysilane and 20 mL of deionized water component one were added to a reaction bottle, and glacial acetic acid was added to adjust the pH to 3 to obtain solution A; 10 g of nano-silicon dioxide, 100 mL of deionized water component two, and 100 mL of anhydrous ethanol were evenly dispersed to obtain solution B; solution B was added to solution A, the temperature was controlled at 50° C., and the solution was kept warm for 3 hours under stirring conditions, centrifuged, filtered, washed, and dried to obtain modified silica.

[0049] Comparative Example 2 The preparation method of modified silicon dioxide comprises the following steps:

[0050] S1: Add 5g of γ-aminopropyltriethoxysilane and 20mL of deionized water component 1 into a reaction bottle, add glacial acetic acid to adjust the pH to 3, and obtain solution A; evenly disperse 10g of nano-silicon dioxide, 100mL of deionized water component 2, and 100mL of anhydrous ethanol to obtain solution B; add solution B to solution A, control the temperature to 50°C, keep warm for 3h under stirring, centrifuge, filter, wash, and dry to obtain component 1;

[0051] S2: Add 10 g of component 1 and 300 mL of N,N-dimethylformamide into a reaction kettle and disperse them evenly. Add 1 g of succinic anhydride and react at room temperature for 6 h under stirring. Wash with water and dry to obtain modified silica.

[0052] Comparative Example 3 A method for preparing a modified epoxy resin adhesive comprises the following steps:

[0053] A1: 10 g of the modified silica prepared in Comparative Example 1, 2 g of 1-thioglycerol, 100 mL of tetrahydrofuran, and 1 mL of deionized water were added to a reaction kettle and dispersed evenly, 3 g of magnesium sulfate was added, and the mixture was reacted at room temperature for 24 h under stirring, filtered, and rotary evaporated to obtain mercapto silica;

[0054] A2: Add 5 g of mercaptosilicon dioxide, 2 g of 1,8-diazabicycloundec-7-ene, and 100 g of bisphenol A epoxy resin (epoxy resin with the brand name CYD-127 produced by Baling Petrochemical Branch of Sinopec Asset Management Company) into a reaction bottle, place it in a vacuum drying oven for degassing, and then control the temperature in the drying oven to 70°C for 3 h and control the temperature to 150°C for 1 h to obtain an adhesive.

[0055] Comparative Example 4 A method for preparing a modified epoxy resin adhesive comprises the following steps:

[0056] A1: 10 g of the modified silica prepared in Comparative Example 1 and 2 g of 1-thioglycerol were mixed to form a modifier;

[0057] A2: Add 5g of modifier, 2g of 1,8-diazabicycloundec-7-ene and 100g of bisphenol A epoxy resin (epoxy resin with brand number CYD-127 produced by Baling Petrochemical Branch of Sinopec Asset Management Company) into a reaction bottle, place it in a vacuum drying oven for degassing, and then control the temperature in the drying oven to 70℃ for 3h and control the temperature to 150℃ for 1h to obtain an adhesive.

[0058] Comparative Example 5 A method for preparing a modified epoxy resin adhesive comprises the following steps:

[0059] A1: 10 g of the modified silica prepared in Comparative Example 2, 2 g of 1-thioglycerol, 100 mL of tetrahydrofuran, and 1 mL of deionized water were added to a reaction kettle and dispersed evenly, 3 g of magnesium sulfate was added, and the mixture was reacted at room temperature for 24 h under stirring, filtered, and rotary evaporated to obtain mercapto silica;

[0060] A2: Add 5 g of mercaptosilicon dioxide, 2 g of 1,8-diazabicycloundec-7-ene, and 100 g of bisphenol A epoxy resin (epoxy resin with the brand name CYD-127 produced by Baling Petrochemical Branch of Sinopec Asset Management Company) into a reaction bottle, place it in a vacuum drying oven for degassing, and then control the temperature in the drying oven to 70°C for 3 h and control the temperature to 150°C for 1 h to obtain an adhesive.

[0061] Performance Testing

[0062] (1) Impact strength: tested according to GB / T 2571-2021 “Impact test method for resin castings”, using an impact testing machine for testing. The test results are shown in Table 1;

[0063] (2) Shear strength: The test was conducted according to GB / T 7124-2008 “Test method for tensile shear strength of adhesives (metal to metal)” using a CMT6303 universal testing machine (tensile speed 5 mm / min). The test results are shown in Table 1.

[0064] (3) Water resistance: The water resistance of the adhesive films prepared in Examples 4-6 and Comparative Examples 3-5 was tested by immersion method. The prepared samples were dried naturally at room temperature, dried in a dryer at 60°C until constant weight was measured as m1, and the dried samples were immersed in deionized water at 22°C for 48 hours. The surface moisture of the immersed samples was absorbed and the weight was measured as m2. The water absorption rate η was calculated according to the following formula:

[0065] η=[(m2-m1) / m1]×100%

[0066] In the formula, η-water absorption rate, %; m1-weight of the sample when dry, mg; m1-weight of the sample after immersion in water, mg; the test results are shown in Table 1;

[0067] Table 1: Statistical table of performance test data of Examples 4-6 and Comparative Examples 3-5

[0068]

[0069] As can be seen from Table 1, the adhesives prepared in Examples 4-6 of the present application have good toughness and mechanical properties, and have excellent water resistance.

[0070] (4) T-peel strength: The test was conducted in accordance with GB / T 2791-1995 “Adhesive T-peel strength test method - Flexible material to flexible material”. The peel strength obtained by performing a single bonding-peel test was recorded as S1. The peeled adhesive was subjected to a continuous bonding-peel test, which was repeated 20 times. The peel strength obtained by performing 20 repeated bonding-peel strength tests was recorded as S20. The test results are shown in Table 2.

[0071] Table 2: Statistical table of bonding performance test data of Examples 4-6 and Comparative Examples 3-5

[0072]

[0073] As can be seen from Table 1, the adhesives prepared in Examples 4 to 6 of the present application have excellent bonding strength to the substrate, and still maintain a relatively high bonding strength after multiple peeling-bonding cycles.

[0074] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.

Claims

1. A method for preparing a modified epoxy resin adhesive, characterized in that: The steps include: A1: Add modified silica, 1-thioglycerol, tetrahydrofuran and deionized water into a reaction kettle and disperse them evenly, add magnesium sulfate, react at room temperature for 24-30 hours under stirring conditions, filter and rotary evaporate to obtain mercapto silica; A2: Add mercapto silicon dioxide, 1,8-diazabicycloundec-7-ene and epoxy resin into a reaction bottle, place in a vacuum drying oven for degassing, and then perform curing treatment in the drying oven to obtain an adhesive; The preparation method of the modified silicon dioxide comprises the following steps: S1: Add γ-aminopropyltriethoxysilane and deionized water component 1 to a reaction bottle, adjust the pH to 3-4, and obtain solution A; disperse nano-silicon dioxide, deionized water component 2, and anhydrous ethanol evenly to obtain solution B; add solution B to solution A, control the temperature to 50-60°C, keep warm for 3-6 hours under stirring conditions, centrifuge, filter, wash, and dry to obtain component 1; S2: Add component 1 and N,N-dimethylformamide into a reaction kettle and disperse them evenly, add succinic anhydride, react at room temperature for 6-9 hours under stirring, wash with water, and dry to obtain component 2; S3: In a nitrogen atmosphere, aminomethylboronic acid pinacol ester hydrochloride, component 2, 2-(1H-benzotriazo L-1-yl)-1,1,3,3-tetramethyluronium tetrafluoroborate and N,N-dimethylformamide are added to a reaction bottle, the temperature is controlled at -20 to 0°C, the reaction is kept warm for 1-3 hours, N,N-diisopropylamine is added, the reaction is kept warm for 1-3 hours, the solvent is removed in vacuo, washed and dried to obtain modified silica.

2. The method for preparing a modified epoxy resin adhesive according to claim 1, characterized in that: The addition ratio of modified silica, 1-thioglycerol, tetrahydrofuran, deionized water, and magnesium sulfate in A1 is 10 g: 2-4 g: 100-200 mL: 0.5-1 mL: 3-7 g.

3. The method for preparing a modified epoxy resin adhesive according to claim 1, characterized in that: The mass ratio of mercapto silicon dioxide, 1,8-diazabicycloundec-7-ene and epoxy resin in A2 is 1-10:0.5-2:

100.

4. The method for preparing a modified epoxy resin adhesive according to claim 1, characterized in that: The specific steps of the curing treatment in A2 are: controlling the temperature to 70-90°C for 1-3 hours, and controlling the temperature to 120-150°C for 0.5-1 hour.

5. The method for preparing a modified epoxy resin adhesive according to claim 1, characterized in that: The addition ratio of γ-aminopropyltriethoxysilane, deionized water component one, nano silicon dioxide, deionized water component two, and anhydrous ethanol in S1 is 0.1-0.5 g: 2-5 mL: 1 g: 10-50 mL: 10-50 mL.

6. The method for preparing a modified epoxy resin adhesive according to claim 1, characterized in that: The addition ratio of component 1, N,N-dimethylformamide and succinic anhydride in S2 is 1g:30-50mL:0.1-0.3g.

7. The method for preparing a modified epoxy resin adhesive according to claim 1, characterized in that: The addition ratio of aminomethylboronic acid pinacol ester hydrochloride, component two, 2-(1H-benzotriazol L-1-yl)-1,1,3,3-tetramethyluronium tetrafluoroborate, N,N-dimethylformamide, and N,N-diisopropylamine in S3 is 0.4-1g:10g:0.5-1g:10-100mL:0.5-1g.