A copper surface roughening liquid and its preparation method and application

The uneven roughening morphology of the copper surface under the forward and reverse pulse electrodeposition technology was solved by using a copper surface roughening liquid composed of a specific ratio of chloromethylbenzotriazole, carboxylic acid compounds and polyethyleneimine. solve the problem, achieve high adhesion and uniform appearance between the copper surface and the solder mask ink, and ensure the product quality of the printed circuit board.

CN118308728BActive Publication Date: 2024-10-11ZHUHAI BANMING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410277473.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-12
Publication Date
2024-10-11
Estimated Expiration
2044-03-12

AI Technical Summary

Technical Problem

When using forward and reverse pulse electrodeposition technology for copper plating, there is a large difference between the high potential area of ​​the orifice and the copper crystals deposited on the surface, resulting in changes in the roughened morphology of the copper surface, making it difficult to form a uniform roughened morphology, affecting the copper layer and the The adhesion of dielectric polymer materials leads to product color difference and failure.

Method used

A specific ratio of chloromethylbenzotriazole, carboxylic acid compounds and polyethyleneimine is used as a roughening agent, combined with copper ions, chloride ions and organic acids to form a grid plus star-like corrosion inhibition layer. , through a specific addition sequence and concentration ratio, a copper surface roughening liquid is prepared, which is used to treat the copper surface after copper plating to form a uniform roughening effect.

Benefits of technology

It achieves a uniform color appearance of the copper surface with no white spots or bright spots, and improves the adhesion between the copper surface and the solder mask ink to meet the needs of subsequent processing and ensure product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004736374080000021
    Figure BDA0004736374080000021
  • Figure BDA0004736374080000031
    Figure BDA0004736374080000031
  • Figure BDA0004736374080000051
    Figure BDA0004736374080000051
Patent Text Reader

Abstract

The present invention belongs to the technical field of printed circuit boards, and provides a copper surface roughening liquid, a preparation method thereof, and an application thereof. The copper surface roughening liquid of the present invention contains a specific concentration of organic acid, copper ions, chloride ions, and a roughening agent, wherein the roughening agent is a combination of chloromethylbenzotriazole, carboxylic acid compounds, and polyethyleneimine in a specific ratio. When the forward and reverse pulse electrodeposition technology is used in the production of communication backplanes, the copper crystals deposited on the surface and the high potential area of ​​the orifice are quite different, resulting in a change in the morphology of the roughening of the copper surface, which makes it difficult to form a roughening or uniform roughening morphology on this part of the copper surface. The copper surface roughening liquid provided by the present invention can be used to roughen the copper surface after pulse electrodeposition copper plating, so that the copper surface forms a uniform roughening effect, meeting the needs of post-processing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of printed circuit boards, and more specifically to a copper surface roughening liquid and a preparation method and application thereof. Background Art

[0002] With the rapid development of electronic information technology, the printed circuit board (PCB) industry has developed rapidly. The communication backplane is the most widely used circuit board in the construction of 5G base stations. Its main function is to carry various functional sub-boards, distribute power to each sub-board and realize the interconnection of signals and electrical connections of each sub-board. The backplane and the sub-boards it carries jointly realize the functions of the system. In order to realize the high-capacity and high-speed transmission of communications and data in 5G base stations, the design of the communication backplane tends to be high-density and high-integration, thereby promoting the development of the backplane in the direction of large size, multi-layer number and small aperture.

[0003] The increase in the number of layers of the communication backplane leads to an increase in the overall thickness of the board, while the aperture of the through hole is constantly decreasing due to the increase in the integration of the backplane, resulting in an increasing thickness-to-diameter ratio of the through holes on the backplane (the ratio of the board thickness to the aperture). Electroplating copper is a key technology for achieving through-hole interconnection. For through holes with a high aspect ratio, the current density at the center of the hole during the electroplating process will be much lower than the current density at the hole mouth, which often leads to a large difference in the plating thickness between the hole center and the hole mouth, making it difficult to achieve good interconnection of the through holes; the thickness-to-diameter ratio of the communication backplane through holes continues to increase, making it increasingly difficult to achieve uniform electroplating of copper in the through holes.

[0004] In the past, direct current electrodeposition was the main method for depositing copper in through-holes. However, for through-holes with a high aspect ratio of more than 10:1, direct current deposition often failed to produce uniform coatings. Subsequently, pulse electrodeposition technology emerged and was introduced into the production of printed circuit boards (PCBs). It was found that the use of forward and reverse pulse electrodeposition technology could significantly increase the thickness of the copper layer in the hole and improve the quality of the coating. It showed great superiority in obtaining functional coatings and saving precious metals, which greatly promoted the application of forward and reverse pulse electrodeposition technology in the printed circuit industry. However, while copper plating using forward and reverse pulse electrodeposition technology improves the thickness of copper in the hole, due to the change in the deposition method, it also leads to some subsequent processing problems that need to be improved.

[0005] The bonding reliability between the conductor copper layer and the dielectric polymer material on the PCB is one of the main manifestations of the key performance and reliability of the circuit board. At present, in the PCB manufacturing process, chemical roughening (roughening liquid treatment) of the copper layer is a common method to improve the adhesion between copper and dielectric polymer (resist plating ink and solder resist ink).

[0006] The mechanism of the existing roughening liquid to treat the copper layer is to form a uniform roughening morphology on the copper surface through the difference in micro-etching rate between different crystal directions and between crystals. However, when the forward and reverse pulse electrodeposition technology is used in PCB production, there is often a large difference between the copper crystals deposited on the surface and the high potential area of ​​the orifice. The difference in the crystal structure of the copper surface causes the morphological changes of the roughening of the copper surface, which makes it difficult to form roughening or uniform roughening morphology on the copper surface in these areas. After printing the solder mask ink, color difference occurs on the PCB surface, resulting in unqualified products. In current production, high-temperature baking is generally performed after electroplating to recrystallize the deposited copper layer crystals, so as to improve the roughening effect. However, high-temperature baking will increase production time and production costs, and in many cases baking cannot completely solve such problems.

[0007] Therefore, it is urgent to develop a method to improve the morphological changes of copper surface roughening, so as to solve the problem that when copper is plated using forward and reverse pulse electrodeposition technology, the morphological changes of the copper surface are caused by the large difference between the high potential area of ​​the hole mouth and the copper crystals deposited on the surface, which makes it difficult to form roughening or uniform roughening morphology on this part of the copper surface. Summary of the invention

[0008] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a copper surface roughening liquid and a preparation method and application thereof. The copper surface roughening liquid provided by the present invention can be used to treat a copper surface, especially a copper-plated surface by forward and reverse pulse electrodeposition, so that the appearance of the copper surface is uniform in color, free of white spots and bright spots, and the copper surface has high adhesion to the solder resist ink.

[0009] A first aspect of the present invention provides a copper surface roughening solution.

[0010] Specifically, a copper surface roughening solution includes the following components according to the concentration of the components:

[0011]

[0012] The roughening agent is a combination of chloromethylbenzotriazole, a carboxylic acid compound and polyethyleneimine, and the weight ratio of the three components is 1:(0.5-2):(3-8) respectively.

[0013] The roughening agent of the copper surface roughening liquid of the present invention adopts a combination of chloromethylbenzotriazole, carboxylic acid compounds and polyethyleneimine in a specific ratio, and utilizes the different corrosion inhibition properties of chloromethylbenzotriazole and carboxylic acid compounds. In addition, under the enhanced adsorption and dispersion effect of polyethyleneimine, the roughening agent can form a grid-plus-star-shaped corrosion inhibition layer on the copper surface, and cooperates with the copper corrosion effect of copper ions, chloride ions and organic acids in a specific concentration in the roughening liquid, so as to finally form an ideal copper roughening surface.

[0014] Preferably, the weight ratio of the three components in the roughening agent is 1:(0.5-1.5):(4-6) in sequence.

[0015] Further preferably, the weight ratio of the three components in the roughening agent is 1:(1-1.5):(5-6) respectively.

[0016] Preferably, the carboxylic acid compound is selected from carboxylic acid compounds having a molecular structure as shown in the following formula (I):

[0017]

[0018] Preferably, the weight average molecular weight of the polyethyleneimine is 1000-10000.

[0019] Preferably, the organic acid includes at least one of formic acid, acetic acid, propionic acid, butyric acid and valeric acid.

[0020] Preferably, the copper ions are provided by a divalent copper compound.

[0021] Preferably, the divalent copper compound is copper chloride and / or copper oxide.

[0022] Preferably, the chloride ions are provided by a soluble chloride salt.

[0023] Preferably, the soluble chloride salt is at least one of sodium chloride, potassium chloride, ammonium chloride and copper chloride.

[0024] Preferably, the copper surface roughening solution also includes water.

[0025] A second aspect of the present invention provides a method for preparing a copper surface roughening solution.

[0026] A method for preparing a copper surface roughening solution comprises the following steps:

[0027] The organic acid and water are mixed, and a divalent copper compound, a soluble chloride salt, chloromethylbenzotriazole, a carboxylic acid compound, and polyethyleneimine are added in sequence and mixed to obtain the copper surface roughening solution.

[0028] The present invention adds chloromethylbenzotriazole, carboxylic acid compounds and polyethyleneimine in sequence, which can stabilize the adsorption capacity of the roughening agent on the copper surface. Changing the addition sequence may lead to uneven adsorption of the roughening agent, thereby causing uneven roughening effect.

[0029] A third aspect of the present invention provides an application of a copper surface roughening liquid.

[0030] The invention discloses an application of a copper surface roughening liquid in the preparation of a printed circuit board.

[0031] A method for using a copper surface roughening liquid comprises the following steps:

[0032] The copper-plated communication backplane is degreased, washed with water, roughened with the copper surface roughening liquid, washed with water, pickled, and dried.

[0033] Preferably, the copper surface roughening liquid is roughened by spraying it up and down using a horizontal conveying device.

[0034] Preferably, the roughening temperature is 25-35° C., and / or the roughening time is 30-90 s, and / or the spraying pressure is 15-25 PSI.

[0035] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0036] The present invention provides a copper surface roughening liquid, which contains organic acid, copper ions, chloride ions, and a roughening agent at a specific concentration, wherein the roughening agent is a combination of chloromethylbenzotriazole, carboxylic acid compounds, and polyethyleneimine in a specific ratio. When the forward and reverse pulse electrodeposition technology is used in the production of communication backplanes, the copper crystals deposited on the surface and the high potential area of ​​the orifice are quite different, resulting in a change in the morphology of the roughening of the copper surface, which makes it difficult to form a roughening or uniform roughening morphology on this part of the copper surface. The copper surface roughening liquid provided by the present invention can be used to roughen the copper surface after pulse electrodeposition copper plating. The composite roughening agent in the copper surface roughening liquid is combined with the interaction of organic acid, copper ions, and chloride ions of appropriate concentrations in the system to form a uniform roughening effect on the copper surface, meeting the needs of post-processing. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a scanning electron microscope image (SEM) of the copper surface after being treated with the copper surface roughening solution of Example 1 of the present invention;

[0038] Figure 2 This is a scanning electron microscope image of the copper surface after being treated with the copper surface roughening liquid in Comparative Example 1. DETAILED DESCRIPTION

[0039] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0040] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0041] Example 1

[0042] A copper surface roughening solution includes the components shown in Table 1.

[0043] The method for preparing the copper surface roughening solution comprises the following steps:

[0044] (1) Add formic acid into water, stir and dissolve, and mix well;

[0045] (2) adding copper oxide to the solution obtained in step (1), stirring to dissolve, and mixing evenly;

[0046] (3) adding potassium chloride to the solution obtained in step (2), stirring to dissolve, and mixing evenly;

[0047] (4) adding chloromethylbenzotriazole, a carboxylic acid compound, and polyethyleneimine (weight average molecular weight 5000) in a weight ratio of 1:1:5 to the solution obtained in step (3), stirring to dissolve, and mixing evenly;

[0048] (5) Add pure water to the standard volume and mix well to obtain a copper surface roughening liquid for a communication backplane.

[0049] Embodiment 2-9

[0050] The copper surface roughening solution of Examples 2-9 is different from that of Example 1 in that the concentrations of the components are different, as shown in Table 1.

[0051] Example 10

[0052] A copper surface roughening solution, comprising the following components according to the concentration of the components:

[0053]

[0054] The roughening agent is a combination of chloromethylbenzotriazole, a carboxylic acid compound and polyethyleneimine in a weight ratio of 1:1:5.

[0055] The method for preparing the copper surface roughening solution comprises the following steps:

[0056] (1) Add acetic acid to an appropriate amount of water, stir and dissolve, and mix well;

[0057] (2) adding copper chloride to the solution obtained in step (1), stirring to dissolve, and mixing evenly;

[0058] (3) adding sodium chloride to the solution obtained in step (2), stirring to dissolve, and mixing evenly;

[0059] (4) adding chloromethylbenzotriazole, a carboxylic acid compound, and polyethyleneimine (weight average molecular weight 5000) in a weight ratio of 1:1:5 to the solution obtained in step (3), stirring to dissolve, and mixing evenly;

[0060] (5) Add pure water to the standard volume and mix well to obtain a copper surface roughening liquid for a communication backplane.

[0061] Comparative Example 1

[0062] This comparative example provides a copper surface roughening solution, which is different from Example 1 in that the weight ratio of chloromethylbenzotriazole, carboxylic acid compound and polyethyleneimine is replaced with 1:1:10.

[0063] Comparative Examples 2-9

[0064] The copper surface roughening solution of Comparative Examples 2-9 is different from that of Example 1 in that the concentrations of the components are different, as shown in Table 1.

[0065] Comparative Example 10

[0066] This comparative example provides a copper surface roughening solution, which is different from Example 1 in that chloromethylbenzotriazole is replaced by an equal amount of 4-methylbenzotriazole.

[0067] Comparative Example 11

[0068] This comparative example provides a copper surface roughening solution, which is different from Example 1 in that the carboxylic acid compound is replaced by an equal amount of lactic acid.

[0069] Comparative Example 12

[0070] This comparative example provides a copper surface roughening solution, which is different from Example 1 in that the preparation method is different. Specifically, step (4) of Example 1 is replaced by: adding chloromethylbenzotriazole, carboxylic acid compound, and polyethyleneimine to the solution obtained in step (3), stirring to dissolve, and mixing evenly.

[0071] Table 1 Components and concentrations in various examples and comparative examples

[0072] Organic acid g / L Copper ion g / L Chloride ion g / L Roughening agent g / L Example 1 70 30 50 5 Example 2 40 30 50 5 Example 3 100 30 50 5 Example 4 70 10 50 5 Example 5 70 50 50 5 Example 6 70 30 20 5 Example 7 70 30 80 5 Example 8 70 30 50 1 Example 9 70 30 50 10 Example 10 70 30 50 5 Comparative Example 1 70 30 50 5 Comparative Example 2 20 30 50 5 Comparative Example 3 200 30 50 5 Comparative Example 4 70 0 50 5 Comparative Example 5 70 60 50 5 Comparative Example 6 70 30 5 5 Comparative Example 7 70 30 100 5 Comparative Example 8 70 30 50 0.1 Comparative Example 9 70 30 50 30 Comparative Example 10 70 30 50 5 Comparative Example 11 70 30 50 5 Comparative Example 12 70 30 50 5

[0073] Application Examples

[0074] The communication backplane after copper electroplating using the forward and reverse pulse electrodeposition technology is treated according to the following process: degreasing→water washing→roughening→water washing→pickling→drying, wherein the copper surface roughening liquid prepared in the above embodiments and comparative examples is respectively used for roughening, and the roughening uses a horizontal conveyor equipment up and down spraying method, the use temperature of the copper surface roughening liquid is 30°C, the time is 60s, and the spraying pressure is 20PSI; the degreasing is 5% BTH-2072 acidic cleaning agent solution, the time is 60s; the pickling uses 5% hydrochloric acid solution, the time is 30s; the drying temperature is 85°C, and the time is 60s.

[0075] Figure 1 and Figure 2 The following are scanning electron microscope images (SEM) of the copper surface treated by the copper surface roughening solution of Example 1 and Comparative Example 1 using the method of the above application example. By comparison, it can be seen that: Figure 1 The copper surface treated in Example 1 is more uniform.

[0076] Product effect testing

[0077] 1. Test method:

[0078] (1) Micro-etching amount detection: A 100 mm × 100 mm double-sided copper-clad laminate is passed through a horizontal spray device according to the process of the embodiment. The weight change of the copper product before and after is measured, and the thickness of the copper layer etched away is calculated as the micro-etching amount. The micro-etching amount is preferably controlled between 0.8-1.2 μm;

[0079] (2) Surface appearance: Observe the treated copper surface under a 10x magnifying glass. If the surface color is uniform, without white spots or bright spots, it is qualified; otherwise, it is unqualified.

[0080] (3) Adhesion test: Coat the roughened communication backplane with a thickness of 25 μm solder mask ink, pre-bake at 80°C for 3 hours, and then bake at 155°C for 1 hour to complete the curing. Use 3M brand 600 series tape to perform adhesion test on the edge of solder mask ink in the hole ring area. Repeat the test three times in the same area. If there is no solder mask ink torn off the tape, it is qualified, otherwise it is unqualified.

[0081] 2. Test results

[0082] Table 2 Application test results of the copper surface roughening solution prepared in each embodiment and comparative example

[0083]

[0084]

[0085] It can be seen from the results in the above table that the appearance of the copper surface treated with the copper surface roughening liquid provided in Examples 1-10 of the present invention is qualified, and the bonding strength test results are all qualified, that is, a copper surface with uniform appearance color, no white spots, and no bright spots is obtained, and the adhesion between the copper surface and the solder mask ink is high.

[0086] The copper surface roughening liquid of Comparative Example 1 changes the component ratio of the roughening agent and increases the amount of polyethyleneimine, resulting in decreased adhesion between the copper surface and the solder resist ink.

[0087] The copper surface roughening solution of Comparative Example 2 reduces the concentration of organic acid, resulting in unqualified copper surface appearance and adhesion between the copper surface and the solder resist ink. The copper surface roughening solution of Comparative Example 3 increases the concentration of organic acid, resulting in decreased adhesion between the copper surface and the solder resist ink, and a large amount of micro-etching. The copper surface roughening solution of Comparative Example 4 does not contain copper ions, and the copper surface roughening solution of Comparative Example 5 increases the concentration of copper ions, both of which result in unqualified copper surface appearance and adhesion tests between the copper surface and the solder resist ink. Comparative Example 6 reduces the concentration of chloride ions, resulting in unqualified copper surface appearance, copper surface and adhesion tests between the solder resist ink. Comparative Example 7 increases the concentration of chloride ions, resulting in decreased adhesion between the copper surface and the solder resist ink, and a large amount of micro-etching. Comparative Example 8 reduces the concentration of the roughening agent, resulting in a large amount of micro-etching, and Comparative Example 9 increases the concentration of the roughening agent. Comparative Examples 8 and 9 both result in unqualified copper surface appearance, copper surface and adhesion tests between the solder resist ink. The above results show that the present invention utilizes organic acid, copper ions, chloride ions and roughening agent in a specific concentration, which can make the components fully exert their synergistic effect, improve the appearance of the copper surface after roughening treatment, and improve the adhesion between the copper surface and the solder mask ink.

[0088] In Comparative Example 10, chloromethylbenzotriazole in the roughening agent is replaced with 4-methylbenzotriazole. Since the electron-withdrawing property of the chlorine substituent changes the adsorption capacity of the benzotriazole compound, the adsorption property of chloromethylbenzotriazole is more suitable for cooperation with other components of the copper surface roughening solution of the present invention to form an ideal corrosion inhibition layer. However, the copper surface roughening solution of Comparative Example 10 loses the effect of chloride ions, resulting in the appearance of the treated copper surface and the adhesion test of the copper surface and the solder mask ink failing.

[0089] In Comparative Example 11, the carboxylic acid compound in the roughening agent is replaced with lactic acid. Since the required grid-shaped and dot-shaped anti-corrosion layer cannot be formed on the copper surface in advance, the appearance of the copper surface after roughening and the adhesion test of the copper surface and the solder mask ink are unqualified, and the amount of micro-etching is large.

[0090] Since the comparative example 12 was not carried out according to a specific order of adding materials, the appearance and bonding strength tests of the copper surface after the roughening treatment were both unqualified.

Claims

1. A copper surface roughening solution, characterized in that: According to the concentration of the components, the following components are included: Organic acid 40-100g / L, Copper ion 10-50g / L, Chloride ion 20-80g / L, Roughening agent 1.0-10g / L; The roughening agent is a combination of chloromethylbenzotriazole, a carboxylic acid compound, and polyethyleneimine, and the weight ratio of the three components is 1: (0.5-2): (3-8); The carboxylic acid compound is selected from carboxylic acid compounds having a molecular structure as shown in the following formula (I): Formula (I); The copper surface roughening solution is prepared by the following preparation method: Mixing an organic acid and water, and sequentially adding a divalent copper compound, a soluble chloride salt, chloromethylbenzotriazole, a carboxylic acid compound, and polyethyleneimine, and mixing to obtain the copper surface roughening solution; The copper ions are provided by divalent copper compounds; and the chloride ions are provided by soluble chloride salts.

2. The copper surface roughening solution according to claim 1, characterized in that: The weight ratios of the three components in the roughening agent are 1:(0.5-1.5):(4-6) respectively.

3. The copper surface roughening solution according to claim 1, characterized in that: The weight average molecular weight of the polyethyleneimine is 1000-10000.

4. The copper surface roughening solution according to claim 1, characterized in that: The organic acid includes at least one of formic acid, acetic acid, propionic acid, butyric acid and valeric acid.

5. The method for preparing the copper surface roughening solution according to any one of claims 1 to 4, characterized in that: The steps include: The organic acid and water are mixed, and a divalent copper compound, a soluble chloride salt, chloromethylbenzotriazole, a carboxylic acid compound, and polyethyleneimine are added in sequence and mixed to obtain the copper surface roughening solution.

6. Use of the copper surface roughening solution according to any one of claims 1 to 4 in the preparation of printed circuit boards.

7. The method for using the copper surface roughening solution according to any one of claims 1 to 4, comprising the following steps: The copper-plated communication backplane is degreased, washed with water, roughened with the copper surface roughening liquid, washed with water, pickled, and dried.