A nano zinc oxide toughening agent for plastics and preparation method thereof
By preparing nano zinc oxide toughening additives, combining graphene oxide and antibacterial base materials, the problem of insufficient toughness of plastics is solved, significantly improving the toughness and antibacterial properties of plastics, and providing flame retardant effects, suitable for a wide range of application.
Patent Information
- Application Number
- CN202410619181.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-18
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-05-18
AI Technical Summary
Existing plastic toughening additives cannot meet the increasingly stringent toughness requirements, and common additives are prone to cracks and cracks in the bonding areas, and lack antibacterial and flame retardant properties.
Using nano zinc oxide, graphene oxide solution, cetyl trimethyl ammonium bromide and antibacterial base materials, nano zinc oxide toughening additives are prepared through specific mixing and processing steps to improve the toughness and antibacterial effect of the plastic. and flame retardant properties.
It significantly improves the tensile strength and bending strength of plastics, enhances antibacterial ability, and provides auxiliary flame retardant effects, suitable for a wider market application.
Smart Images

Figure CN118325199B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plastic production, in particular to a nano zinc oxide toughening aid for plastics and a preparation method thereof. Background Art
[0002] Plastic is a high molecular compound made from monomers through addition polymerization or condensation polymerization. It has a medium deformation resistance, between fiber and rubber. It is composed of synthetic resin and additives such as fillers, toughening agents, stabilizers, lubricants, and colorants.
[0003] Toughening agents refer to substances that can increase the flexibility of the adhesive film layer. Some thermosetting resin adhesives, such as epoxy resins, phenolic resins and unsaturated polyester resins, have low elongation and high brittleness after curing. When the bonding parts are subjected to external forces, cracks are easily generated and rapidly expand, resulting in cracking of the adhesive layer. They are not fatigue-resistant and cannot be used for structural bonding. Therefore, it is necessary to find ways to reduce brittleness, increase toughness, and increase bearing strength. Any substance that can reduce brittleness, increase toughness, and does not affect the other main properties of the adhesive is a toughening agent. It can be divided into rubber toughening agents and thermoplastic elastomer toughening agents. However, common toughening agents cannot meet the increasingly stringent toughness requirements. Therefore, how to effectively improve the performance of toughening agents has become an important issue that needs to be urgently solved in my country's plastic processing industry.
[0004] Therefore, the present invention provides a nano zinc oxide toughening agent for plastics and a preparation method thereof, which are used to solve the above-mentioned related technical problems. Summary of the invention
[0005] The object of the present invention is to provide a nano zinc oxide toughening agent for plastics and a preparation method thereof. The nano zinc oxide toughening agent prepared by the present invention not only has a significant toughening effect, but also can significantly enhance the antibacterial effect of plastics; and also has an auxiliary flame retardant effect.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] The first aspect of the present invention provides a nano zinc oxide toughening agent for plastics, wherein the nano zinc oxide toughening agent is made of the following raw materials in parts by weight: 20 to 30 parts of a nano zinc oxide base material, 8 to 12 parts of a graphene oxide solution, 30 to 40 parts of hexadecyltrimethylammonium bromide, 6 to 10 parts of an antibacterial base material and 25 to 35 parts of deionized water.
[0008] The present invention is further configured as follows: the preparation process of the nano zinc oxide base material is as follows:
[0009] Place an appropriate amount of zinc acetate solution in an appropriate amount of sodium hydroxide solution at a volume ratio of 0.24 to 0.36:1, and mix at 50 to 80 r / min for 8 to 10 minutes;
[0010] Then treat it at 90-94°C for 12-14h, cool it to room temperature, filter it, rinse the product with deionized water for 4-8 times, and treat it in a drying oven at 80-90°C for 6-7h to obtain a nano zinc oxide base material.
[0011] The present invention is further configured as follows: the zinc acetate solution is prepared by mixing zinc acetate and deionized water at a solid-liquid ratio of 0.12 to 0.22 g / mL.
[0012] The present invention is further configured as follows: the sodium hydroxide solution is prepared by mixing sodium hydroxide and deionized water at a solid-liquid ratio of 0.08 to 0.15 g / mL.
[0013] The present invention is further configured as follows: the preparation process of the graphene oxide solution is as follows:
[0014] A proper amount of graphite oxide is fully dispersed in a proper amount of 50% ethanol aqueous solution at a solid-liquid ratio of 0.012-0.016 g / mL, and treated for 300-320 minutes at -5--1°C and 8000-10000 r / min to obtain a graphene oxide solution.
[0015] The present invention is further configured as follows: the preparation process of the antibacterial base material is as follows:
[0016] A proper amount of titanium dioxide nanotubes is fully dispersed in a proper amount of carvacrol at a solid-liquid ratio of 0.12 to 0.32 g / mL, and ultrasonically treated for 30 to 40 minutes at 2 to 10°C and 150 W power, and then placed in a vacuum drying oven for 40 to 50 minutes;
[0017] The mixture is then centrifuged at 8000-8200 r / min for 12-16 minutes, the obtained product is washed with anhydrous ethanol for 5-8 times, and then treated in a drying oven at 80-90° C. for 2-3 hours to obtain an antibacterial base material.
[0018] The second aspect of the present invention also provides a method for preparing the above-mentioned nano zinc oxide toughening agent for plastics, comprising the following steps:
[0019] Step 1, accurately weighing the nano zinc oxide base material, graphene oxide solution, hexadecyltrimethylammonium bromide, antibacterial base material and deionized water respectively, and then placing the nano zinc oxide base material, graphene oxide solution, hexadecyltrimethylammonium bromide, antibacterial base material and deionized water in a mixing device for mixing for 20 to 30 minutes to obtain a mixed material;
[0020] Step 2: drying the obtained mixture in an oven at 60-80°C for 60-100 minutes to obtain a dried product;
[0021] Step 3: Place the dried product in a tubular resistance furnace, evacuate the furnace, and then introduce H2. After the air is exhausted, heat the tubular resistance furnace to 280°C in a H2 atmosphere and keep it warm for 50 to 60 minutes. Cool the furnace to room temperature to obtain a finished product of nano zinc oxide toughening additive.
[0022] The present invention is further configured as follows: in step three, the heating rate of the tubular resistance furnace is 6-10° C. / min.
[0023] The present invention is further configured as follows: in step three, H2 is kept flowing during the process of cooling down to room temperature in the furnace.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The nano zinc oxide toughening agent prepared by the present invention is prepared from nano zinc oxide base material, graphene oxide solution, hexadecyl trimethyl ammonium bromide, antibacterial base material and deionized water as raw materials; the nano zinc oxide toughening agent prepared by the present invention not only has a significant toughening effect, but also can significantly improve the antibacterial effect of plastics; and also has an auxiliary flame retardant effect. The nano zinc oxide toughening agent for plastics provided by the present invention and the preparation method thereof have a broader market prospect and are more suitable for promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0027] Figure 1 It is a statistical diagram of the tensile strength of the present invention;
[0028] Figure 2 It is a statistical chart of the Escherichia coli sterilization rate of the present invention. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Embodiment 1:
[0031] The present embodiment provides a nano zinc oxide toughening agent for plastics, wherein the nano zinc oxide toughening agent is made of the following raw materials in parts by weight: 20 parts of nano zinc oxide base material, 8 parts of graphene oxide solution, 30 parts of hexadecyltrimethylammonium bromide, 6 parts of antibacterial base material and 25 parts of deionized water.
[0032] Among them, the preparation process of nano zinc oxide base material is as follows:
[0033] Place an appropriate amount of zinc acetate solution in an appropriate amount of sodium hydroxide solution at a volume ratio of 0.24:1 and mix at 50 r / min for 8 minutes;
[0034] Then, the mixture was treated at 90° C. for 12 h, cooled to room temperature, and filtered. The obtained product was rinsed with deionized water for 4 times, and then treated in a drying oven at 80° C. for 6 h to obtain a nano zinc oxide base material.
[0035] Furthermore, the zinc acetate solution is prepared by mixing zinc acetate and deionized water at a solid-liquid ratio of 0.12 g / mL.
[0036] The sodium hydroxide solution is prepared by mixing sodium hydroxide and deionized water at a solid-liquid ratio of 0.08 g / mL.
[0037] In addition, the preparation process of graphene oxide solution is as follows:
[0038] An appropriate amount of graphite oxide was fully dispersed in an appropriate amount of 50% ethanol aqueous solution at a solid-liquid ratio of 0.012 g / mL, and treated at -5°C and 8000 r / min for 300 min to obtain a graphene oxide solution.
[0039] The preparation process of the antibacterial base material is as follows:
[0040] An appropriate amount of titanium dioxide nanotubes was fully dispersed in an appropriate amount of carvacrol at a solid-liquid ratio of 0.12 g / mL, and ultrasonically treated for 30 min at 2°C and 150 W power, and then placed in a vacuum drying oven and maintained at pressure for 40 min;
[0041] The mixture was centrifuged at 8000 r / min for 12 min, and the product was washed 5 times with anhydrous ethanol and then treated in a drying oven at 80° C. for 2 h to obtain an antibacterial base material.
[0042] In addition, this embodiment also provides a method for preparing a nano zinc oxide toughening agent for plastics, comprising the following steps:
[0043] Step 1: Accurately weigh the nano zinc oxide base material, graphene oxide solution, hexadecyltrimethylammonium bromide, antibacterial base material and deionized water respectively, and then place the nano zinc oxide base material, graphene oxide solution, hexadecyltrimethylammonium bromide, antibacterial base material and deionized water in a mixing device for mixing for 20 minutes to obtain a mixed material.
[0044] Step 2: Place the obtained mixture in an oven at 60°C and dry it for 60 minutes to obtain a dry product.
[0045] Step 3: Place the dried product in a tubular resistance furnace, evacuate the furnace, and then introduce H2. After the air is exhausted, heat the tubular resistance furnace to 280°C in a H2 atmosphere and keep it warm for 50 minutes. Cool the furnace to room temperature to obtain a finished product of nano zinc oxide toughening additive.
[0046] Among them, the heating rate of the tubular resistance furnace is 6℃ / min.
[0047] The H2 flow was maintained during the furnace cooling to room temperature.
[0048] Embodiment 2:
[0049] The present embodiment provides a nano zinc oxide toughening agent for plastics, wherein the nano zinc oxide toughening agent is made of the following raw materials in parts by weight: 25 parts of nano zinc oxide base material, 10 parts of graphene oxide solution, 35 parts of hexadecyltrimethylammonium bromide, 8 parts of antibacterial base material and 30 parts of deionized water.
[0050] Among them, the preparation process of nano zinc oxide base material is as follows:
[0051] Place an appropriate amount of zinc acetate solution in an appropriate amount of sodium hydroxide solution at a volume ratio of 0.3:1, and mix at 650 r / min for 9 minutes;
[0052] Then, the mixture was treated at 92° C. for 13 h, cooled to room temperature, and filtered. The obtained product was rinsed with deionized water for 6 times, and then treated in a drying oven at 85° C. for 7 h to obtain a nano zinc oxide base material.
[0053] Furthermore, the zinc acetate solution is prepared by mixing zinc acetate and deionized water at a solid-liquid ratio of 0.17 g / mL.
[0054] The sodium hydroxide solution is prepared by mixing sodium hydroxide and deionized water at a solid-liquid ratio of 0.12 g / mL.
[0055] In addition, the preparation process of graphene oxide solution is as follows:
[0056] An appropriate amount of graphite oxide was fully dispersed in an appropriate amount of 50% ethanol aqueous solution at a solid-liquid ratio of 0.014 g / mL, and treated at -3°C and 9000 r / min for 310 min to obtain a graphene oxide solution.
[0057] The preparation process of the antibacterial base material is as follows:
[0058] An appropriate amount of titanium dioxide nanotubes was fully dispersed in an appropriate amount of carvacrol at a solid-liquid ratio of 0.22 g / mL, and ultrasonically treated at 8°C and 150 W for 35 min, and then placed in a vacuum drying oven for 45 min;
[0059] The mixture was centrifuged at 8100 r / min for 14 min, and the product was washed 6 times with anhydrous ethanol and then treated in a drying oven at 85° C. for 3 h to obtain an antibacterial base material.
[0060] In addition, this embodiment also provides a method for preparing a nano zinc oxide toughening agent for plastics, comprising the following steps:
[0061] Step 1: Accurately weigh the nano zinc oxide base material, graphene oxide solution, hexadecyltrimethylammonium bromide, antibacterial base material and deionized water respectively, and then place the nano zinc oxide base material, graphene oxide solution, hexadecyltrimethylammonium bromide, antibacterial base material and deionized water in a mixing device for mixing for 25 minutes to obtain a mixed material.
[0062] Step 2: Place the obtained mixture in an oven at 70°C and dry it for 80 minutes to obtain a dry product.
[0063] Step 3: Place the dried product in a tubular resistance furnace, evacuate the furnace, and then introduce H2. After the air is exhausted, heat the tubular resistance furnace to 280°C in a H2 atmosphere and keep it warm for 55 minutes. Cool the furnace to room temperature to obtain a finished nano zinc oxide toughening agent.
[0064] Among them, the heating rate of the tubular resistance furnace is 8℃ / min.
[0065] The H2 flow was maintained during the furnace cooling to room temperature.
[0066] Embodiment 3:
[0067] The present embodiment provides a nano zinc oxide toughening agent for plastics, wherein the nano zinc oxide toughening agent is made of the following raw materials in parts by weight: 30 parts of nano zinc oxide base material, 12 parts of graphene oxide solution, 40 parts of hexadecyltrimethylammonium bromide, 10 parts of antibacterial base material and 35 parts of deionized water.
[0068] Among them, the preparation process of nano zinc oxide base material is as follows:
[0069] Place an appropriate amount of zinc acetate solution in an appropriate amount of sodium hydroxide solution at a volume ratio of 0.36:1, and mix at 80 r / min for 10 min;
[0070] Then, the mixture was treated at 94° C. for 14 h, cooled to room temperature, and filtered. The obtained product was rinsed with deionized water for 8 times, and then treated in a drying oven at 90° C. for 7 h to obtain a nano zinc oxide base material.
[0071] Furthermore, the zinc acetate solution is prepared by mixing zinc acetate and deionized water at a solid-liquid ratio of 0.22 g / mL.
[0072] The sodium hydroxide solution is prepared by mixing sodium hydroxide and deionized water at a solid-liquid ratio of 0.15 g / mL.
[0073] In addition, the preparation process of graphene oxide solution is as follows:
[0074] An appropriate amount of graphite oxide was fully dispersed in an appropriate amount of 50% ethanol aqueous solution at a solid-liquid ratio of 0.016 g / mL, and treated at -1°C and 1000 r / min for 320 min to obtain a graphene oxide solution.
[0075] The preparation process of the antibacterial base material is as follows:
[0076] An appropriate amount of titanium dioxide nanotubes was fully dispersed in an appropriate amount of carvacrol at a solid-liquid ratio of 0.32 g / mL, and ultrasonically treated at 10°C and 150 W for 40 min, and then placed in a vacuum drying oven for 50 min;
[0077] The mixture was centrifuged at 8200 r / min for 16 min, and the product was washed 8 times with anhydrous ethanol and then treated in a drying oven at 90° C. for 3 h to obtain an antibacterial base material.
[0078] In addition, this embodiment also provides a method for preparing a nano zinc oxide toughening agent for plastics, comprising the following steps:
[0079] Step 1: Accurately weigh the nano zinc oxide base material, graphene oxide solution, hexadecyltrimethylammonium bromide, antibacterial base material and deionized water respectively, and then place the nano zinc oxide base material, graphene oxide solution, hexadecyltrimethylammonium bromide, antibacterial base material and deionized water in a mixing device for mixing for 30 minutes to obtain a mixed material.
[0080] Step 2: Place the obtained mixture in an oven at 80°C and dry it for 100 minutes to obtain a dry product.
[0081] Step 3: Place the dried product in a tubular resistance furnace, evacuate the furnace, and then introduce H2. After the air is exhausted, heat the tubular resistance furnace to 280°C in a H2 atmosphere and keep it warm for 60 minutes. Cool the furnace to room temperature to obtain a finished product of nano zinc oxide toughening additive.
[0082] Among them, the heating rate of the tubular resistance furnace is 10℃ / min.
[0083] The H2 flow was maintained during the furnace cooling to room temperature.
[0084] Comparative Example 1: The preparation method of the nano zinc oxide toughening agent and the specific ratio of raw materials provided in this example are substantially the same as those in Example 1, with the main difference being that the nano zinc oxide base material in this example is replaced by commercially available nano zinc oxide (purchased from Shandong Baiya Chemical Co., Ltd.).
[0085] Comparative Example 2: The preparation method of the nano zinc oxide toughening agent and the specific ratio of raw materials provided in this example are substantially the same as those in Example 1, with the main difference being that this example does not contain a graphene oxide solution.
[0086] Comparative Example 3: The preparation method of the nano zinc oxide toughening agent provided in this embodiment and the specific ratio of the raw materials are substantially the same as those in Example 1, the main difference being that: this embodiment does not contain an antibacterial base material;
[0087] Comparative Example 4: The preparation method of the nano zinc oxide toughening agent and the specific ratio of raw materials provided in this example are substantially the same as those in Example 1, the main difference being that step three is not included.
[0088] Effect test
[0089] The nano zinc oxide toughening aids prepared by Examples 1 to 3 of the present invention are respectively recorded as Experimental Examples 1 to 3; the nano zinc oxide toughening aids prepared by Comparative Examples 1 to 4 are recorded as Comparative Examples 1 to 4; 30 parts of copolymerized polypropylene, 12 parts of nano zinc oxide toughening aids, 5 parts of cross-linking agent TMPTA, 0.2 parts of antioxidant 1010 and 12 parts of fatty acid amide are uniformly mixed, and the mixed product is added to a twin-screw extruder for extrusion and blending, and the screw speed is set to 350 rpm. After the extrudate is water-cooled, it is cut into the required size and then dried to obtain a toughened plastic product; then the performance of equal amounts of each group of samples is tested.
[0090] Test 1. Mechanical properties test and result analysis:
[0091] The tensile strength of plastic products was measured according to the testing standard of GB / T1040.1-2018, and the flexural strength of plastic products was measured according to the testing standard of GB / T9341-2008. The relevant data are recorded in Table 1.
[0092] Table 1: Test data record table
[0093] Group Tensile strength(MPa) Bending strength(MPa) Example 1 Group 28 34 Example 1 Group 28 33 Example 1 Group 27 33 Comparison group 1 16 22 Comparison of 2 groups 20 24 Comparison of 3 groups 18 23 Comparison of 4 groups 26 33
[0094] From Table 1 and Figure 1 It can be seen that compared with the control group, the nano zinc oxide toughening agents of Examples 1 to 3 can significantly improve the tensile strength and bending strength of plastic products, and at the same time, the difference between the example groups is not obvious. The above results show that the nano zinc oxide toughening agents of Examples 1 to 3 have a significant toughening effect.
[0095] In order to verify the effects of the various components of the additive, experiments of Comparative Examples 1 to 4 were set up.
[0096] The main difference between the raw material ratio of the nano zinc oxide toughening agent in Comparative Example 1 and Example 1 is that the nano zinc oxide base material is replaced by commercially available nano zinc oxide. Compared with the Example 1 group, it was found that the tensile strength of the Comparative Example 1 group was reduced by 12MPa and the bending strength was reduced by 12MPa. This result shows that the nano zinc oxide base material plays an important role in improving the toughening performance of plastics.
[0097] The main difference between the raw material ratio of the nano zinc oxide toughening agent in Comparative Example 2 and Example 1 is that the graphene oxide solution is not contained. Compared with the group in Example 1, it is found that the tensile strength of the group in Comparative Example 2 is reduced by 8MPa and the bending strength is reduced by 10MPa. This result shows that the graphene oxide solution plays a certain role in improving the toughening performance of plastics.
[0098] The main difference between the raw material ratio of the nano zinc oxide toughening agent in Comparative Example 3 and Example 1 is that the antibacterial base material is not included. Compared with the group in Example 1, it was found that the tensile strength of the group in Comparative Example 3 was reduced by 2MPa and the bending strength was reduced by 11MPa. This result shows that the antibacterial base material plays a role in improving the toughening performance of plastics.
[0099] The main difference between the raw material ratio of nano zinc oxide toughening agent in comparative example 4 and example 1 is that step 3 is not included. Compared with the group in example 1, the tensile strength of the comparative example 4 group was reduced by 10 MPa and the bending strength was reduced by 1 MPa. This result shows that step 3 has little effect on improving the toughening performance of plastics.
[0100] Test 2, antibacterial test and result analysis:
[0101] The antibacterial performance test was carried out according to the test standard of QB / T2591-2003A, and the relevant data were recorded in Table 2.
[0102] Table 2: Test data record table
[0103] Group Escherichia coli sterilization rate (%) Staphylococcus aureus sterilization rate (%) Example 1 Group 98 97 Example 1 Group 98 98 Example 1 Group 97 98 Comparison group 1 95 96 Comparison of 2 groups 90 92 Comparison of 3 groups 85 88 Comparison of 4 groups 90 91
[0104] From Table 2 and Figure 2 It can be seen that compared with the control group, the nano zinc oxide toughening agents of Examples 1, 2, and 3 can significantly improve the sterilization rate of Escherichia coli and Staphylococcus aureus; at the same time, the difference between the example groups is not obvious. The above results show that the nano zinc oxide toughening agents of Examples 1 to 3 have significant antibacterial effects.
[0105] In order to verify the effects of the various components of the additive, experiments of Comparative Examples 1 to 4 were set up.
[0106] The main difference between the raw material ratio of the nano zinc oxide toughening agent in Comparative Example 1 and Example 1 is that the nano zinc oxide base material is replaced by commercially available nano zinc oxide. Compared with the Example 1 group, it was found that the bactericidal rate of Escherichia coli in the Comparative Example 1 group was reduced by 2%, and the bactericidal rate of Staphylococcus aureus was reduced by 1%. This result shows that the nano zinc oxide base material has little effect on improving the antibacterial properties of plastics.
[0107] The main difference between the raw material ratio of the nano zinc oxide toughening agent in Comparative Example 2 and Example 1 is that the graphene oxide solution is not included. Compared with the Example 1 group, the bactericidal rate of Escherichia coli in Comparative Example 2 was reduced by 8%, and the bactericidal rate of Staphylococcus aureus was reduced by 5%. This result shows that the graphene oxide solution plays a certain role in improving the antibacterial properties of plastics.
[0108] The main difference between the raw material ratio of the nano zinc oxide toughening agent in Comparative Example 3 and Example 1 is that the antibacterial base material is not included. Compared with the Example 1 group, it was found that the bactericidal rate of Escherichia coli in Comparative Example 3 group was reduced by 13%, and the bactericidal rate of Staphylococcus aureus was reduced by 9%. This result shows that the antibacterial base material plays an important role in improving the antibacterial properties of plastics.
[0109] The main difference between the raw material ratio of the nano zinc oxide toughening agent in Comparative Example 4 and Example 1 is that step 3 is not included. Compared with Example 1, the sterilization rate of Escherichia coli in Comparative Example 4 was reduced by 8% and the sterilization rate of Staphylococcus aureus was reduced by 6%. This result shows that step 3 has an effect on improving the antibacterial properties of plastics.
[0110] Test 3, antibacterial test and result analysis:
[0111] The flame retardant performance test was carried out according to the test standard of GB / T2406-93, and the relevant data were recorded in Table 3.
[0112] Table 3: Test data record table
[0113]
[0114]
[0115] As shown in Table 3, compared with the control group, the nano zinc oxide toughening agents of Examples 1, 2, and 3 can significantly improve the flame retardant properties; at the same time, the differences between the example groups are not obvious. The above results show that the nano zinc oxide toughening agents of Examples 1 to 3 have the effect of improving the flame retardant properties of plastics.
[0116] In order to verify the effects of the various components of the additive, experiments of Comparative Examples 1 to 4 were set up.
[0117] The main difference between the raw material ratio of the nano zinc oxide toughening agent in Comparative Example 1 and Example 1 is that the nano zinc oxide base material is replaced by commercially available nano zinc oxide. Compared with the Example 1 group, it is found that the oxygen index of the Comparative Example 1 group is reduced by 1%. This result shows that the nano zinc oxide base material has little effect on improving the flame retardant properties of plastics.
[0118] The main difference between the raw material ratio of the nano zinc oxide toughening agent in Comparative Example 2 and Example 1 is that the graphene oxide solution is not contained. Compared with the group in Example 1, it is found that the oxygen index of the comparative example 2 group is reduced by 10%. This result shows that the graphene oxide solution plays an important role in improving the flame retardant properties of plastics.
[0119] The main difference between the raw material ratio of the nano zinc oxide toughening agent in Comparative Example 3 and Example 1 is that the antibacterial base material is not included. Compared with the group in Example 1, it is found that the oxygen index of the group in Comparative Example 3 is reduced by 5%. This result shows that the antibacterial base material plays a certain role in improving the flame retardant properties of plastics.
[0120] The main difference between the raw material ratio of the nano zinc oxide toughening agent in Comparative Example 4 and Example 1 is that step 3 is not included. Compared with Example 1, the oxygen index of Comparative Example 4 is reduced by 7%. This result shows that step 3 has an effect on improving the flame retardant properties of plastics.
[0121] From the above, it can be seen that the nano zinc oxide toughening agent prepared by the present invention not only has a significant toughening effect, but also can significantly enhance the antibacterial effect of plastics; and also has an auxiliary flame retardant effect. This shows that the nano zinc oxide toughening agent produced by the present invention has a broader market prospect and is more suitable for promotion.
[0122] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0123] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A nano zinc oxide toughening agent for plastics, characterized in that: The nano zinc oxide toughening aid is made of the following raw materials in parts by weight: 20 to 30 parts of nano zinc oxide base material, 8 to 12 parts of graphene oxide solution, 30 to 40 parts of hexadecyltrimethylammonium bromide, 6 to 10 parts of antibacterial base material and 25 to 35 parts of deionized water; The preparation process of the nano zinc oxide base material is as follows: Place the zinc acetate solution in the sodium hydroxide solution at a volume ratio of 0.24 to 0.36:1 and mix at 50 to 80 r / min for 8 to 10 minutes; Then, the mixture is treated at 90-94°C for 12-14 hours, cooled to room temperature, filtered, and the obtained product is rinsed with deionized water for 4-8 times, and then treated in a drying oven at 80-90°C for 6-7 hours to obtain a nano zinc oxide base material; The preparation process of the antibacterial base material is as follows: The titanium dioxide nanotubes are fully dispersed in carvacrol at a solid-liquid ratio of 0.12 to 0.32 g / mL, and ultrasonically treated at 2 to 10°C and 150 W for 30 to 40 minutes, and then placed in a vacuum drying oven for 40 to 50 minutes; The product is then centrifuged at 8000-8200 r / min for 12-16 minutes, washed with anhydrous ethanol for 5-8 times, and then treated in a drying oven at 80-90° C. for 2-3 hours to obtain an antibacterial base material; The preparation method of the nano zinc oxide toughening agent for plastics comprises the following steps: Step 1, accurately weighing the nano zinc oxide base material, graphene oxide solution, hexadecyltrimethylammonium bromide, antibacterial base material and deionized water respectively, and then placing the nano zinc oxide base material, graphene oxide solution, hexadecyltrimethylammonium bromide, antibacterial base material and deionized water in a mixing device for mixing for 20 to 30 minutes to obtain a mixed material; Step 2: drying the obtained mixture in an oven at 60-80°C for 60-100 minutes to obtain a dried product; Step 3: Place the dried product in a tubular resistance furnace, evacuate the furnace, and then introduce H2. After the air is exhausted, heat the tubular resistance furnace to 280°C in a H2 atmosphere and keep it warm for 50 to 60 minutes. Cool the furnace to room temperature to obtain a finished product of nano zinc oxide toughening additive.
2. A nano zinc oxide toughening agent for plastics according to claim 1, characterized in that: The zinc acetate solution is prepared by mixing zinc acetate and deionized water at a solid-liquid ratio of 0.12 to 0.22 g / mL.
3. A nano zinc oxide toughening agent for plastics according to claim 1, characterized in that: The sodium hydroxide solution is prepared by mixing sodium hydroxide and deionized water at a solid-liquid ratio of 0.08 to 0.15 g / mL.
4. A nano zinc oxide toughening agent for plastics according to claim 1, characterized in that: The preparation process of the graphene oxide solution is as follows: The graphite oxide is fully dispersed in a 50% ethanol aqueous solution at a solid-liquid ratio of 0.012-0.016 g / mL, and treated at -5--1°C and 8000-10000 r / min for 300-320 minutes to obtain a graphene oxide solution.
5. A method for preparing a nano zinc oxide toughening agent for plastics according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1, accurately weighing the nano zinc oxide base material, graphene oxide solution, hexadecyltrimethylammonium bromide, antibacterial base material and deionized water respectively, and then placing the nano zinc oxide base material, graphene oxide solution, hexadecyltrimethylammonium bromide, antibacterial base material and deionized water in a mixing device for mixing for 20 to 30 minutes to obtain a mixed material; Step 2: drying the obtained mixture in an oven at 60-80°C for 60-100 minutes to obtain a dried product; Step 3: Place the dried product in a tubular resistance furnace, evacuate the furnace, and then introduce H2. After the air is exhausted, heat the tubular resistance furnace to 280°C in a H2 atmosphere and keep it warm for 50 to 60 minutes. Cool the furnace to room temperature to obtain a finished product of nano zinc oxide toughening additive.
6. The method for preparing a nano zinc oxide toughening agent for plastics according to claim 5, characterized in that: In step three, the heating rate of the tubular resistance furnace is 6-10° C. / min.
7. The method for preparing a nano zinc oxide toughening agent for plastics according to claim 5, characterized in that: In step 3, H2 is kept flowing during the process of cooling down to room temperature in the furnace.