Graphene terminal ohmic contact electrode diamond nuclear detector and preparation method thereof
By introducing graphene-terminated ohmic contact electrodes and passivation layers into the diamond core detector, the performance problems of the diamond core detector were solved, the charge collection efficiency and response speed were improved, and high-efficiency detection performance was achieved.
Patent Information
- Application Number
- CN202410548931.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-06
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-05-06
AI Technical Summary
Existing diamond nuclear detectors suffer from scattering centers, interface traps, and resistivity effects, resulting in poor charge collection efficiency, energy resolution, and time response characteristics.
A graphene-terminated ohmic contact electrode diamond core detector is formed by setting graphene and metal layers above and below the intrinsic diamond layer and using a passivation layer. The interface is optimized to be a C-C bond. The work function of titanium metal and graphene is matched, and silsesquioxane-modified polyimide is used as the passivation layer.
It improves charge collection efficiency, reduces ohmic contact resistance, enhances device output current and response speed, improves detector sensitivity and yield, and has the capability to operate at high voltage and high current.
Smart Images

Figure CN118315472B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of semiconductor technology, in particular to a graphene terminal ohmic contact electrode diamond nuclear detector and a preparation method thereof. Background Art
[0002] Diamond is widely used in extreme environments due to its advantages such as strong critical breakdown field, high carrier mobility, high thermal conductivity, strong radiation resistance, and large bandgap (5.5eV). Its excellent material properties make it widely used in nuclear energy applications, space exploration, radioactive medicine, dose monitoring and other fields.
[0003] Diamond nuclear detectors interact with diamond materials to form electron-hole pairs when radiation, neutrons, and protons that are larger than the diamond bandgap width are collected by electrodes on both sides to generate electrical signals to monitor radiation, etc. The parameters that affect monitoring efficiency mainly include charge collection efficiency, energy resolution, IV characteristics, and time response characteristics.
[0004] The main factors that affect the performance of diamond detectors are the scattering centers caused by the doping of diamond itself, which affects the time response characteristics and charge collection efficiency; the interface traps generated between diamond and buffer layer and between buffer layer and metal, which affect the charge collection efficiency and IV characteristics; the resistivity of the overall structure of diamond-buffer layer-metal affects the energy resolution efficiency and IV characteristics.
[0005] In order to solve the main factors affecting the performance of diamond detectors, the present invention provides a graphene terminal ohmic contact electrode diamond nuclear detector and a preparation method thereof. Summary of the invention
[0006] In view of the deficiencies in the prior art, the present invention provides a graphene-terminated ohmic contact electrode diamond nuclear detector and a preparation method thereof to solve the problems raised in the above-mentioned background technology.
[0007] To achieve the above-mentioned purpose, the present invention provides the following technical solutions: a graphene-terminated ohmic contact electrode diamond nuclear detector, comprising an intrinsic diamond layer, the intrinsic diamond layer is located in the middle of the nuclear detector device, graphene layers are arranged above and below the intrinsic diamond layer, metal layers are arranged on the surfaces of the graphene layers located on the upper and lower sides of the intrinsic diamond layer, and passivation layers are arranged on the surfaces of the metal layers on both sides, and the passivation layers are located on the surface of the nuclear detector device;
[0008] The nuclear detector uses a graphene layer and a metal layer to form an ohmic contact electrode.
[0009] To further optimize the technical solution, the intrinsic diamond layer is the device radiation area of the nuclear detector, the intrinsic diamond layer is made of intrinsic diamond material, and the thickness of the intrinsic diamond layer is 500-1500nm.
[0010] To further optimize the technical solution, the passivation layer adopts silsesquioxane-modified polyimide, and the preparation method is:
[0011] A1: nitrogen is injected into a stirred reactor, 400-600 parts of N-methyl-pyrrolidone is added, the temperature of the reactor is set to 30-40°C, 10-20 parts of p-phenylenediamine, 0.05-0.5 parts of 1,1'-diaminoferrocene; 0.05-0.5 parts of aminopropylheptyl-cage polysilsesquioxane, and 30-60 parts of pyromellitic dianhydride are added, and the temperature is raised to 40-50°C under a nitrogen atmosphere and heated while stirring for 100-200 minutes to obtain a polyamic acid;
[0012] A2: The polyamic acid is spun at a high speed of 1000-2000 rpm or more to remove bubbles. Then, it is applied to the surface of the metal layer 3 on both sides by a spin coater, and dried for 30-50 minutes at a temperature of 100-130° C. in a nitrogen atmosphere to prepare a gel film, and the temperature of the gel film is raised to 430-480° C. at a rate of 2-5° C. / min, and heat-treated for 60-100 minutes, and then cooled to 30-40° C. at a rate of 2-5° C. / min to obtain a silsesquioxane-modified polyimide.
[0013] To further optimize the technical solution, the metal layer is made of titanium and the thickness of the metal layer is 200-300 nm.
[0014] To further optimize the technical solution, the thickness of the graphene layer is 100-120nm.
[0015] A method for preparing a graphene-terminated ohmic contact electrode diamond nuclear detector is prepared based on the above-mentioned graphene-terminated ohmic contact electrode diamond nuclear detector, comprising the following specific steps:
[0016] S1, growing graphene on the intrinsic diamond layer;
[0017] S2, depositing titanium metal on the intrinsic diamond graphene layer by magnetron sputtering;
[0018] S3, depositing a passivation layer on the titanium metal;
[0019] S4, flip the wafer and repeat steps S1-S3.
[0020] To further optimize the technical solution, in step S1, titanium is used as a catalyst to in-situ grow a graphene layer on the intrinsic diamond layer, and the specific process includes:
[0021] Cleaning the intrinsic diamond surface: Before starting, first use high-purity solvents such as acetone, ethanol and deionized water to thoroughly clean the diamond surface through ultrasonic cleaning to remove organic matter and other contaminants on the diamond surface to ensure the growth quality of graphene;
[0022] Vacuum treatment and placement of titanium metal: The cleaned diamond sample is placed inside the crucible, and the titanium metal sheet is placed on top of it. Then, the entire device is evacuated to 1x10 -7 -5x10 -7 mbar high vacuum environment to exclude air and moisture and reduce the impact of impurities;
[0023] Heating and graphene growth: In a vacuum environment, the heating device is heated to 500°C and maintained for 4 minutes. Under this temperature condition, titanium metal will act as a catalyst to promote the decomposition and recombination of the carbon source on the diamond surface, thereby growing a uniform layer of graphene on the diamond surface;
[0024] Cleaning: After graphene growth is completed, the sample is cleaned with an appropriate solvent at room temperature to remove any unreacted catalyst residues or other impurities that may be present.
[0025] To further optimize the technical solution, in step S4, the wafer is turned over, and then steps S1 to S3 are repeated on the other side of the intrinsic diamond, that is:
[0026] Titanium is used as a catalyst to grow a graphene layer in situ on top of the diamond, and then titanium metal is deposited on the graphene layer by magnetron sputtering. Finally, a passivation layer is deposited on the titanium metal to increase the effective contact area of the detector.
[0027] To further optimize the technical solution, in step S1, the graphene layer is grown in situ by titanium metal catalysis, no foreign material is introduced on the surface of the intrinsic diamond layer, and the interface of the device is CC bond without heterogeneous bonding, so as to ensure low defects at the interface between the intrinsic diamond layer and the graphene layer.
[0028] To further optimize the technical solution, in step S2, the metal layer is deposited using titanium metal, which is the same as the graphene catalytic metal and does not introduce new impurities, thereby ensuring the cleanliness of the processing technology. At the same time, the work functions of titanium metal and graphene are similar, thereby achieving low-resistance contact of the device.
[0029] Compared with the prior art, the present invention provides a graphene terminal ohmic contact electrode diamond nuclear detector and a preparation method thereof, which has the following beneficial effects:
[0030] 1. The graphene-terminated ohmic contact electrode diamond nuclear detector and its preparation method use intrinsic diamond materials with high material quality, no scattering centers, traps and defect energy levels caused by dopants, good internal transport characteristics of the device and high charge collection rate.
[0031] 2. The graphene-terminated ohmic contact electrode diamond nuclear detector and its preparation method use a graphene layer and a metal layer to form an ohmic contact electrode. Since the resistivity of graphene is extremely low, the ohmic contact resistance of the device is small, the output current and gain of the device are high, and the response speed is fast. At the same time, doping is not used to reduce the ohmic contact resistance, which effectively reduces the defect density of the intrinsic diamond to metal electrode part in the device. Therefore, when electron-hole pairs are formed inside the device, they are more easily collected by the electrodes on both sides of the detector, thereby improving the sensitivity of the device.
[0032] 3. The graphene-terminated ohmic contact electrode diamond nuclear detector and its preparation method do not introduce foreign materials on the surface of the intrinsic diamond layer. The interface of the device is a CC bond without heterogeneous bonding, thereby ensuring low defects at the interface between the intrinsic diamond layer and the graphene layer. The metal layer is made of titanium metal, which is the same as the graphene catalytic metal and will not introduce new impurities, which can effectively ensure the cleanliness of the processing technology and improve the yield rate. The work function of titanium metal is similar to that of graphene, which can achieve low-resistance contact of the device, and it has good anti-electromigration characteristics and has high voltage and high current working conditions.
[0033] 4. p-phenylenediamine and pyromellitic anhydride form polyamic acid through polycondensation. In this process, the amino group (-NH2) of p-phenylenediamine reacts with the anhydride group (-COOH) to form an amide bond (-CONH-) and releases water molecules. As the reaction proceeds, the prepolymer chain gradually grows and eventually forms a high molecular weight polyamic acid. 1,1'-Diaminoferrocene, as a bifunctional monomer, can undergo a similar polycondensation reaction with pyromellitic anhydride. The introduction of ferrocene groups into polymer chains enhances the electronic properties of the material and may improve thermal stability. Polysilsesquioxane is a polyhedral siloxane that reacts to form a polymer containing an inorganic-organic hybrid network. This structure increases the mechanical strength and chemical resistance of the polymer. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] FIG1 is a cross-sectional view of the structure of a diamond nuclear detector with graphene terminal ohmic contact electrode proposed by the present invention;
[0035] FIG2 is a structural cross-sectional view of step S1 in a method for preparing a diamond nuclear detector with a graphene terminal ohmic contact electrode according to the present invention;
[0036] FIG3 is a structural cross-sectional view of step S2 in a method for preparing a diamond nuclear detector with a graphene terminal ohmic contact electrode according to the present invention;
[0037] FIG4 is a structural cross-sectional view of step S3 in a method for preparing a diamond nuclear detector with a graphene terminal ohmic contact electrode according to the present invention;
[0038] FIG. 5 is a structural cross-sectional view of step S4 in a method for preparing a diamond nuclear detector with a graphene terminal ohmic contact electrode according to the present invention.
[0039] In the figure: 1. Intrinsic diamond layer; 2. Graphene layer; 3. Metal layer; 4. Passivation layer. DETAILED DESCRIPTION
[0040] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] Embodiment 1:
[0042] A method for preparing a graphene-terminated ohmic contact electrode diamond nuclear detector is prepared based on the above-mentioned graphene-terminated ohmic contact electrode diamond nuclear detector, comprising the following specific steps:
[0043] S1. As shown in FIG. 2 , graphene is grown on the intrinsic diamond layer 1 .
[0044] Among them, titanium is used as a catalyst to in-situ grow a graphene layer 2 on the intrinsic diamond layer 1. The specific process includes:
[0045] Cleaning the intrinsic diamond surface: Before starting, first use high-purity solvents such as acetone, ethanol and deionized water to thoroughly clean the diamond surface through ultrasonic cleaning to remove organic matter and other contaminants on the diamond surface to ensure the growth quality of graphene;
[0046] Vacuum treatment and placement of titanium metal: Place the cleaned diamond sample inside the crucible and place the titanium metal sheet on top of it. Then, evacuate the entire device to 10 -7 mbar high vacuum environment to exclude air and moisture and reduce the impact of impurities;
[0047] Heating and graphene growth: In a vacuum environment, the heating device is heated to 450°C and maintained for 4 minutes. Under this temperature condition, titanium metal will act as a catalyst to promote the decomposition and recombination of the carbon source on the diamond surface, thereby growing a uniform layer of graphene on the diamond surface;
[0048] Cleaning: After graphene growth is completed, the sample is cleaned with an appropriate solvent at room temperature to remove any unreacted catalyst residues or other impurities that may be present.
[0049] The graphene layer 2 is grown in situ by titanium metal catalysis. No foreign material is introduced on the surface of the intrinsic diamond layer 1. The interface of the device is CC bond without heterogeneous bonding, which is used to ensure low defects at the interface between the intrinsic diamond layer 1 and the graphene layer 2.
[0050] S2. As shown in FIG. 3 , titanium metal is deposited on the intrinsic diamond graphene layer 2 by magnetron sputtering.
[0051] Among them, the metal layer 3 is deposited with titanium metal, which is the same as the graphene catalytic metal and will not introduce new impurities. It is used to ensure the cleanliness of the processing technology and improve the yield. At the same time, the work function of titanium metal is similar to that of graphene, which is used to achieve low-resistance contact of the device, and it has good anti-electromigration characteristics and has high voltage and high current working conditions.
[0052] The magnetron sputtering step provides the necessary interface for the subsequent passivation layer deposition. S3. As shown in FIG4 , a passivation layer 4 is deposited on the titanium metal.
[0053] The passivation layer is made of silsesquioxane-modified polyimide, and the preparation method of the passivation layer 4 is as follows:
[0054] A1: In parts by weight, nitrogen was injected into a stirred reactor, 400 parts of N-methyl-pyrrolidone were added, the temperature of the reactor was set to 30°C, 10 parts of p-phenylenediamine, 0.05 parts of 1,1'-diaminoferrocene; 0.05 parts of aminopropylheptyl-cage polysilsesquioxane, and 30 parts of pyromellitic dianhydride were added, and the temperature was raised to 40°C under a nitrogen atmosphere and stirred for 100 minutes while heating, to prepare a polyamic acid;
[0055] A2: The polyamic acid was spun at a high speed of more than 1000 pm to remove bubbles. Then, it was applied to the surface of the metal layer 3 on both sides by a spin coater, and dried for 30 minutes at a temperature of 100°C in a nitrogen atmosphere to prepare a gel film. The temperature of the gel film was raised to 430°C at a rate of 2°C / min, and heat-treated for 60 minutes, and then cooled to 30°C at a rate of 2°C / min to obtain a passivation layer 4.
[0056] S4. As shown in FIG5 , flip the wafer and repeat steps S1 to S3.
[0057] The wafer is turned over, and then steps S1 to S3 are repeated on the other side of the intrinsic diamond, that is:
[0058] A graphene layer 2 is grown in situ on the diamond using titanium as a catalyst, titanium metal is then deposited on the graphene layer 2 by magnetron sputtering, and finally a passivation layer 4 is deposited on the titanium metal to increase the effective contact area of the detector.
[0059] The metal layer is made of titanium and has a thickness of 200 nm. Further optimizing the technical solution, the thickness of the graphene layer is 100 nm.
[0060] The intrinsic diamond layer is made of intrinsic diamond material, and the thickness of the intrinsic diamond layer is 500 nm.
[0061] Embodiment 2:
[0062] A method for preparing a graphene-terminated ohmic contact electrode diamond nuclear detector is prepared based on the above-mentioned graphene-terminated ohmic contact electrode diamond nuclear detector, comprising the following specific steps:
[0063] S1. As shown in FIG. 2 , graphene is grown on the intrinsic diamond layer 1 .
[0064] Among them, titanium is used as a catalyst to in-situ grow a graphene layer 2 on the intrinsic diamond layer 1. The specific process includes:
[0065] Cleaning the intrinsic diamond surface: Before starting, first use high-purity solvents such as acetone, ethanol and deionized water to thoroughly clean the diamond surface through ultrasonic cleaning to remove organic matter and other contaminants on the diamond surface to ensure the growth quality of graphene;
[0066] Vacuum treatment and placement of titanium metal: Place the cleaned diamond sample inside the crucible and place the titanium metal sheet on top of it. Then, evacuate the entire device to 3X10 -7mbar high vacuum environment to exclude air and moisture and reduce the impact of impurities;
[0067] Heating and graphene growth: In a vacuum environment, the heating device is heated to 480°C and maintained for 8 minutes. Under this temperature condition, titanium metal will act as a catalyst to promote the decomposition and recombination of the carbon source on the diamond surface, thereby growing a uniform layer of graphene on the diamond surface;
[0068] Cleaning: After graphene growth is completed, the sample is cleaned with an appropriate solvent at room temperature to remove any unreacted catalyst residues or other impurities that may be present.
[0069] Furthermore, the graphene layer 2 is grown in situ using titanium metal catalysis, and no foreign material is introduced on the surface of the intrinsic diamond layer 1. The interface of the device is CC bonded without heterogeneous bonding, which is used to ensure low defects at the interface between the intrinsic diamond layer 1 and the graphene layer 2.
[0070] S2. As shown in FIG. 3 , titanium metal is deposited on the intrinsic diamond graphene layer 2 by magnetron sputtering.
[0071] Among them, the metal layer 3 is deposited with titanium metal, which is the same as the graphene catalytic metal and will not introduce new impurities. It is used to ensure the cleanliness of the processing technology and improve the yield. At the same time, the work function of titanium metal is similar to that of graphene, which is used to achieve low-resistance contact of the device, and it has good anti-electromigration characteristics and has high voltage and high current working conditions.
[0072] Magnetron sputtering is an effective thin film preparation technology that can achieve high-quality, high-density and high-purity metal films at lower temperatures. This step provides the necessary interface for the subsequent passivation layer deposition.
[0073] S3. As shown in FIG. 4 , a passivation layer 4 is deposited on the titanium metal.
[0074] The passivation layer is made of silsesquioxane-modified polyimide, and the preparation method of the passivation layer 4 is as follows:
[0075] A1: In parts by weight, nitrogen was injected into a stirred reactor, 450 parts of N-methyl-pyrrolidone was added, the temperature of the reactor was set to 34°C, 15 parts of p-phenylenediamine, 0.2 parts of 1,1'-diaminoferrocene; 0.2 parts of aminopropylheptyl-cage polysilsesquioxane, and 40 parts of pyromellitic dianhydride were added, and the temperature was raised to 45°C under a nitrogen atmosphere and stirred for 140 minutes while heating to prepare a polyamic acid;
[0076] A2: The polyamic acid was spun at a high speed of more than 1500 rpm to remove bubbles. Then, the polyamic acid was applied to the surface of the metal layer 3 on both sides by a spin coater, and dried for 35 minutes at a temperature of 120°C in a nitrogen atmosphere to prepare a gel film. The temperature of the gel film was raised to 440°C at a rate of 3°C / min, and heat-treated for 70 minutes, and then cooled to 35°C at a rate of 3°C / min to obtain a passivation layer 4.
[0077] S4. As shown in FIG5 , flip the wafer and repeat steps S1 to S3.
[0078] The wafer is turned over, and then steps S1 to S3 are repeated on the other side of the intrinsic diamond, that is:
[0079] A graphene layer 2 is grown in situ on the diamond using titanium as a catalyst, titanium metal is then deposited on the graphene layer 2 by magnetron sputtering, and finally a passivation layer 4 is deposited on the titanium metal to increase the effective contact area of the detector.
[0080] The metal layer is made of titanium and has a thickness of 240 nm. Further optimizing the technical solution, the thickness of the graphene layer is 110 nm.
[0081] The intrinsic diamond layer is made of intrinsic diamond material, and the thickness of the intrinsic diamond layer is 1000 nm.
[0082] Embodiment 3:
[0083] A method for preparing a graphene-terminated ohmic contact electrode diamond nuclear detector is prepared based on the above-mentioned graphene-terminated ohmic contact electrode diamond nuclear detector, comprising the following specific steps:
[0084] S1. As shown in FIG. 2 , graphene is grown on the intrinsic diamond layer 1 .
[0085] Among them, titanium is used as a catalyst to in-situ grow a graphene layer 2 on the intrinsic diamond layer 1. The specific process includes:
[0086] Cleaning the intrinsic diamond surface: Before starting, first use high-purity solvents such as acetone, ethanol and deionized water to thoroughly clean the diamond surface through ultrasonic cleaning to remove organic matter and other contaminants on the diamond surface to ensure the growth quality of graphene;
[0087] Vacuum treatment and placement of titanium metal: Place the cleaned diamond sample inside the crucible and place the titanium metal sheet on top of it. Then, evacuate the entire device to 7X10 -7mbar high vacuum environment to exclude air and moisture and reduce the impact of impurities;
[0088] Heating and graphene growth: In a vacuum environment, the heating device is heated to 550°C and maintained for 10 minutes. Under this temperature condition, titanium metal will act as a catalyst to promote the decomposition and recombination of the carbon source on the diamond surface, thereby growing a uniform layer of graphene on the diamond surface;
[0089] Cleaning: After graphene growth is completed, the sample is cleaned with an appropriate solvent at room temperature to remove any unreacted catalyst residues or other impurities that may be present.
[0090] Furthermore, the graphene layer 2 is grown in situ using titanium metal catalysis, and no foreign material is introduced on the surface of the intrinsic diamond layer 1. The interface of the device is CC bonded without heterogeneous bonding, which is used to ensure low defects at the interface between the intrinsic diamond layer 1 and the graphene layer 2.
[0091] S2. As shown in FIG. 3 , titanium metal is deposited on the intrinsic diamond graphene layer 2 by magnetron sputtering.
[0092] Among them, the metal layer 3 is deposited with titanium metal, which is the same as the graphene catalytic metal and will not introduce new impurities. It is used to ensure the cleanliness of the processing technology and improve the yield. At the same time, the work function of titanium metal is similar to that of graphene, which is used to achieve low-resistance contact of the device, and it has good anti-electromigration characteristics and has high voltage and high current working conditions.
[0093] Magnetron sputtering is an effective thin film preparation technology that can achieve high-quality, high-density and high-purity metal films at lower temperatures. This step provides the necessary interface for the subsequent passivation layer deposition.
[0094] S3. As shown in FIG. 4 , a passivation layer 4 is deposited on the titanium metal.
[0095] The passivation layer is made of silsesquioxane-modified polyimide, and the preparation method of the passivation layer 4 is as follows:
[0096] A1: In parts by weight, nitrogen is injected into a stirred reactor, 400-600 parts of N-methyl-pyrrolidone is added, the temperature of the reactor is set to 30-40°C, 10-20 parts of p-phenylenediamine, 0.05-0.5 parts of 1,1'-diaminoferrocene; 0.05-0.5 parts of aminopropylheptyl-cage polysilsesquioxane, and 30-60 parts of pyromellitic dianhydride are added, and the temperature is raised to 40-50°C under a nitrogen atmosphere and heated while stirring for 100-200 minutes to prepare a polyamic acid;
[0097] A2: The polyamic acid is spun at a high speed of 1000-2000 rpm or more to remove bubbles. Then, it is applied to the surface of the metal layer 3 on both sides by a spin coater, and dried for 30-50 minutes at a temperature of 100-130° C. in a nitrogen atmosphere to prepare a gel film, and the temperature of the gel film is raised to 430-480° C. at a rate of 2-5° C. / min, and heat-treated for 60-100 minutes, and then cooled to 30-40° C. at a rate of 2-5° C. / min to obtain a passivation layer 4.
[0098] S4. As shown in FIG5 , flip the wafer and repeat steps S1 to S3.
[0099] The wafer is turned over, and then steps S1 to S3 are repeated on the other side of the intrinsic diamond, that is:
[0100] A graphene layer 2 is grown in situ on the diamond using titanium as a catalyst, titanium metal is then deposited on the graphene layer 2 by magnetron sputtering, and finally a passivation layer 4 is deposited on the titanium metal to increase the effective contact area of the detector.
[0101] The metal layer is made of titanium and has a thickness of 300 nm. The graphene layer has a thickness of 120 nm.
[0102] The intrinsic diamond layer is made of intrinsic diamond material, and the thickness of the intrinsic diamond layer is 1500 nm.
[0103] Comparative Example 1:
[0104] The passivation layer 4 uses commercially available polyamic acid, MV9500, and the rest is the same as in Example 1.
[0105] Comparative Example 2:
[0106] The aminopropylheptyl-cage polysilsesquioxane was not added, and the other steps were the same as in Example 1.
[0107] Comparative Example 3:
[0108] The other steps were the same as those in Example 1 except that 1,1'-diaminoferrocene was not added.
[0109] The test data of the graphene terminal ohmic contact electrode diamond nuclear detector are as follows:
[0110] Test data
[0111]
[0112] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0113] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A graphene-terminated ohmic contact electrode diamond nuclear detector, characterized in that: It comprises an intrinsic diamond layer, the intrinsic diamond layer is located in the middle of the device of the nuclear detector, graphene layers are arranged above and below the intrinsic diamond layer, metal layers are arranged on the surfaces of the graphene layers on the upper and lower sides of the intrinsic diamond layer, and passivation layers are arranged on the surfaces of the metal layers on both sides, and the passivation layers are located on the device surface of the nuclear detector; The nuclear detector uses a graphene layer and a metal layer to form an ohmic contact electrode; The passivation layer adopts silsesquioxane modified polyimide, and the preparation method is as follows: A1: nitrogen is injected into a stirred reactor, 400-600 parts of N-methyl-pyrrolidone is added, the temperature of the reactor is set to 30-40°C, 10-20 parts of p-phenylenediamine, 0.05-0.5 parts of 1,1'-diaminoferrocene; 0.05-0.5 parts of aminopropylheptyl-cage polysilsesquioxane, and 30-60 parts of pyromellitic dianhydride are added, and the temperature is raised to 40-50°C under a nitrogen atmosphere and heated while stirring for 100-200 minutes to obtain a polyamic acid; A2: The polyamic acid is subjected to high-speed rotation at 1000-2000 rpm or more to remove bubbles, and then coated on the surface of the metal layer 3 on both sides by a spin coater, and dried for 30-50 minutes at a temperature of 100-130° C. under a nitrogen atmosphere to prepare a gel film, and the temperature of the gel film is raised to 430-480° C. at a rate of 2-5° C. / min, and heat-treated for 60-100 minutes, and then cooled to 30-40° C. at a rate of 2-5° C. / min to obtain a silsesquioxane-modified polyimide.
2. The graphene-terminated ohmic contact electrode diamond nuclear detector according to claim 1, characterized in that: The intrinsic diamond layer is the device radiation area of the nuclear detector. The intrinsic diamond layer adopts intrinsic diamond material. The thickness of the intrinsic diamond layer is 500-1500nm.
3. The graphene-terminated ohmic contact electrode diamond nuclear detector according to claim 1, characterized in that: The metal layer is made of titanium and has a thickness of 200-300 nm.
4. The graphene-terminated ohmic contact electrode diamond nuclear detector according to claim 1, characterized in that: The thickness of the graphene layer is 100 nm.
5. A method for preparing a graphene-terminated ohmic contact electrode diamond nuclear detector, prepared based on the graphene-terminated ohmic contact electrode diamond nuclear detector according to any one of claims 1 to 4, characterized in that: The specific steps include: S1, growing graphene on the intrinsic diamond layer; S2, depositing titanium metal on the intrinsic diamond graphene layer by magnetron sputtering; S3, depositing a passivation layer on the titanium metal; S4. Flip the wafer and repeat steps S1-S3.
6. The method for preparing a graphene-terminated ohmic contact electrode diamond nuclear detector according to claim 5, characterized in that: In step S1, titanium is used as a catalyst to in-situ grow a graphene layer on the intrinsic diamond layer. The specific process includes: Cleaning the intrinsic diamond surface: Before starting, first use a high-purity solvent selected from acetone, ethanol and deionized water to thoroughly clean the diamond surface by ultrasonic cleaning to remove organic matter and other contaminants on the diamond surface to ensure the growth quality of graphene; Vacuum treatment and placement of titanium metal: The cleaned diamond sample is placed inside the crucible, and the titanium metal sheet is placed on top of it. Then, the entire device is evacuated to 1x10 -7 -5x10 -7 mbar high vacuum environment to exclude air and moisture and reduce the impact of impurities; Heating and graphene growth: In a vacuum environment, heat the device to 450-550°C and maintain for 4-10 minutes. Under this temperature condition, titanium metal will act as a catalyst to promote the decomposition and recombination of the carbon source on the diamond surface, thereby growing a uniform layer of graphene on the diamond surface; Cleaning: After graphene growth is completed, the sample is cleaned with an appropriate solvent at room temperature to remove any unreacted catalyst residues or other impurities that may be present.
7. The method for preparing a graphene-terminated ohmic contact electrode diamond nuclear detector according to claim 5, characterized in that: In step S4, the wafer is turned over, and then steps S1 to S3 are repeated on the other side of the intrinsic diamond, that is: Titanium is used as a catalyst to grow a graphene layer in situ on top of the diamond, and then titanium metal is deposited on the graphene layer by magnetron sputtering. Finally, a passivation layer is deposited on the titanium metal to increase the effective contact area of the detector.
8. The method for preparing a graphene-terminated ohmic contact electrode diamond nuclear detector according to claim 5, characterized in that: In step S1, the graphene layer is grown in situ by titanium metal catalysis, and no foreign material is introduced on the surface of the intrinsic diamond layer. The interface of the device is CC bond without heterogeneous bonding, so as to ensure low defects at the interface between the intrinsic diamond layer and the graphene layer.
9. The method for preparing a graphene-terminated ohmic contact electrode diamond nuclear detector according to claim 5, characterized in that: In the step S2, the metal layer is deposited using titanium metal, which is the same as the graphene catalytic metal.