Electroplating process method for stainless steel part

Through electrochemical polishing and ultrasonic cleaning, the problem of insufficient binding force of the surface oxide layer removal and plating of stainless steel welding products is solved, and efficient electroplating treatment is achieved, the gloss and binding force of the coating is improved, and the salt spray corrosion resistance is significantly improved.

CN118932448APending Publication Date: 2024-11-12GUIZHOU ZHENHUA HUALIAN ELECTRONICS
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410998287.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to effectively remove the dense oxide layer on the surface of stainless steel welded products, and the coating bonding force after electroplating is insufficient, it is easy to bubble and delaminate, and it is not resistant to salt spray corrosion, and the product functional characteristics change significantly.

Method used

The stainless steel parts are electroplating by electrochemical polishing, ultrasonic cleaning and pre-plating processes, including electrochemical polishing to remove oxide scales, ultrasonic cleaning to remove deep hole electrochemically dissolve slag, pre-plating of high-chlorine nickel and copper plating to form a uniform plating layer.

Benefits of technology

The oxidation scale is completely removed, the coating has high bonding force and gloss, the coating qualification rate reaches more than 95%, the salt spray corrosion resistance time exceeds 96 hours, and the product performance remains stable.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an electroplating process method of a stainless steel part, which comprises the following steps: hanging the stainless steel part, then carrying out ultrasonic oil removal, carrying out electrochemical polishing after cleaning, and then washing with water; carrying out ultrasonic cleaning, activating, washing with water, then carrying out a high chlorine nickel pre-plating process, carrying out copper pre-plating after washing with water, and then carrying out washing, neutralizing and washing processes; and the procedures of semi-bright nickel plating and bright nickel plating are conducted, the procedure of ultrasonic hot water washing is conducted after water washing is conducted, and finally drying is conducted. The method for removing the oxide skin through electrochemical anode dissolution under the stable pressure condition is efficient and rapid, the efficiency of removing the oxide skin compared with a conventional chemical oxide skin removing method is improved, and the oxide layer is thoroughly removed. Through an electrochemical anodic dissolution method, oxide skin of cracks, deep holes and grooves of the part can be well removed, and the uniformity and binding force of a plating layer are high. The influence on the size of the part is small, and the performance characteristics of the part are guaranteed through the size change at the micron level.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electroplating technology, and in particular relates to an electroplating process method for stainless steel parts. Background Art

[0002] With the development of society, the application field of stainless steel materials is becoming wider and wider. In order to realize the application field of stainless steel products, it is necessary to give stainless steel materials products special properties, and the demand for electroplating is becoming more and more extensive. At present, there are many processes for electroplating of stainless steel materials, but there are basically no processes and methods for electroplating of stainless steel welding products. The technical problems that need to be solved include: 1. The removal technology of the black and dense oxide layer formed by welding of stainless steel; 2. The coating bonding strength of the parts is good through treatment, and there is no blistering and delamination; 3. The salt spray treatment of the product can achieve rust-free for more than 96 hours; 4. After electroplating, the functional characteristics of the product do not change significantly.

[0003] The patent document with publication number CN109440152A discloses an iron embryo electroplating process, and discloses a process flow of electroplating using nickel sulfate, nickel chloride, and boric acid. However, this process is used for electroplating iron embryos, which is different from the stainless steel material to be processed in this application; and the technical problem to be solved is: avoiding the generation of highly toxic hydrogen cyanide gas during the use of cyanide and reducing the discharge of wastewater and waste gas, while the technical problem to be solved in this application is to increase the performance of the coating.

[0004] The patent document with publication number CN111270278A discloses a stainless steel electroplating gold process and its processing technology and application, providing pre-treatment: electrolytic degreasing of stainless steel; electroplating of acidic bottom gold layer; electroplating of 18K gold layer; electroplating of 23K gold layer; anti-discoloration passivation coating treatment. The electroplating materials and methods used in this process are different from the process methods used in this application.

[0005] The patent document with the publication number CN109338432A discloses an electroplating process for stainless steel and aluminum alloy composite parts: pre-treat the composite parts to expose the clean and active substrate; use the pre-treated composite parts as anodes and metal nickel as cathodes to pre-oxidize in a pre-nickel plating tank to activate the stainless steel part of the composite parts and anodize the aluminum alloy part to produce micropores; exchange the cathode and anode of the pre-nickel plating tank, and pre-plate in the pre-nickel plating tank to activate the nickel layer on the stainless steel surface. The principle is similar to that of this patent, but the electroplating materials and methods used are different from the process methods used in this patent, and the operation time is longer. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides an electroplating process method for stainless steel parts.

[0007] The present invention is achieved through the following technical solutions.

[0008] The present invention provides a stainless steel electroplating process method, which comprises a process of electroplating the stainless steel part through hanging, electrochemical polishing, ultrasonic cleaning and pre-plating procedures.

[0009] A stainless steel electroplating process comprises the following steps:

[0010] S1: Hang the stainless steel parts, then perform ultrasonic degreasing, perform electrochemical polishing after cleaning, and then wash with water.

[0011] S2: ultrasonically clean the stainless steel parts after step S1, and then perform a high-chlorine nickel pre-plating process after activation and water washing, and then perform a copper pre-plating process after water washing, and then perform water washing, neutralization, and water washing processes.

[0012] S3: The stainless steel parts after step S2 are subjected to semi-bright nickel plating and bright nickel plating processes, and then subjected to ultrasonic hot water washing process after water washing, and finally dried.

[0013] Preferably, the ultrasonic cleaning comprises the following steps: the cleaning solution is water, and the cleaning is performed for 3-5 minutes at an ultrasonic frequency of 20-35 Hz.

[0014] Preferably, the electrochemical polishing is an electrochemical anode dissolution and polishing process, and the steps include hanging the stainless steel part on the anode rod as the anode and hanging the lead plate on the cathode rod as the cathode in the electrochemical polishing process.

[0015] Preferably, the electrochemical polishing step comprises: placing the stainless steel part in an electrolyte containing 50-70V% phosphoric acid and 40-20V% sulfuric acid at a temperature of 50-80°C, setting the DC rectifier to a voltage-stabilizing state, and maintaining the voltage at 11-12V for 2-9S.

[0016] Preferably, the electrochemical polishing step includes: first adding phosphoric acid and sulfuric acid in the polishing process tank, then adding 3-5v% of additives, using a lead plate as a cathode, heating to 50-80°C, and after heating to the temperature, using a stainless steel part as an anode, and continuing for 2-9S at a voltage stabilized at 11-12V.

[0017] Preferably, the pre-plating process is a high-chloride nickel pre-plating process, and the steps include: using 130-300 g / L nickel chloride, analytical pure hydrochloric acid solution, under steady flow conditions, with the stainless steel part as the cathode and the nickel plate as the anode, for 2-9 minutes.

[0018] Preferably, the solution using analytically pure hydrochloric acid is 100-200 mL / L.

[0019] Preferably, the pre-plating process is a high-chloride nickel pre-plating process, and the steps include: the solution preparation method is to add 1 / 4 pure water to the pre-plating process tank, add analytical pure hydrochloric acid, then dissolve the nickel chloride and add it to the process tank, stir and perform electroplating at a temperature of 20-30°C in a steady flow manner.

[0020] Preferably, the conductivity of pure water is ≤10us / cm.

[0021] The beneficial effects of the present invention are:

[0022] 1. The present invention adopts the method of removing oxide scale by electrochemical anodic dissolution under constant voltage conditions, which is efficient and fast. The conventional chemical oxide scale removal efficiency time is 20-30min, and the electrochemical polishing of the present application can be completed within 20S, which is more than 95% shorter than the conventional chemical oxide scale removal efficiency time, and the oxide layer is completely removed.

[0023] 2. The patented method of the present invention can improve the glossiness of the substrate to a certain extent, and the coating of the parts is bright after electroplating.

[0024] 3. The present invention uses the method of electrochemical anodic dissolution to effectively remove the oxide scale in the gaps, deep holes and grooves of parts, and the coating uniformity and bonding strength are high.

[0025] 4. Through the method of ultrasonic cleaning, the slag particles produced by electrochemical dissolution of deep holes and cavities of parts can be removed, ensuring the uniformity of the coating without particles.

[0026] 5. The coating of the present invention has excellent bonding strength, no delamination or blistering, a coating pass rate of more than 95%, and high coating brightness.

[0027] 6. The patent of this invention has little impact on the size of parts, and the size changes at the um level ensure the performance characteristics of the parts. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further described below, but the scope of protection claimed is not limited to the description.

[0029] Embodiment 1:

[0030] A stainless steel electroplating process comprises the following steps:

[0031] S1: Hang the stainless steel parts, then perform ultrasonic degreasing, perform electrochemical polishing after cleaning, and then wash with water;

[0032] S2: ultrasonically clean the stainless steel parts after step S1, and then perform a high-chlorine nickel pre-plating process after activation and water washing, and then perform a copper pre-plating process after water washing, and then perform water washing, neutralization, and water washing processes after completion;

[0033] S3: The stainless steel parts after step S2 are subjected to semi-bright nickel plating and bright nickel plating processes, and then subjected to ultrasonic hot water washing process after water washing, and finally dried.

[0034] The electrochemical polishing is an electrochemical anode dissolution and polishing process, and the steps include hanging the stainless steel part on the anode rod as the anode and hanging the lead plate on the cathode rod as the cathode.

[0035] The electrochemical polishing step includes: placing the stainless steel part in an electrolyte containing 50V% phosphoric acid and 40V% sulfuric acid, under the condition of temperature of 50°C, setting the DC rectifier to a voltage-stabilizing state, and maintaining the voltage at 11V for 2S, and electrochemically dissolving and polishing the dense oxide layer of the stainless steel part when power is turned on, completing the electrochemical polishing and dissolution of the oxide scale of the stainless steel part, removing the surface oxide layer, and increasing the surface finish to a certain extent.

[0036] The pre-plating process is a high-chloride nickel pre-plating process, and the steps include: using a solution with a ratio of 130g / L nickel chloride and 100mL / L analytical pure hydrochloric acid, under steady flow conditions, with the stainless steel part as the cathode and the nickel plate as the anode, for 2 minutes.

[0037] The electrochemical polishing steps include: first adding phosphoric acid and sulfuric acid in the polishing process tank, then adding 3v% of additives, the additives include commercially available LD-3360 stainless steel electrolytic polishing agent, using a lead plate as a cathode, heating to 50°C, and after heating to the temperature, using a stainless steel part as an anode, and continuing for 2S at a voltage stabilized at 11V.

[0038] The pre-plating process is a high-chlorine nickel pre-plating process, and the steps include: the solution preparation method is to add 1 / 4 pure water in the pre-plating process tank, the water conductivity is ≤10us / cm, add analytical pure hydrochloric acid, and then dissolve the nickel chloride and add it to the process tank, stir and electroplate at a temperature of 20°C in a steady flow manner. Within 5 minutes after the pre-nickel plating process begins, the color appearance of the stainless steel parts needs to be checked, and it can be a uniform light gray; in this case, the stainless steel parts can be given a strong activation energy to ensure that the coating has good bonding strength.

[0039] The ultrasonic cleaning comprises the following steps: the cleaning solution is water, and the cleaning is performed for 3 minutes at an ultrasonic frequency of 20 Hz, so as to remove particles adsorbed on the surface and holes and cavities, and ensure the uniformity of the appearance quality of the stainless steel parts.

[0040] In the pre-copper plating process, the stainless steel parts are electroplated in a cyanide-containing copper plating solution, using a steady flow method and the time is controlled at 2.6 minutes. A purple-red uniform copper plating layer is formed on the surface of the stainless steel parts, further improving the bonding strength of the plating layer.

[0041] The water washing steps are all to put the stainless steel parts of the corresponding steps into the water tank and soak them for 5S.

[0042] The ultrasonic oil removal step comprises: maintaining the temperature of the water at 50° C. and the frequency at 60 Hz for 5 minutes.

[0043] The activation step includes: treating the stainless steel parts with a solution of hydrochloric acid and water in a ratio of 1:1 at room temperature. When the parts are activated, the hanger moves up and down or left and right for 10 seconds to allow the stainless steel parts to fully contact with the solution, and then enter the next process.

[0044] The pre-copper plating step includes: using a solution prepared with sodium cyanide and cuprous cyanide, with a current of 2A per hanging, and maintaining the temperature at 30°C for 3 minutes, during which the appearance of the stainless steel parts is carefully observed. During the pre-copper plating process of the stainless steel parts, slight bubbles are generated, and the surface is gradually covered with a purple-red copper layer. If the parts generate more bubbles and the coating is red and dark, the current is reduced.

[0045] The neutralization step includes: preparing sulfuric acid and water, a solution with a sulfuric acid concentration of 10%, completely immersing the stainless steel parts, moving the hanger up and down for 5 seconds, and then transferring to the next process after the time is up;

[0046] The semi-bright nickel plating and bright nickel plating steps include: using a solution prepared by 260 g / L nickel sulfate, 25 g / L nickel chloride, 40 g / L boric acid and 300 liters of deionized water, and soaking at a temperature of 50° C. for 5 minutes.

[0047] The ultrasonic hot water washing step includes: placing the stainless steel part in a tank with deionized water, heating it to 70° C., turning on an ultrasonic sounder, and maintaining it at a frequency of 60 Hz for 15 minutes.

[0048] The drying step comprises: blowing the stainless steel part with a high-pressure air gun and then drying it at 70° C. for 5 minutes.

[0049] Embodiment 2:

[0050] A stainless steel electroplating process comprises the following steps:

[0051] S1: Hang the stainless steel parts, then perform ultrasonic degreasing, perform electrochemical polishing after cleaning, and then wash with water;

[0052] S2: ultrasonically clean the stainless steel parts after step S1, and then perform a high-chlorine nickel pre-plating process after activation and water washing, and then perform a copper pre-plating process after water washing, and then perform water washing, neutralization, and water washing processes after completion;

[0053] S3: The stainless steel parts after step S2 are subjected to semi-bright nickel plating and bright nickel plating processes, and then subjected to ultrasonic hot water washing process after water washing, and finally dried.

[0054] The electrochemical polishing is an electrochemical anode dissolution and polishing process, and the steps include hanging the stainless steel part on the anode rod as the anode and hanging the lead plate on the cathode rod as the cathode.

[0055] The electrochemical polishing step includes: placing the stainless steel part in an electrolyte containing 70V% phosphoric acid and 20V% sulfuric acid, under the condition of temperature 80°C, setting the DC rectifier to a voltage-stabilizing state, and maintaining the voltage at 12V for 9S, and electrochemically dissolving and polishing the dense oxide layer of the stainless steel part when power is turned on, completing the electrochemical polishing and dissolution of the oxide scale of the stainless steel part, removing the surface oxide layer, and increasing the surface finish to a certain extent.

[0056] The pre-plating process is a high-chloride nickel pre-plating process, and the steps include: using a solution with a ratio of 300g / L nickel chloride and 200mL / L analytical pure hydrochloric acid, under steady flow conditions, with the stainless steel part as the cathode and the nickel plate as the anode, for 9 minutes.

[0057] The electrochemical polishing steps include: first adding phosphoric acid and sulfuric acid in the polishing process tank, then adding 5v% of additives, the additives include commercially available LD-3360 stainless steel electrolytic polishing agent, using a lead plate as a cathode, heating to 80°C, and after heating to the temperature, using a stainless steel part as an anode, and continuing for 9S at a voltage stabilized at 12V.

[0058] The pre-plating process is a high-chlorine nickel pre-plating process, and the steps include: the solution preparation method is to add 1 / 4 pure water in the pre-plating process tank, the water conductivity is ≤10us / cm, add analytical pure hydrochloric acid, and then dissolve the nickel chloride and add it to the process tank, stir and electroplate at a temperature of 30°C in a steady flow manner. Within 5 minutes after the pre-nickel plating process begins, the color appearance of the stainless steel parts needs to be checked, and it can be a uniform light gray; in this case, the stainless steel parts can be given a strong activation energy to ensure that the coating has good bonding strength.

[0059] The ultrasonic cleaning comprises the following steps: the cleaning solution is water, and the cleaning is performed for 5 minutes at an ultrasonic frequency of 35 Hz, so as to remove particles adsorbed on the surface and holes and cavities, and ensure the uniformity of the appearance quality of the stainless steel parts.

[0060] In the pre-copper plating process, the stainless steel parts are electroplated in a cyanide-containing copper plating solution, using a steady flow method and the time is controlled within 2 minutes. A purple-red uniform copper plating layer is formed on the surface of the stainless steel parts, further improving the bonding strength of the plating layer.

[0061] The water washing steps are all to put the stainless steel parts of the corresponding steps into a water tank and soak them for 10S.

[0062] The ultrasonic degreasing step comprises: maintaining the temperature of the water at 60° C. and the frequency at 60 Hz for 10 minutes.

[0063] The activation step includes: treating the stainless steel parts with a solution of hydrochloric acid and water in a ratio of 1:1 at room temperature. When the parts are activated, the hanger moves up and down or left and right for 15 seconds to allow the stainless steel parts to fully contact with the solution, and then enter the next process.

[0064] The pre-copper plating step includes: using a solution prepared with sodium cyanide and cuprous cyanide, with a current of 3A per hanging, and maintaining a temperature of 40°C for 3 minutes, during which the appearance of the stainless steel parts is carefully observed. During the pre-copper plating process of the stainless steel parts, slight bubbles are generated, and a layer of purple-red copper layer is gradually covered on the surface. If the parts generate more bubbles and the coating is red and dark, the current is reduced.

[0065] The neutralization step includes: preparing sulfuric acid and water, a solution with a sulfuric acid concentration of 10%, completely immersing the stainless steel parts, and moving the hanger up and down for 10 seconds, and then moving to the next process after the time is up;

[0066] The semi-bright nickel plating and bright nickel plating steps include: using a solution prepared by 260 g / L nickel sulfate, 25 g / L nickel chloride, 40 g / L boric acid and 300 liters of deionized water, and soaking at a temperature of 55° C. for 5 minutes.

[0067] The ultrasonic hot water washing step includes: placing the stainless steel part in a tank with deionized water, heating it to 80° C., turning on an ultrasonic sounder, and maintaining it at a frequency of 60 Hz for 15 minutes.

[0068] The drying step comprises: blowing the stainless steel part with a high-pressure air gun and then drying it at 80° C. for 10 minutes.

[0069] Embodiment 3:

[0070] A stainless steel electroplating process comprises the following steps:

[0071] S1: Hang the stainless steel parts, then perform ultrasonic degreasing, perform electrochemical polishing after cleaning, and then wash with water;

[0072] S2: ultrasonically clean the stainless steel parts after step S1, and then perform a high-chlorine nickel pre-plating process after activation and water washing, and then perform a copper pre-plating process after water washing, and then perform water washing, neutralization, and water washing processes after completion;

[0073] S3: The stainless steel parts after step S2 are subjected to semi-bright nickel plating and bright nickel plating processes, and then subjected to ultrasonic hot water washing process after water washing, and finally dried.

[0074] The electrochemical polishing is an electrochemical anode dissolution and polishing process, and the steps include hanging the stainless steel part on the anode rod as the anode and hanging the lead plate on the cathode rod as the cathode.

[0075] The electrochemical polishing step includes: placing the stainless steel part in an electrolyte containing 60V% phosphoric acid and 30V% sulfuric acid, under the condition of temperature of 70°C, setting the DC rectifier to a voltage-stabilizing state, and maintaining the voltage at 11.5V for 6S, and electrochemically dissolving and polishing the dense oxide layer of the stainless steel part when power is turned on, completing the electrochemical polishing and dissolution of the oxide scale of the stainless steel part, removing the surface oxide layer, and increasing the surface finish to a certain extent.

[0076] The pre-plating process is a high-chloride nickel pre-plating process, and the steps include: using a solution with a ratio of 210g / L nickel chloride and 160mL / L analytical pure hydrochloric acid, under steady flow conditions, with the stainless steel part as the cathode and the nickel plate as the anode, for 5 minutes.

[0077] The electrochemical polishing steps include: first adding phosphoric acid and sulfuric acid in the polishing process tank, then adding 4v% of additives, the additives include commercially available LD-3360 stainless steel electrolytic polishing agent, using a lead plate as a cathode, heating to 60°C, and after heating to the temperature, using a stainless steel part as an anode, and continuing for 6S at a voltage stabilized at 11V.

[0078] The pre-plating process is a high-chlorine nickel pre-plating process, and the steps include: the solution preparation method is to add 1 / 4 pure water in the pre-plating process tank, the water conductivity is ≤10us / cm, add analytical pure hydrochloric acid, and then dissolve the nickel chloride and add it to the process tank, stir and electroplate at a temperature of 25°C in a steady flow manner. Within 5 minutes after the start of the pre-nickel plating process, the color appearance of the stainless steel parts needs to be checked, and it can be a uniform light gray; in this case, the stainless steel parts can be given a strong activation energy to ensure that the coating has good bonding strength.

[0079] The ultrasonic cleaning comprises the following steps: the cleaning solution is water, and the cleaning is performed for 4 minutes at an ultrasonic frequency of 30 Hz to remove particles adsorbed on the surface and holes and cavities, thereby ensuring the uniformity of the appearance quality of the stainless steel parts.

[0080] In the pre-copper plating process, the stainless steel parts are electroplated in a cyanide-containing copper plating solution, using a steady flow method and the time is controlled within 2 minutes. A purple-red uniform copper plating layer is formed on the surface of the stainless steel parts, further improving the bonding strength of the plating layer.

[0081] The water washing steps are all to put the stainless steel parts of the corresponding steps into the water tank and soak them for 7S.

[0082] The ultrasonic oil removal step includes: maintaining the temperature of 55° C. in water at a frequency of 60 Hz for 7 minutes.

[0083] The activation step includes: treating the stainless steel parts with a solution of hydrochloric acid and water in a ratio of 1:1 at room temperature. When the parts are activated, the hanger moves up and down or left and right for 12 seconds to allow the stainless steel parts to fully contact with the solution, and then enter the next process.

[0084] The pre-copper plating step includes: using a solution prepared with sodium cyanide and cuprous cyanide, with a current of 2A per hanging, and maintaining the temperature at 35°C for 3 minutes, during which the appearance of the stainless steel parts is carefully observed. During the pre-copper plating process of the stainless steel parts, slight bubbles are generated, and the surface is gradually covered with a purple-red copper layer. If the parts generate more bubbles and the coating is red and dark, the current is reduced.

[0085] The neutralization step includes: preparing sulfuric acid and water, a solution with a sulfuric acid concentration of 10%, completely immersing the stainless steel parts, and moving the hanger up and down for 8 seconds, and then going to the next process after the time is up;

[0086] The semi-bright nickel plating and bright nickel plating steps include: using a solution prepared by 290 g / L nickel sulfate, 30 g / L nickel chloride, 46 g / L boric acid and 300 liters of deionized water, and soaking at a temperature of 53° C. for 5 minutes.

[0087] The ultrasonic hot water washing step includes: placing the stainless steel part in a tank with deionized water, heating it to 76° C., turning on an ultrasonic sounder, and maintaining it at a frequency of 60 Hz for 15 minutes.

[0088] The drying step comprises: blowing the stainless steel part with a high-pressure air gun and then drying it at 75° C. for 8 minutes.

[0089] The same batch of stainless steel parts were electroplated by the processes of Examples 1-3, and the thickness of the coating on the electroplated parts was measured. The average value was obtained by measuring three locations on each electroplated part, and the average value was obtained by measuring three electroplated parts in each example. The electroplated parts were subjected to 10 repeated 90-degree bending tests to observe the coating conditions. The results are shown in the following table.

[0090] Coating thickness(μm) Minimum coating thickness (μm) Coating after bending Example 1 10.24 10.11 No cracking or falling off Example 2 11.05 10.57 No cracking or falling off Example 3 10.89 10.34 No cracking or falling off

[0091] As can be seen from the above table, the coating thickness of the electroplated parts prepared in Examples 1-3 all reached more than 10 μm, and the minimum coating thickness was not less than 10 μm, which met the process production requirements. In addition, the coating was not damaged after bending, and the surface coating had good bonding strength.

Claims

1. A method for electroplating a stainless steel part, characterized in that: It includes the process of electroplating stainless steel parts through hanging, electrochemical polishing, ultrasonic cleaning and pre-plating steps.

2. The electroplating process for stainless steel parts according to claim 1, characterized in that: The following steps are involved: S1: Hang the stainless steel parts, then perform ultrasonic degreasing, perform electrochemical polishing after cleaning, and then wash with water; S2: ultrasonically clean the stainless steel parts after step S1, and then perform a high-chlorine nickel pre-plating process after activation and water washing, and then perform a copper pre-plating process after water washing, and then perform water washing, neutralization, and water washing processes after completion; S3: The stainless steel parts after step S2 are subjected to semi-bright nickel plating and bright nickel plating processes, and then subjected to ultrasonic hot water washing process after water washing, and finally dried.

3. The electroplating process for stainless steel parts according to claim 2, characterized in that: The ultrasonic cleaning comprises the following steps: the cleaning solution is water, and the cleaning is performed for 3-5 minutes at an ultrasonic frequency of 20-35 Hz.

4. The electroplating process for stainless steel parts according to claim 1, characterized in that: The electrochemical polishing is an electrochemical anode dissolution and polishing process, and the steps include hanging the stainless steel part on the anode rod as the anode and hanging the lead plate on the cathode rod as the cathode.

5. The electroplating process for stainless steel parts according to claim 1, characterized in that: The electrochemical polishing step includes: placing the stainless steel part in an electrolyte containing 50-70V% phosphoric acid and 40-20V% sulfuric acid at a temperature of 50-80°C, setting the DC rectifier to a voltage-stabilizing state, and maintaining the voltage at 11-12V for 2-9S.

6. The electroplating process for stainless steel parts according to claim 5, characterized in that: The electrochemical polishing steps include: first adding phosphoric acid and sulfuric acid in the polishing process tank, then adding 3-5v% of additives, using a lead plate as a cathode, heating to 50-80°C, and after heating to the temperature, using a stainless steel part as an anode, and continuing for 2-9S at a voltage stabilized at 11-12V.

7. The electroplating process for stainless steel parts according to claim 1, characterized in that: The pre-plating process is a high-chloride nickel pre-plating process, and the steps include: using 130-300 g / L nickel chloride, analytical pure hydrochloric acid solution, under steady flow conditions, with the stainless steel part as the cathode and the nickel plate as the anode, for 2-9 minutes.

8. The electroplating process for stainless steel parts according to claim 7, characterized in that: The solution used is 100-200 mL / L of analytical pure hydrochloric acid.

9. The electroplating process for stainless steel parts according to claim 7, characterized in that: The pre-plating process is a high-chloride nickel pre-plating process, and the steps include: the solution preparation method is to add 1 / 4 pure water to the pre-plating process tank, add analytical pure hydrochloric acid, then dissolve the nickel chloride and add it to the process tank, stir and perform electroplating at a temperature of 20-30°C in a steady flow manner.

10. The electroplating process for stainless steel parts according to claim 9, characterized in that: The conductivity of pure water is ≤10us / cm.