A method for preparing fluorinated polybenzimidazole proton exchange membrane
By introducing a fluorinated cross-linking agent into polybenzimidazole and compounding it with MXene nanosheets, the problem of reduced mechanical properties and insufficient proton conductivity of polybenzimidazole proton exchange membranes has been solved, and high-performance proton exchange membrane preparation has been achieved, which is suitable for for high temperature fuel cells.
Patent Information
- Application Number
- CN202410413444.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-08
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-04-08
AI Technical Summary
The mechanical properties of polybenzimidazole proton exchange membranes decrease after doping with phosphoric acid, and existing cross-linking methods may reduce proton conductivity, limiting its application.
By introducing a fluorinated cross-linking agent into polybenzimidazole for modification and compounding with MXene nanosheets, a cross-linked fluorinated loaded polybenzimidazole membrane is formed to improve oxidation stability, alkali resistance, proton conductivity and Mechanical properties.
The oxidation stability, alkali resistance, proton conductivity and mechanical properties of the polybenzimidazole proton exchange membrane are significantly improved, meeting the needs of high-performance fuel cells.
Smart Images

Figure CN118325154B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of research and development of fuel cell proton exchange membrane materials, and in particular to a method for preparing a fluorinated polybenzimidazole proton exchange membrane. Background Art
[0002] Fuel cells are electrochemical devices that convert chemical energy into electrical energy. They are considered the first choice for clean green energy due to their high power generation efficiency and zero pollution. Proton exchange membrane, as one of the core components of fuel cells, has an important influence on their performance.
[0003] Polybenzimidazole is a polymer with benzimidazole groups as repeating units, usually made by polycondensation of benzyltetramine and diacids and their derivatives as monomers, and has excellent thermal stability, good dimensional stability and wear resistance. Among them, fluorinated polybenzimidazole refers to the introduction of F elements into the polymer skeleton, especially the introduction of large and flexible groups hexafluoroisopropyl (-C(CF3)2-), which can make the polymer exhibit excellent thermal stability and good free radical antioxidant ability.
[0004] After polybenzimidazole is protonated by phosphoric acid doping, it can be used as a proton exchange membrane for high-temperature fuel cells. However, phosphoric acid adsorption weakens the interaction between the -NH group and the -N=C group on the imidazole ring in the polybenzimidazole molecule, causing the mechanical properties of the polybenzimidazole proton exchange membrane to deteriorate, which greatly limits its application. Therefore, polybenzimidazole needs to be modified to meet the requirements of use. Common modification methods include copolymerization, grafting, cross-linking, and introduction of inorganic materials.
[0005] The search found that: in the patent with publication number CN104151587A, a novel cross-linked polybenzimidazole membrane with enhanced mechanical properties is prepared by covalent cross-linking using polybenzimidazole resin as raw material, binary or polycyclic halogenated compounds and epoxy compounds as cross-linking agents through solvent evaporation method. The introduction of the cross-linking agent in the above method may reduce the phosphoric acid doping amount of the polybenzimidazole membrane, and thus may reduce the proton conductivity of the polybenzimidazole proton exchange membrane.
[0006] Further search revealed that the surface of MXene nanosheets contains a large amount of OH - Introducing it into polybenzimidazole can achieve the effect of improving proton conductivity, and MXene nanosheets can interact with the -NH group and -N=C group on the imidazole ring in the polybenzimidazole molecule through hydrogen bonds, thereby improving the mechanical properties of the benzimidazole proton exchange membrane. Summary of the invention
[0007] The present invention provides a method for preparing a fluorinated polybenzimidazole proton exchange membrane, which introduces a fluorinated crosslinking agent into polybenzimidazole for modification to achieve the technical effect of improving the oxidation stability and alkali resistance of the polybenzimidazole membrane, and on this basis, it is composited with MXene nanosheets to achieve the technical goal of simultaneously improving the proton conductivity and mechanical properties of the fluorinated polybenzimidazole proton exchange membrane.
[0008] A method for preparing a fluorinated polybenzimidazole proton exchange membrane comprises the following steps:
[0009] Step 1: preparing a cross-linked fluorinated supported polybenzimidazole membrane: the epoxy functional group of the fluorinated cross-linking agent undergoes a ring-opening reaction with the amino functional group of the polybenzimidazole, and the hydrogen atoms of the hydroxyl groups carried on the surface of the MXene nanosheets form hydrogen bonds with the nitrogen atoms in the polybenzimidazole, thereby achieving a fluorinated cross-linked supported composite modification effect, and a cross-linked fluorinated supported polybenzimidazole membrane is prepared through a cross-linking curing reaction;
[0010] The fluorinated cross-linking agent is cross-linking agent I or cross-linking agent II;
[0011] Step 2: First, soak the cross-linked fluorinated supported polybenzimidazole membrane in a potassium hydroxide solution for 6 to 20 hours, then soak it in deionized water for 6 to 20 hours, and finally soak it in an 85% phosphoric acid solution at 80 to 120° C. for 30 to 50 hours to prepare a fluorinated polybenzimidazole proton exchange membrane.
[0012] Preferably, the preparation method of the cross-linking agent I is:
[0013] Step S1-1, generating a dipiperidyl fluorinated monomer by esterification reaction of the carboxyl functional group of 4,4'-(hexafluoroisopropylidene)bis(benzoic acid) with the hydroxyl functional group of 1-methyl-4-piperidinol;
[0014] Step S1-2, utilizing the nucleophilic substitution reaction mechanism, the tertiary amine functional group of the nucleophilic reagent dipiperidyl fluorinated monomer and the chlorine functional group of epichlorohydrin undergo quaternization reaction to generate crosslinking agent I.
[0015] Preferably, the preparation method of the cross-linking agent II is:
[0016] Step S2-1, generating a tetrapiperidyl fluorinated monomer by esterification reaction of the carboxyl functional group of 4,4'-(2,2,2-trifluoro-1-trifluoromethyl)ethylenebis(1,2-phthalic acid) with the hydroxyl functional group of 1-methyl-4-piperidinol;
[0017] Step S2-2, using the nucleophilic substitution reaction mechanism, the tertiary amine functional group of the tetrapiperidyl fluorinated monomer as a nucleophilic reagent and the chlorine functional group of epichlorohydrin undergo quaternization reaction to generate a crosslinking agent II.
[0018] The fluorinated polybenzimidazole proton exchange membrane prepared according to the above method is a loaded cross-linked fluorinated polybenzimidazole proton exchange membrane I or a loaded cross-linked fluorinated polybenzimidazole proton exchange membrane II.
[0019] Preferably, the fluorinated polybenzimidazole proton exchange membrane has a tensile strength of 7.5 to 10 MPa and a proton conductivity of 45 to 57%.
[0020] Preferably, the raw material used for the supported cross-linked fluorinated polybenzimidazole proton exchange membrane I is supported cross-linked fluorinated polybenzimidazole membrane I.
[0021] Preferably, the raw material used for the supported cross-linked fluorinated polybenzimidazole proton exchange membrane II is supported cross-linked fluorinated polybenzimidazole membrane II.
[0022] Beneficial Effects
[0023] The present invention firstly prepares four cross-linked fluorinated polyimidazole membranes, which are: cross-linked fluorinated polybenzimidazole membrane I, cross-linked fluorinated polybenzimidazole membrane II, loaded cross-linked fluorinated polybenzimidazole membrane I, loaded cross-linked fluorinated polybenzimidazole membrane II;
[0024] The experiment found that the oxidation stability and alkali resistance of the cross-linked fluorinated polyimidazole membrane were significantly better than those of other non-cross-linked polyimidazole membranes.
[0025] Furthermore, four kinds of proton exchange membranes were prepared using the above four cross-linked fluorinated polyimidazole membranes as raw materials, namely: cross-linked fluorinated polybenzimidazole proton exchange membrane I, cross-linked fluorinated polybenzimidazole proton exchange membrane II, loaded cross-linked fluorinated polybenzimidazole proton exchange membrane I, loaded cross-linked fluorinated polybenzimidazole proton exchange membrane II;
[0026] Through experiments, it was found that the proton exchange membrane prepared by the composite modification method of fluorination cross-linking and loading nanomaterials not only has better proton conductivity, but also has better mechanical properties.
[0027] The invention provides a modification method for preparing a proton exchange membrane with better proton conductivity and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 is the chemical reaction formula for synthesizing the dipiperidyl fluorinated monomer;
[0029] Figure 2 is the chemical structural formula of cross-linking agent I;
[0030] Figure 3 is the chemical structural formula of fluorine-containing functional monomer I;
[0031] Figure 4is the chemical structural formula of a tetrapiperidinyl fluorinated monomer;
[0032] Figure 5 is the chemical structural formula of cross-linking agent II;
[0033] Figure 6 is the chemical structural formula of fluorine-containing functional monomer II;
[0034] Figure 7 The performance test results of each polyimidazole film;
[0035] Figure 8 The performance test results of each proton exchange membrane are shown in Figure 2. DETAILED DESCRIPTION
[0036] Experimental Example 1:
[0037] Synthesis of dipiperidyl fluorinated monomer: The carboxyl functional group of 4,4'-(hexafluoroisopropylidene)bis(benzoic acid) undergoes esterification with the hydroxyl functional group of 1-methyl-4-piperidinol to generate a dipiperidyl fluorinated monomer. The chemical reaction formula is as follows: Figure 1 As shown;
[0038] The specific experimental steps for synthesizing the dipiperidyl fluorine-containing monomer are as follows: 7.8 g of 4,4'-(hexafluoroisopropylidene)bis(benzoic acid), 4.6 g of 1-methyl-4-piperidinol and 100 mL of toluene are added to a round-bottom flask with a water separator, 0.05 g of concentrated sulfuric acid is added dropwise, and then stirred in a 65°C water bath for 2 h, washed with saturated brine, dried with anhydrous magnesium sulfate, and rotary evaporated to remove toluene to obtain a dipiperidyl fluorine-containing monomer;
[0039] The H NMR spectrum of the dipiperidyl fluorinated monomer is characterized as follows: 1 H NMR (DMSO-d6, 400MHz) δ: 2.13-2.18 (m, 8H), 2.32 (s, 6H), 2.64-2.77 (m, 8H), 4.95-5.00 (m, 2H), 7.42-7.44 (d, 4H), 7.91-7.93 (d, 4H);
[0040] Synthesis of crosslinker I: Using the nucleophilic substitution reaction mechanism, the tertiary amine functional group of the nucleophilic reagent dipiperidyl fluorinated monomer and the chlorine functional group of epichlorohydrin undergo quaternization reaction to generate crosslinker I, whose chemical structure is as follows: Figure 2 As shown;
[0041] The specific experimental steps for synthesizing crosslinker I are as follows: 5.9 g of dipiperidyl fluorinated monomer, 2.4 mL of epichlorohydrin and 50 mL of acetonitrile are added to a three-necked flask, heated to 50° C. for reaction for 12 h under nitrogen and mechanical stirring, and distilled under reduced pressure to remove excess epichlorohydrin, washed with ether, and dried under vacuum to obtain crosslinker I;
[0042] The H NMR spectrum of crosslinker I is characterized as follows: 1 H NMR (DMSO-d6, 400MHz) δ: 2.23-2.27 (m, 8H), 3.30 (s, 6H), 3.40-3.43 (m, 4H), 3.56-3.58 (d, 4H), 3.69-3.77(m, 8H), 4.04-4.09(m, 2H), 5.12-5.17(m, 2H), 7.41-7.43(d, 4H), 7.90-7.92(d, 4H);
[0043] Fluorine-containing functional monomer I: Using the nucleophilic substitution reaction mechanism, the tertiary amine functional group of the nucleophilic reagent dipiperidyl fluorine-containing monomer and the chlorine functional group of 1-chloropropane undergo quaternization reaction to generate fluorine-containing functional monomer I, whose chemical structure is as follows Figure 3 As shown;
[0044] The fluorine-containing functional monomer I was synthesized. The synthesis steps and reaction conditions of the synthetic monomer I were similar to those of the crosslinker I. The difference between the synthetic monomer I and the crosslinker I was that 2.4 mL of epichlorohydrin was replaced by 2.7 mL of 1-chloropropane.
[0045] The nuclear magnetic resonance hydrogen spectrum of the fluorine-containing functional monomer I is characterized as follows: 1 H NMR (DMSO-d6, 400MHz) δ: 1.09-1.12 (t, 6H), 1.63-1.69 (m, 4H), 2.17-2.26 (m, 8H), 3.23 (s, 6H), 3.54-3.56(t, 4H), 3.64-3.69(m, 8H), 5.11-5.16(m, 2H), 7.41-7.43(d, 4H), 7.89-7.91(d, 4H).
[0046] Experimental Example 2:
[0047] Synthesis of tetrapiperidinyl fluorinated monomers: The carboxyl functional group of 4,4'-(2,2,2-trifluoro-1-trifluoromethyl)ethylenebis(1,2-phthalic acid) reacts with the hydroxyl functional group of 1-methyl-4-piperidinol to generate tetrapiperidinyl fluorinated monomers, whose chemical structure is as follows: Figure 4 As shown;
[0048] The specific experimental steps for synthesizing the tetrapiperidinyl fluorinated monomer are as follows: 4.8 g of 4,4'-(2,2,2-trifluoro-1-trifluoromethyl)ethylenebis(1,2-phthalic acid), 2.3 g of 1-methyl-4-piperidinol and 100 mL of toluene are added to a round-bottom flask with a water separator, 0.1 g of concentrated sulfuric acid is added dropwise, and then stirred in a 65°C water bath for 2 h, washed with saturated brine, dried over anhydrous magnesium sulfate, and rotary evaporated to remove toluene to obtain a tetrapiperidinyl fluorinated monomer;
[0049] The hydrogen nuclear magnetic resonance spectrum of the tetrapiperidinyl fluorinated monomer is characterized as follows: 1 H NMR (DMSO-d6, 400MHz) δ: 2.11-2.20 (m, 16H), 2.35 (s, 12H), 2.64-2.77 (m, 1 6H), 4.96-5.00(m, 4H), 7.55-7.57(d, 2H), 7.78(s, 2H), 7.85-7.86(d, 2H);
[0050] Synthesis of crosslinker II: Using the nucleophilic substitution reaction mechanism, the tertiary amine functional group of the tetrapiperidinyl fluorinated monomer and the chlorine functional group of epichlorohydrin undergo quaternization reaction to generate crosslinker II, whose chemical structure is as follows: Figure 5 As shown;
[0051] Synthesize crosslinker II. The synthesis steps and reaction conditions of the crosslinker II are similar to those of the crosslinker I. The difference between the synthesis steps and reaction conditions of the crosslinker II and the crosslinker I is that 4.4 g of tetrapiperidyl fluorinated monomer is used to replace 5.9 g of dipiperidyl fluorinated monomer.
[0052] The H NMR spectrum of crosslinker II is characterized as follows: 1 H NMR (DMSO-d6, 400MHz) δ: 2.22-2.26 (m, 16H), 3.30 (s, 12H), 3.40-3.44 (m, 8H), 3.56-3.58 (d, 8H), 3.70- 3.78(m, 16H), 4.01-4.04(m, 4H), 5.15-5.19(m, 4H), 7.55-7.57(d, 2H), 7.78(s, 2H), 7.84-7.86(d, 2H);
[0053] Synthesis of fluorinated functional monomer II: Using the nucleophilic substitution reaction mechanism, the tertiary amine functional group of the tetrapiperidinyl fluorinated monomer and the chlorine functional group of 1-chloropropane undergo quaternization reaction to generate fluorinated functional monomer II, whose chemical structure is as follows: Figure 6 As shown;
[0054] Synthesize fluorine-containing functional monomer II. The synthesis steps and reaction conditions are similar to those of the synthesis experiment of crosslinker II. The difference between the synthesis experiment of crosslinker II and the synthesis experiment of fluorine-containing functional monomer II is that 2.4 mL of epichlorohydrin is replaced by 2.7 mL of 1-chloropropane.
[0055] The nuclear magnetic resonance hydrogen spectrum of the fluorine-containing functional monomer II is characterized as follows: 1 H NMR (DMSO-d6, 400MHz) δ: 1.08-1.11 (t, 12H), 1.63-1.70 (m, 8H), 2.17-2.26 (m, 16H), 3.23 (s, 12H), 3.54 -3.56(t, 8H), 3.63-3.70(m, 16H), 5.14-5.20(m, 4H), 7.55-7.57(d, 2H), 7.78(s, 2H), 7.84-7.86(d, 2H).
[0056] Experimental Example 3:
[0057] Preparation of MXene nanosheets: 1.6 g of titanium aluminum carbide, 2.0 g of lithium fluoride and 50 mL of hydrochloric acid were added to a reactor, stirred and reacted in a 25°C water bath for 48 h, the pH of the solution was adjusted to neutral with deionized water, ultrasonically shaken, repeatedly centrifuged, and filtered to dry to obtain MXene nanosheets.
[0058] Embodiment 1:
[0059] The cross-linked fluorinated polybenzimidazole membrane I is prepared by the following mechanism: the cross-linked fluorinated polybenzimidazole membrane I is prepared by the cross-linking curing reaction between the epoxy functional group of the cross-linking agent I and the amino functional group of the polybenzimidazole;
[0060] The specific experimental steps for preparing the cross-linked fluorinated polybenzimidazole membrane I are as follows: 15 g of polybenzimidazole particles and 150 mL of N,N-dimethylacetamide are added to a beaker to form a polybenzimidazole solution, 7.7 g of cross-linking agent I is added to the beaker, and stirred for 4 hours to mix evenly; the mixed solution is directly cast on a glass plate with a smooth surface, and a programmed temperature rise process is performed according to the following steps: first, it is dried in a vacuum oven at 80°C for 24 hours to evaporate most of the solvent; then, the vacuum oven temperature is increased to 150°C for reaction for 3 hours to obtain a cross-linked fluorinated polybenzimidazole membrane I with an average thickness of 75 μm;
[0061] The preparation method of polybenzimidazole particles is as follows: 4.3g 3,3'-diaminobenzidine, 6.4g diphenyl isophthalate and 100mL N,N-dimethylacetamide are added to a three-necked flask, and the temperature is raised to 260°C for reaction for 2h under the action of nitrogen and mechanical stirring. During the heating process, when the viscosity of the reaction mixture increases to the point where stirring is impossible, the mechanical stirring is turned off to obtain a prepolymer, which is then cooled to room temperature and ground into powder; the prepolymer is added to a three-necked flask with nitrogen, stirred and reacted in a 340°C salt bath for 2h, naturally cooled to room temperature, vacuum dried and ground to obtain polybenzimidazole particles; the viscosity of the polybenzimidazole is measured using an Ubbelohde viscometer, the polybenzimidazole is dissolved in N,N-dimethylacetamide using concentrated sulfuric acid as a solvent, 100mL of a polybenzimidazole solution with a concentration of 5g / L is prepared, the viscosity is tested at 25°C, and the viscosity average molecular weight is calculated to be 30314;
[0062] Preparation of polybenzimidazole membrane: 15 g of polybenzimidazole particles and 100 mL of N,N-dimethylacetamide were added into a beaker to form a polybenzimidazole solution, which was directly cast onto a smooth glass plate. According to the experimental method of cross-linked fluorinated polybenzimidazole membrane I, a polybenzimidazole membrane with an average thickness of 75 μm was prepared.
[0063] Embodiment 2:
[0064] The cross-linked fluorinated polybenzimidazole membrane II is prepared by cross-linking and curing reaction between the epoxy functional group of the cross-linking agent II and the amino functional group of the polybenzimidazole;
[0065] The preparation steps and reaction conditions of cross-linked fluorinated polybenzimidazole membrane II are similar to those of cross-linked fluorinated polybenzimidazole membrane I. The difference between the preparation steps and reaction conditions of cross-linked fluorinated polybenzimidazole membrane II and the preparation experiment of cross-linked fluorinated polybenzimidazole membrane I is that 12.4 g of cross-linker II replaces 7.7 g of cross-linker I.
[0066] Embodiment three:
[0067] The non-crosslinked fluorinated polybenzimidazole membrane I is prepared by directly compounding the fluorinated functional monomer I with polybenzimidazole and then undergoing a curing reaction to prepare the non-crosslinked fluorinated polybenzimidazole membrane I;
[0068] The non-cross-linked fluorinated polybenzimidazole membrane I was prepared. The preparation steps and reaction conditions were similar to those of the cross-linked fluorinated polybenzimidazole membrane I. The difference between the non-cross-linked fluorinated polybenzimidazole membrane I and the cross-linked fluorinated polybenzimidazole membrane I was that 7.4 g of fluorinated functional monomer I was used to replace 7.7 g of cross-linking agent I.
[0069] Embodiment 4:
[0070] The non-crosslinked fluorinated polybenzimidazole membrane II is prepared, and the mechanism is as follows: the non-crosslinked fluorinated polybenzimidazole membrane II is obtained by directly compounding the fluorinated functional monomer II with polybenzimidazole and then undergoing a curing reaction;
[0071] The non-cross-linked fluorinated polybenzimidazole membrane II was prepared. The preparation steps and reaction conditions were similar to those of the cross-linked fluorinated polybenzimidazole membrane I. The difference between the non-cross-linked fluorinated polybenzimidazole membrane II and the cross-linked fluorinated polybenzimidazole membrane I was that 11.8 g of fluorinated functional monomer II was used to replace 7.7 g of cross-linking agent I.
[0072] Embodiment five:
[0073] Preparation of loaded cross-linked fluorinated polybenzimidazole membrane I, the mechanism of which is: on the one hand, the epoxy functional group of the cross-linking agent I reacts with the amino functional group of the polybenzimidazole to form a ring-opening reaction, and on the other hand, the hydrogen atoms of the hydroxyl groups loaded on the surface of the MXene nanosheets form hydrogen bonds with the nitrogen atoms in the polybenzimidazole to achieve loaded cross-linking composite action, and the loaded cross-linked fluorinated polybenzimidazole membrane I is prepared through a cross-linking curing reaction;
[0074] The specific experimental steps for preparing the loaded cross-linked fluorinated polybenzimidazole membrane I are as follows: 15 g of polybenzimidazole particles (prepared by the method in Example 1) and 100 mL of N,N-dimethylacetamide are added to a beaker to form a polybenzimidazole solution, 50 mL of MXene nanosheet solution (prepared by 1 g of MXene nanosheets and 50 mL of N,N-dimethylacetamide) and 7.7 g of cross-linking agent I are added to the beaker, and stirred for 4 hours to mix evenly; the mixed solution is directly cast on a glass plate with a smooth surface, and a loaded cross-linked fluorinated polybenzimidazole membrane I with an average thickness of 75 μm is prepared according to the experimental method of the cross-linked fluorinated polybenzimidazole membrane I.
[0075] Embodiment six:
[0076] Preparation of loaded cross-linked fluorinated polybenzimidazole membrane II, the mechanism of which is: on the one hand, the epoxy functional group of the cross-linking agent II reacts with the amino functional group of the polybenzimidazole to form a ring-opening reaction, and on the other hand, the hydrogen atoms of the hydroxyl groups loaded on the surface of the MXene nanosheets form hydrogen bonds with the nitrogen atoms in the polybenzimidazole to achieve loaded cross-linking composite action, and the loaded cross-linked fluorinated polybenzimidazole membrane II is prepared through a cross-linking curing reaction;
[0077] Prepare loaded cross-linked fluorinated polybenzimidazole membrane II. Its preparation steps and reaction conditions refer to the preparation experiment of loaded cross-linked fluorinated polybenzimidazole membrane I. The difference between it and the preparation experiment of loaded cross-linked fluorinated polybenzimidazole membrane I is that 12.4g of cross-linker II replaces 7.7g of cross-linker I.
[0078] Embodiment seven:
[0079] Preparation of proton exchange membrane: soaking the polyimidazole membrane in 5 mol / L potassium hydroxide solution and deionized water for 12 hours, then immersing it in 85% phosphoric acid solution at 100°C for 48 hours, doping the film with phosphoric acid, taking it out and vacuum drying it at 90°C for 12 hours to obtain a proton exchange membrane;
[0080] Using cross-linked fluorinated polybenzimidazole membrane I as the polyimidazole membrane, and according to the experimental method for preparing proton exchange membrane, a cross-linked fluorinated polybenzimidazole proton exchange membrane I is prepared;
[0081] Using cross-linked fluorinated polybenzimidazole membrane II as the polyimidazole membrane, and according to the experimental method for preparing proton exchange membrane, a cross-linked fluorinated polybenzimidazole proton exchange membrane II is prepared;
[0082] Using non-crosslinked fluorinated polybenzimidazole membrane I as the polyimidazole membrane, and according to the experimental method for preparing proton exchange membrane, a non-crosslinked fluorinated polybenzimidazole proton exchange membrane I is prepared;
[0083] Using non-crosslinked fluorinated polybenzimidazole membrane II as the polyimidazole membrane, and according to the experimental method for preparing proton exchange membrane, non-crosslinked fluorinated polybenzimidazole proton exchange membrane II is prepared;
[0084] Using a loaded cross-linked fluorinated polybenzimidazole membrane I as a polyimidazole membrane, and according to an experimental method for preparing a proton exchange membrane, a loaded cross-linked fluorinated polybenzimidazole proton exchange membrane I is prepared;
[0085] Using the loaded cross-linked fluorinated polybenzimidazole membrane II as the polyimidazole membrane, and according to the experimental method for preparing the proton exchange membrane, the loaded cross-linked fluorinated polybenzimidazole proton exchange membrane II is prepared;
[0086] A polybenzimidazole proton exchange membrane is prepared by using a polybenzimidazole membrane as the polyimidazole membrane and following an experimental method for preparing a proton exchange membrane.
[0087] Performance test experiment 1:
[0088] The following performance tests were performed on the polyimidazole films in the above-mentioned embodiments 1 to 6, and the specific test methods are as follows:
[0089] 1. Oxidation stability performance test:
[0090] The oxidation stability of polyimidazole membrane was tested by Fenton reagent oxidation method, and its oxidation stability was analyzed by the mass retention rate of polyimidazole membrane.
[0091] The specific test steps of the oxidative stability performance are as follows: immerse a 2 cm × 2 cm square polyimidazole film in Fenton's reagent (3% H2O2, 2ppm FeSO4), place it in a constant temperature oven at 80°C, take out the polyimidazole film after immersion for 72 hours, rinse it repeatedly with deionized water, and dry it in an oven at 100°C. Record the mass retention rate of the polyimidazole film to characterize its oxidative stability performance. The greater the mass retention rate, the better the oxidative stability performance. The specific method is as follows:
[0092] Quality retention rate (%) = m (after film drying) / m (before film soaking);
[0093] 2. Alkali resistance test:
[0094] The alkali resistance of polyimidazole film was analyzed by its mechanical stability under alkaline conditions, and its mechanical stability was tested using an Instron 5565 universal tensile testing machine;
[0095] The specific test steps for alkali resistance are as follows: immerse a 15mm×5mm polyimidazole film in a 6mol / L sodium hydroxide solution at 60°C for 72h, take it out and wash it repeatedly with deionized water, dry it in an oven at 100°C, and then fix it on a tensile testing machine. Perform a tensile test at a tensile rate of 2mm / min, and record the change rate of the tensile strength of the polyimidazole film before and after immersion in sodium hydroxide to characterize its alkali resistance. The smaller the change rate of the tensile strength, the better the alkali resistance. The specific method is as follows:
[0096] Tensile strength change rate (%) = (tensile strength of the film before soaking in sodium hydroxide - tensile strength of the film after soaking in sodium hydroxide) / tensile strength of the film before soaking in sodium hydroxide;
[0097] 3. Mechanical properties test:
[0098] The mechanical properties of polyimidazole film were tested using an Instron 5565 universal tensile testing machine, and its mechanical properties were analyzed by the tensile strength of the polyimidazole film;
[0099] The specific test steps of mechanical properties are as follows: fix a 15mm×5mm polyimidazole film on a tensile testing machine, perform a tensile test at a tensile rate of 2mm / min, and record the tensile strength of the polyimidazole film. The specific method is as follows:
[0100] Tensile strength = tension / (polyimidazole film width × polyimidazole film thickness);
[0101] The above experimental results are shown in Table 1 below;
[0102] Table 1 Performance experimental results of various polyimidazole films
[0103]
[0104]
[0105] According to the experimental data in Table 1, Figure 7 , through analysis Figure 7 The following conclusions can be drawn:
[0106] First: The oxidation stability of fluorinated polyimidazole membrane is significantly better than that of non-fluorinated polyimidazole membrane;
[0107] Second: The alkali resistance of the cross-linked fluorinated polyimidazole membrane is significantly better than that of other non-cross-linked polyimidazole membranes.
[0108] Performance test experiment 2:
[0109] The proton exchange membrane in the above-mentioned embodiment 7 was subjected to the following performance test, and the specific test method is as follows:
[0110] 1. Mechanical properties test:
[0111] The mechanical properties of the proton exchange membrane were tested using an Instron 5565 universal tensile testing machine, and its mechanical properties were analyzed by the tensile strength of the proton exchange membrane;
[0112] The specific test steps for the mechanical properties of the proton exchange membrane are the same as the specific test steps for the mechanical properties of the polyimidazole membrane in the performance test experiment 1.
[0113] 2. Proton conduction performance test:
[0114] The proton conductivity of the proton exchange membrane was tested using the Autolab PGSTAT302N electrochemical workstation, and its proton conductivity was analyzed by the proton conductivity of the proton exchange membrane;
[0115] The specific test steps of proton conductivity performance are as follows: fix the 5cm×1cm proton exchange membrane on the electrode fixture of the electrochemical workstation, use the four-electrode method to test the impedance value of the membrane at 150°C, and calculate the proton conductivity of the proton exchange membrane. The specific method is as follows:
[0116] Proton conductivity = distance between two electrodes / (cross-sectional area of membrane × impedance of membrane);
[0117] The above experimental results are shown in Table 2 below;
[0118] Table 2 Performance test results of various proton exchange membranes
[0119]
[0120]
[0121] According to the experimental data in Table 2, Figure 8 , through analysis Figure 8 The following conclusions can be drawn:
[0122] The proton exchange membrane prepared by composite modification of polybenzimidazole by fluorination and cross-linking and loading MXene nanosheets not only significantly improved the proton conductivity performance but also obtained excellent mechanical properties. However, the proton exchange membrane prepared by only fluorination and cross-linking modification of polybenzimidazole performed poorly in proton conductivity.
Claims
1. A method for preparing a fluorinated polybenzimidazole proton exchange membrane, characterized in that: The steps include: Step 1: preparing a cross-linked fluorinated supported polybenzimidazole membrane: the epoxy functional group of the fluorinated cross-linking agent undergoes a ring-opening reaction with the amino functional group of the polybenzimidazole, and the hydrogen atoms of the hydroxyl groups carried on the surface of the MXene nanosheets form hydrogen bonds with the nitrogen atoms in the polybenzimidazole, thereby achieving a fluorinated cross-linked supported composite modification effect, and a cross-linked fluorinated supported polybenzimidazole membrane is prepared through a cross-linking curing reaction; The fluorinated cross-linking agent is cross-linking agent I or cross-linking agent II; The chemical structural formula of the crosslinking agent I is: ; The chemical structural formula of the crosslinking agent II is: ; Step 2: The cross-linked fluorinated supported polybenzimidazole membrane is first soaked in a potassium hydroxide solution for 6 to 20 hours, then soaked in deionized water for 6 to 20 hours, and finally soaked in an 85% phosphoric acid solution at 80 to 120° C. for 30 to 50 hours to prepare a fluorinated polybenzimidazole proton exchange membrane.
2. The method for preparing a fluorinated polybenzimidazole proton exchange membrane according to claim 1, characterized in that: The preparation method of the cross-linking agent I is: Step S2-1, generating a dipiperidyl fluorinated monomer by esterification reaction of the carboxyl functional group of 4,4'-(hexafluoroisopropylidene)bis(benzoic acid) with the hydroxyl functional group of 1-methyl-4-piperidinol; Step S2-2, using the nucleophilic substitution reaction mechanism, the tertiary amine functional group of the nucleophilic reagent dipiperidyl fluorinated monomer and the chlorine functional group of epichlorohydrin undergo quaternization reaction to generate crosslinking agent I.
3. The method for preparing a fluorinated polybenzimidazole proton exchange membrane according to claim 1, characterized in that: The preparation method of the crosslinking agent II is: Step S3-1, generating a tetrapiperidyl fluorinated monomer by esterification reaction of the carboxyl functional group of 4,4'-(2,2,2-trifluoro-1-trifluoromethyl)ethylenebis(1,2-phthalic acid) with the hydroxyl functional group of 1-methyl-4-piperidinol; Step S3-2, using the nucleophilic substitution reaction mechanism, the tertiary amine functional group of the tetrapiperidyl fluorinated monomer as a nucleophilic reagent and the chlorine functional group of epichlorohydrin undergo quaternization reaction to generate a crosslinking agent II.
4. The fluorinated polybenzimidazole proton exchange membrane prepared according to the method according to any one of claims 1 to 3, characterized in that: The fluorinated polybenzimidazole proton exchange membrane is an exchange membrane I prepared from a crosslinking agent I, MXene nanosheets and polybenzimidazole, or an exchange membrane II prepared from a crosslinking agent II, MXene nanosheets and polybenzimidazole.
5. The fluorinated polybenzimidazole proton exchange membrane according to claim 4, characterized in that: The fluorinated polybenzimidazole proton exchange membrane has a tensile strength of 7.5-10 MPa and a proton conductivity of 45-57 mS / cm.
Citation Information
Patent Citations
Preparation of novel covalent cross-linking polybenzimidazole proton exchange membrane
CN104151587A
Preparation method of crosslinking type polybenzimidazole proton exchange membrane
CN108400347A
Branching block-type polymer used for proton exchange membrane, preparation method and application
CN109286033A
Preparation method of cross-linked polybenzimidazole proton exchange membrane
CN112803052A
PDCPD material for 5G base station housing and preparation method thereof
CN114573953A