Preparation method of manganese single atom nanocatalyst
The preparation of manganese single-atom hollow nanocube catalysts through metal-organic framework templates solves the problem of preparing manganese single-atom nanocatalysts, achieves efficient degradation of tetracycline, and demonstrates strong adsorption and photocatalytic capabilities.
Patent Information
- Application Number
- CN202410752661.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-06-12
AI Technical Summary
Existing technologies fail to effectively prepare and apply manganese single-atom nanocatalysts, making it difficult to efficiently remove pollutants such as tetracycline in the environment.
Using a metal-organic framework as a template, a hollow structure is formed through acid etching, and manganese ions are adsorbed through ion exchange, followed by high-temperature carbonization to prepare Mn-N3 coordinated manganese single-atom hollow nanocube catalysts for adsorption, enzyme-like catalysis and photocatalysis. Catalyzes the degradation of tetracycline.
Efficient preparation of manganese single-atom catalyst has been achieved. It has low cost, strong adsorption capacity and good photocatalytic performance. It can degrade 50mg/L tetracycline by 95% and 100mg/L by 76% in 10 minutes. It is suitable for a variety of pollutants. degradation.
Smart Images

Figure CN118341984B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of environmental material synthesis, and in particular, to a method for preparing a manganese single-atom nanocatalyst. Background Art
[0002] This section is intended to provide a background or context to what is stated in the claims or specification, and no admission is made that what is described herein is prior art by inclusion in this section.
[0003] Antibiotics are organic compounds that can inhibit the growth and death of various harmful microorganisms. Due to their excellent bactericidal effects, antibiotics have been used in large quantities in recent years. In 2013, the use of antibiotics in my country reached 162,000 tons, and more than 500,000 tons of antibiotics are directly discharged into the environment every year. However, a large amount of antibiotics remaining in the environment will have an impact on the ecosystem. For example, antibiotics can kill or prevent the growth of microorganisms, so they are likely to break the delicate balance of microorganisms in the ecosystem. For example, the microbial activities in the treatment of domestic sewage (septic tanks) and community or industrial sewage treatment plants will be destroyed by antibiotic residues in the wastewater. At the same time, residual antibiotics are biologically toxic and, like most other environmentally active pharmaceutical ingredients, may be harmful to plants, animals and humans. Antibiotics that exist in the environment for a long time can have chronic toxic effects on organisms. Antibiotic substances can be enriched through the food chain, accumulated and amplified in highly developed plants and animals, and produce irreversible changes. Most importantly, antibiotic residues can cause organisms to produce antibiotic resistance genes. This will damage the therapeutic effect of antibiotics and endanger public health safety. Bacteria exposed to antibiotics in the environment may accelerate the persistence or emergence of antibiotic resistance genes, resulting in potential harm to ecosystems and human health.
[0004] In order to reduce the harm that tetracycline may cause to the ecological environment and human health, it is necessary to remove it from natural water bodies and wastewater. So far, a lot of work has been carried out in this field, such as removal of tetracycline from water bodies by adsorption, biodegradation, ion exchange, membrane filtration and photocatalytic degradation. Among them, photocatalytic degradation of tetracycline is considered to be the most favorable method because it has the advantages of low cost, high treatment efficiency, mild reaction conditions and no secondary pollution.
[0005] The metal-organic framework structure composed of metal ions and organic ligands has received increasing attention in recent years due to its extensive application in adsorption and photocatalysis. This material has a specific three-dimensional structure and a series of properties, such as a large specific surface area, strong chemical and thermal stability, and the ability to use different ligands for functional design. At the same time, the metal-organic framework also has good conductivity and excellent electron transfer performance. It is an excellent photocatalytic material that can improve the efficiency of photocatalysis.
[0006] The use of metal organic frameworks as templates to load metal single atoms to form catalysts has developed rapidly in the past few years. Many studies have shown that supported single atom catalysts exhibit excellent catalytic performance in many catalysis, and have very high activity and stability in some catalytic reactions. This is mainly because of the strong interaction between single metal atoms and the coordinating atoms in the carrier. In addition, the unique coordination mode between single metal atoms and the coordinating atoms in the carrier also makes single atom catalysts have structures similar to homogeneous catalysts and enzyme catalysts. The concept of single atom enzyme (SAzyme) proposed in 2019 shows that single atom Fe catalysts with FeN4 active centers have catalase and superoxide dismutase activities, which can effectively remove reactive oxygen species (ROS) in cells. At the same time, single atom catalysts have also attracted widespread attention in the field of photocatalysis due to their advantages such as maximum atomic utilization and fully exposed active sites. By combining Pt single atoms with defective TiO2 carriers, single atom catalysts with good photocatalytic performance were successfully prepared, which promoted the generation of oxygen vacancies on the adjacent TiO2 surface and generated Pt-O-Ti 3+ atomic interface layer, which helps to promote the photogenerated electrons from Ti to 3+ Defect sites migrate to the Pt single-atom active sites, thereby increasing the separation rate of photogenerated electron-hole pairs and greatly improving the photocatalytic HER efficiency. In addition, some MOFs contain special groups that show certain response signals to ultraviolet light or visible light; at the same time, the pore-rich characteristics of MOFs can reduce the migration distance of carriers, which can effectively solve the common problem of electron-hole recombination in conventional semiconductors, and further promote the improvement of their photocatalytic efficiency. Furthermore, composite metal single atoms can not only give play to the optical properties of MOFs, but also utilize the excellent characteristics of single atoms to coordinate and optimize the charge separation efficiency in the photolysis of pollutants to improve degradation capabilities.
[0007] Single-atom catalysts have a clear chemical environment of active centers and are currently the best candidate materials for Fenton-like catalytic reactions. Single-atom nanozymes have highly exposed and clear active sites, thus producing excellent catalytic performance, which can achieve in situ degradation of materials and photocatalytic degradation of pollutants. Applying them to the design of MOF materials can construct a trifunctional material that can adsorb, in situ catalytically degrade pollutants, and photocatalytically degrade pollutants.
[0008] To address the above-mentioned problems, no effective solution has been proposed yet. Summary of the invention
[0009] The embodiment of the present application provides a method for preparing a manganese single-atom nanocatalyst to at least solve the technical problem that manganese single-atom nanocatalysts cannot be prepared in the related art. The catalyst is a solid-phase catalyst with a three-dimensional hollow structure and a particle size of about 150-250nm. It has the characteristics of low catalyst cost, high atomic loading rate and utilization rate, strong adsorption capacity, high enzyme-like catalytic ability and good photocatalytic ability. Using a metal organic framework as a template, after acid etching to form a hollow, manganese ions are adsorbed by ion exchange, and finally a manganese single-atom hollow nanocube is formed by high-temperature carbonization. The crystal plane structure and valence state changes of the manganese element in the material are analyzed by using XRD and XPS; the surface morphology, internal structure and element distribution of the material are observed and analyzed by SEM, TEM and HRTEM; the single-atom morphology and coordination of manganese in the material are analyzed by high-angle annular dark field scanning transmission (HAADF-STEM) and X-ray absorption fine structure spectrum (XAFS). At the same time, it was applied to the degradation of tetracycline, and a high efficiency degradation was obtained, with 95% degradation within 10 minutes for 50 mg / L TC and 76% degradation within 10 minutes for 100 mg / L TC.
[0010] According to one aspect of an embodiment of the present application, a method for preparing a manganese single-atom nanocatalyst is provided, comprising the following steps:
[0011] Step 1: Synthesis of solid nanocubes: First, weigh an appropriate amount of organic ligand, dissolve it in deionized water, stir it magnetically, and mark it as solution A; secondly, weigh a metal ion source and an activator, dissolve them in deionized water, ultrasonicate for 10-20 minutes to achieve uniform dispersion, and mark it as solution B. While solution A is being stirred magnetically at high speed, slowly pour solution B into it. Finally, stir the two vigorously for 120 minutes to obtain a uniform solution. After centrifugation at 12000rpm, dry the obtained solid at 40 degrees vacuum overnight, and grind it to obtain a powder, which is a solid nanocube;
[0012] Step 2: Synthesis of hollow nanocubes: First, weigh the solid nanocubes obtained in step 1 and dissolve them in deionized water, which is labeled as solution C; secondly, weigh an appropriate amount of acid and dissolve it in deionized water, which is labeled as solution D; finally, slowly pour solution D into solution C during magnetic stirring to perform etching reaction, and vigorously stir for 150 minutes to obtain a uniform solution, which is centrifuged at 10,000 rpm and washed three times to obtain a solid, which is dissolved in deionized water and labeled as solution E;
[0013] Step 3: Adding metal salt: First, accurately weigh the metal salt and dissolve it in deionized water, which is marked as solution F. Then, pour solution F into solution E during high-speed magnetic stirring, centrifuge at 10,000 rpm to obtain a solid, and freeze-dry it in a freeze dryer for 48 hours to obtain a powder;
[0014] Step 4: high temperature carbonization in a tubular furnace: the powder obtained by freeze drying in step 3 is placed in a tubular furnace for high temperature carbonization under the condition of passing an inert gas to prevent oxidation. The product obtained after cooling is the Mn SACs manganese single atom nanocatalyst.
[0015] Optionally, the organic ligand in step 1 is any one of 2-methylimidazole and o-diazine.
[0016] Optionally, the above-mentioned metal ion source is any one of zinc sulfate (ZnSO4), zinc chloride (ZnCl2), zinc nitrite (Zn(NO2)2), zinc nitrate (Zn(NO3)2), zinc nitrate hexahydrate (Zn(NO3)2·6H2O), and zinc acetate (Zn(O2CCH3)2).
[0017] Optionally, the activator is any one of cetyltrimethylammonium bromide (CTAB) and polyvinylpyrrolidone (PVP).
[0018] Optionally, the acid used in the acid etching is acetic acid (CH3COOH), hydrofluoric acid (HF) and tannic acid (C 76 H 52 O 46 )
[0019] Optionally, the metal salt is any one of manganese chloride tetrahydrate (MnCl2·4H2O), manganese sulfate monohydrate (MnSO4·H2O), manganese nitrate (Mn(NO3)2), and manganese nitrite (Mn(NO2)2).
[0020] Optionally, in step 1, solution A: the concentration of the organic ligand solution is (0.05 - 0.1) g / mL. Solution B: the concentration of the metal ion source is (0.01 -0.1) g / mL, and the concentration of the activator is (0.001-0.01) g / mL. Solution A and solution B are mixed in a ratio of one to one.
[0021] Optionally, in step 2, solution C: weigh the powder obtained in step 1 and dissolve it in deionized water in a ratio of 1: (100-300). Solution D: the ratio of etching acid to deionized water is (1-1.5): 1. Solution C and solution D are mixed in a ratio of 1: 1.
[0022] Optionally, the solid obtained in step 2 is dissolved in deionized water in a ratio of (1-3):200, and after being uniformly mixed by ultrasonication for 10 minutes to form solution E, 1300-1800 ml of deionized water is added to solution E for dilution, and then solution F is added; the ratio of manganese metal salt to deionized water in solution F is 1:(3-6).
[0023] Optionally, in step 4, the heating rate of the tubular furnace is 1-10°C / s, the reaction temperature is 800-1200°C, and the holding time is 120-360 minutes.
[0024] The Mn-N3 coordinated manganese single atom hollow nanocube catalyst prepared in the present application is a three-dimensional hollow cubic structure, and the loading amount of manganese single atoms is (0.01-8.00) wt%.
[0025] The Mn-N3 coordinated manganese single atom hollow nanocube catalyst provided in the present application can be applied to adsorption degradation, enzyme-like catalytic degradation and photocatalytic degradation of tetracycline, and the specific scheme is as follows:
[0026] The Mn-N3 coordinated manganese single atom catalyst is added to the wastewater to be treated which also contains tetracycline. The pH of the wastewater is between 2-10 and the pollutant concentration is between 10-150 mg / mL. Magnetic stirring is performed during the reaction. After reaching adsorption equilibrium, a xenon lamp is turned on for photocatalytic reaction to degrade tetracycline pollutants in the wastewater.
[0027] Optionally, the mass ratio of the Mn-N3 coordinated manganese single atom catalyst to the wastewater is (0.01-0.1):100, the xenon lamp power is 300-450W, and the light source is filtered to (400-800) nm.
[0028] In the technical solution of this application, the polluted media that can be treated include: antibiotics, pesticides, endocrine disruptors, flame retardants, dyes, polycyclic aromatic hydrocarbons and polychlorinated biphenyls, especially for water bodies contaminated by antibiotics, pesticides and endocrine disruptors.
[0029] All temperatures specified in this application are carried out under room temperature.
[0030] According to another aspect of an embodiment of the present application, a storage medium is further provided, which includes a stored program, and the above method is executed when the program is run.
[0031] According to another aspect of an embodiment of the present application, an electronic device is further provided, including a memory, a processor, and a computer program stored in the memory and executable on the processor, wherein the processor executes the above method through the computer program.
[0032] According to one aspect of the present application, a computer program product or a computer program is provided, the computer program product or the computer program comprising computer instructions, the computer instructions being stored in a computer-readable storage medium. A processor of a computer device reads the computer instructions from the computer-readable storage medium, and the processor executes the computer instructions, so that the computer device performs the steps of any one of the embodiments of the above method.
[0033] The present application uses an etched organic framework as a template, loads manganese atoms through ion exchange adsorption, and obtains a Mn SACs-coordinated manganese single-atom hollow nanocube catalyst through high-temperature carbonization. It degrades organic pollutants through adsorption, enzyme-like catalysis and photocatalysis. Its beneficial effects and advantages over the prior art are as follows:
[0034] 1) The technical problem of the inability to prepare manganese single-atom nanocatalysts in related technologies has been solved. The prepared manganese single atoms are economical, efficient, safe and environmentally friendly. The preparation process is simple, the raw materials are cheap and easy to obtain, and the prepared manganese single-atom catalyst has strong adsorption capacity, high enzyme-like catalytic activity and good photocatalytic ability;
[0035] 2) The preparation method is also applicable to single-atom catalysts of other metals;
[0036] 3) The manganese single atom catalyst prepared in this application has good dispersibility in aqueous solution, and has strong acid and alkali resistance and high temperature resistance, which ensures its high efficiency in pollutant degradation in complex environments, especially for antibiotic pollutants, with short reaction time and high reaction efficiency;
[0037] 4) The present application firstly uses acid etching to form a hollow structure of nanocubes, resulting in a larger specific surface area; secondly, manganese ions are adsorbed into the framework through ion exchange; and then, by high-temperature calcination, oxygen elements in the material are removed during the calcination process in a tubular furnace to form a manganese single atom coordination environment of Mn-N3, exposing a large number of active sites, thereby ensuring the catalytic activity and photocatalytic activity of the metal catalyst;
[0038] 5) The raw materials used in this application are widely available and inexpensive, the technical method is simple and practical, the reaction process is mild, there are no high requirements for reaction equipment, it can be promoted on a large scale, and it has significant economic, environmental and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0040] Figure 1 is a flow chart of a method for preparing a manganese single-atom nanocatalyst according to an embodiment of the present application;
[0041] Figure 2 is a schematic diagram of an XRD pattern of a material according to an embodiment of the present application;
[0042] Figure 3 is a schematic diagram of a Fourier infrared spectrum of a material according to an embodiment of the present application;
[0043] Figure 4 It is a schematic diagram of SEM, TEM and spherical aberration electron microscope images of materials according to the embodiments of the present application;
[0044] Figure 5 is a schematic diagram of elemental images of materials before and after carbonization according to an embodiment of the present application;
[0045] Figure 6 is a schematic diagram of a synchrotron radiation E-space spectrum of a material according to an embodiment of the present application;
[0046] Figure 7 is a schematic diagram of a synchrotron radiation R-space spectrum of a material according to an embodiment of the present application;
[0047] Figure 8 is a schematic diagram of a nitrogen adsorption-desorption isotherm according to an embodiment of the present application;
[0048] Fig. 9 is a schematic diagram of the comparison results of adsorption capacity and Zeta potential at different pH values according to the embodiments of the present application;
[0049] Fig.10 is a schematic diagram of a degradation rate spectrum of TC under the adsorption conditions according to an embodiment of the present application;
[0050] Fig.11 is a schematic diagram of a degradation rate spectrum of TC under adsorption and enzyme-like catalysis conditions according to an embodiment of the present application;
[0051] Fig.12 is a schematic diagram of the degradation rate spectrum of TC under the conditions of adsorption, enzyme-like catalysis and photocatalysis according to the embodiment of the present application;
[0052] Fig.13 It is a schematic diagram of the stability of the cyclic reaction according to an embodiment of the present application. DETAILED DESCRIPTION
[0053] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present application.
[0054] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0055] Example 1
[0056] Figure 1 It is a flow chart of a method for preparing a manganese single atom nanocatalyst according to an embodiment of the present application, which can solve the technical problem that the manganese single atom nanocatalyst cannot be prepared in the related art, such as Figure 1 As shown, the method may include the following steps:
[0057] Step S1, synthesizing solid nanocubes: dissolving an organic ligand in deionized water and performing magnetic stirring to obtain solution A, dissolving a metal ion source and an activator in deionized water, and dispersing them by ultrasonic means to obtain solution B; pouring solution B into solution A during magnetic stirring to mix and stir to obtain a mixed solution; vacuum drying the solid obtained after centrifuging the mixed solution, and grinding it into powder to obtain the solid nanocubes.
[0058] For example, firstly, 2-methylimidazole is accurately weighed and dissolved in deionized water, the ratio of 2-methylimidazole to deionized water is 13.65g:210ml, magnetic stirring is performed for 5 minutes, and it is marked as solution A; secondly, zinc nitrate hexahydrate and hexadecyltrimethylammonium bromide (CTAB) are accurately weighed and dissolved in deionized water, the ratio of zinc nitrate hexahydrate, hexadecyltrimethylammonium bromide (CTAB) and deionized water is 0.9g:0.03g:30ml, ultrasonication is performed for 10 minutes to achieve uniform dispersion, and it is marked as solution B. Solution B is slowly poured into solution A during high-speed magnetic stirring, and finally the two are vigorously stirred for 120 minutes to obtain a uniform white solution, and the obtained solid is dried overnight at 40 degrees vacuum after centrifugation at 12000rpm, and the white powder obtained after grinding is solid nanocubes.
[0059] Step S2, synthesizing hollow nanocubes: dissolving the solid nanocubes in deionized water to obtain solution C, dissolving etching acid in deionized water to obtain solution D; pouring solution D into the solid nanocubes during magnetic stirring of solution C to perform etching reaction to obtain a mixed solution; centrifuging and washing the obtained mixed solution to obtain a solid; dissolving the obtained solid in deionized water to obtain solution E.
[0060] For example, first, 1 g of the solid nanocube obtained in step S1 is weighed and dissolved in 300 mL of deionized water, which is marked as solution C; secondly, tannic acid is weighed and dissolved in deionized water, and the ratio of tannic acid to deionized water is 250 mg: 200 ml, which is marked as solution D; finally, solution D is slowly poured into solution C during magnetic stirring to perform etching reaction, and a uniform light yellow solution is obtained after vigorous stirring for 150 minutes. After centrifugation at 10,000 rpm and washing three times, a solid is obtained, which is dissolved in 1.5 L of deionized water and marked as solution E.
[0061] Step S3, adding metal salt: dissolving the metal salt in deionized water to obtain solution F; pouring solution F into solution E during magnetic stirring to obtain a mixed solution; centrifuging and washing the obtained mixed solution to obtain a solid, and freeze-drying the solid in a freeze dryer to obtain a powder.
[0062] For example, firstly, accurately weigh manganese chloride tetrahydrate and dissolve it in deionized water, the dosage ratio of manganese chloride tetrahydrate to deionized water is 30mg:60ml, marked as solution F. Secondly, pour solution F into solution E during high-speed magnetic stirring, stir for 3 hours, the solution will gradually change from light yellow to dark green. Finally, a dark green uniform solution is obtained, and solid is obtained after centrifugal washing at 10000rpm, and freeze-dried in a freeze dryer for 48 hours to obtain powder.
[0063] Step S4, high-temperature carbonization in a tubular furnace: the obtained powder is placed in a tubular furnace for high-temperature carbonization under the condition of passing an inert gas to prevent oxidation, thereby obtaining a manganese single-atom nanocatalyst.
[0064] For example, the powder obtained by freeze drying in step S3 is placed in a tube furnace under nitrogen to prevent oxidation and maintained at 900° C. for 4 hours for high-temperature carbonization with a heating rate of 5° C. / min. The obtained product is 900-Mn SACs manganese single-atom hollow nanocubes.
[0065] Example 2
[0066] Step 1: First, accurately weigh 2-methylimidazole and dissolve it in deionized water. The ratio of 2-methylimidazole to deionized water is 13.65g:210ml. Stir magnetically for 5 minutes and mark it as solution A. Secondly, accurately weigh zinc nitrate hexahydrate and cetyltrimethylammonium bromide (CTAB), dissolve them in deionized water. The ratio of zinc nitrate hexahydrate, cetyltrimethylammonium bromide (CTAB) and deionized water is 0.9g:0.03g:30ml. Ultrasonicate for 10 minutes to achieve uniform dispersion and mark it as solution B. While solution A is being magnetically stirred at high speed, slowly pour solution B into it. Finally, stir the two vigorously for 120 minutes to obtain a uniform white solution. After centrifugation at 12000rpm, dry the obtained solid at 40 degrees vacuum overnight. After grinding, the white powder obtained is solid nanocubes.
[0067] Step 2: First, weigh 1 g of the solid nanocubes obtained in step 1 and dissolve it in 300 mL of deionized water, which is marked as solution C; secondly, weigh tannic acid and dissolve it in deionized water, the ratio of tannic acid to deionized water is 250 mg: 200 ml, which is marked as solution D; finally, slowly pour solution D into solution C during magnetic stirring for etching reaction, and vigorously stir for 150 minutes to obtain a uniform light yellow solution. After centrifugation at 10,000 rpm and washing three times, a solid is obtained, which is dissolved in 1.5 L of deionized water and marked as solution E.
[0068] Step 3: First, accurately weigh manganese chloride tetrahydrate and dissolve it in deionized water. The ratio of manganese chloride tetrahydrate to deionized water is 30 mg: 60 ml, which is marked as solution F. Then, pour solution F into solution E during high-speed magnetic stirring and stir for 3 hours. The solution will gradually change from light yellow to dark green. Finally, a dark green uniform solution is obtained. After centrifugal washing at 10,000 rpm, a solid is obtained, which is freeze-dried in a freeze dryer for 48 hours to obtain a powder.
[0069] Step 4: The powder obtained by freeze drying in step 3 is placed in a tube furnace at 1000°C for 4 hours for high-temperature carbonization under the condition of nitrogen to prevent oxidation, and the heating rate is 5°C / min. The obtained product is 1000-Mn SACs manganese single atom hollow nanocubes.
[0070] Example 3
[0071] Step 1: First, accurately weigh 2-methylimidazole and dissolve it in deionized water. The ratio of 2-methylimidazole to deionized water is 13.65g:210ml. Stir magnetically for 5 minutes and mark it as solution A. Secondly, accurately weigh zinc nitrate hexahydrate and cetyltrimethylammonium bromide (CTAB), dissolve them in deionized water. The ratio of zinc nitrate hexahydrate, cetyltrimethylammonium bromide (CTAB) and deionized water is 0.9g:0.03g:30ml. Ultrasonicate for 10 minutes to achieve uniform dispersion and mark it as solution B. While solution A is being magnetically stirred at high speed, slowly pour solution B into it. Finally, stir the two vigorously for 120 minutes to obtain a uniform white solution. After centrifugation at 12000rpm, dry the obtained solid at 40 degrees vacuum overnight. After grinding, the white powder obtained is solid nanocubes.
[0072] Step 2: First, weigh 1 g of the solid nanocubes obtained in step 1, dissolve it in 300 mL of deionized water, and mark it as solution C; secondly, weigh tannic acid and dissolve it in deionized water, the ratio of tannic acid to deionized water is 250 mg: 200 ml, and mark it as solution D; finally, slowly pour solution D into solution C during magnetic stirring for etching reaction, and vigorously stir for 150 minutes to obtain a uniform light yellow solution. After centrifugation at 10,000 rpm and washing three times, a solid is obtained, and dried in a vacuum dryer overnight for 48 hours to obtain a light yellow powder.
[0073] Step 3: First, weigh 1 g of the light yellow powder in step 2, dissolve it in 500 mL of deionized water by ultrasonic, and mark it as solution E; secondly, weigh manganese chloride tetrahydrate and dissolve it in deionized water, the ratio of manganese chloride tetrahydrate to deionized water is 10 mg: 20 ml, and mark it as solution F. Then, pour solution F into solution E during high-speed magnetic stirring, stir for 3 hours, centrifuge and wash at 10,000 rpm to obtain a solid, and dry it in a vacuum dryer overnight for 48 hours to obtain a powder.
[0074] Step 4: The powder obtained by freeze drying in step 3 is placed in a tube furnace at 900°C for 4 hours for high-temperature carbonization under the condition of nitrogen to prevent oxidation, and the heating rate is 5°C / min. The obtained product is 900 dry-Mn SACs manganese single atom hollow nanocubes.
[0075] Example 4
[0076] In this example, the 900-Mn SACs manganese single atom hollow nanocubes in Example 1 are used to provide a method for removing tetracycline hydrochloride in an aqueous environment.
[0077] Take 100 mL of 50 mg / L tetracycline hydrochloride solution, add 500 μL of 10 mM ascorbic acid, and continue to add 30 mg / mL of ultrasonic 900-Mn-N3. At room temperature and a rotation speed of 200 rpm, take samples at a certain time interval, filter and add 4 mL of the solution sample into a cuvette, use a UV spectrophotometer to measure the concentration of tetracycline hydrochloride in the sample, and the removal rate is shown in Figure 2. Fig.10 , the catalyst showed good adsorption performance.
[0078] Example 5
[0079] In this example, the 900-Mn SACs manganese single atom hollow nanocubes in Example 1 are used to provide a method for removing tetracycline hydrochloride in an aqueous environment.
[0080] Take 100 mL of 50 mg / L tetracycline hydrochloride solution, add 30 mg / mL of ultrasonic 900-Mn SACs, take samples at a certain time interval at room temperature and a rotation speed of 200 rpm, add 4 mL of the solution sample into a cuvette after filtration, and use a UV spectrophotometer to measure the concentration of tetracycline hydrochloride in the sample. The removal rate is shown in Fig.11 The catalyst exhibited excellent enzyme-like catalytic ability. 30 mgMn SACs could achieve 85% degradation level for 50 mg / mL TC solution within 10 minutes, and could achieve 62% degradation level for 100 mg / mL TC solution within 10 minutes.
[0081] Example 6
[0082] In this example, the 900-Mn SACs manganese single atom hollow nanocubes in Example 1 are used to provide a method for removing tetracycline hydrochloride in an aqueous environment.
[0083] Take 100 mL of 50 mg / L tetracycline hydrochloride solution, add 30 mg / mL of ultrasonic 900-Mn SACs, react at room temperature with a rotation speed of 200 rpm for 1 hour, turn on the xenon lamp, take samples at a certain time interval, filter and add 4 mL of the solution sample into a cuvette, use a UV spectrophotometer to measure the concentration of tetracycline hydrochloride in the sample, and the removal rate is shown in Fig.12 The catalysts exhibited excellent photocatalytic performance. 30 mgMn SACs could achieve a degradation level of 95% for 50 mg / mL TC solution within 10 min, and a degradation level of 76% for 100 mg / mL TC solution within 10 min.
[0084] like Figure 2The figure shows the XRD patterns of the three materials ZIF8 HNCs, MnCl2-ZIF8 HNCs and Mn SACs in the examples. The MnCl2-ZIF8 HNCs formed by the etched CN framework through ion exchange and adsorption of manganese ions have a prominent manganese peak compared to the ZIF8 HNCs, indicating that the material has a corresponding manganese crystal structure and crystal plane; and after high-temperature carbonization to form Mn SACs, the corresponding manganese peak decreases. This is because if manganese exists in the material in the form of a single atom, its crystal structure is amorphous or disordered structure, and an obvious manganese peak usually does not appear in the X-ray diffraction (XRD) spectrum. Because in amorphous or disordered structures, the arrangement of atoms has no long-range order and no diffraction peaks are generated, proving the successful synthesis of manganese-based single-atom materials.
[0085] like Figure 3 As shown, it is the Fourier infrared spectra of three materials ZIF8 HNCs, MnCl2-ZIF8 HNCs and Mn SACs in the embodiment. The infrared spectrum characteristics of the ZIF8 HNCs metal organic framework are shown above. The absorption peaks at 3232 cm-1 and 1658 cm-1 are the hydroxyl stretching and bending vibration modes, respectively, which mainly come from the adsorption of water on the sample surface. The absorption peak in the 3000 cm-1~3100 cm-1 band is mainly related to the unsaturated CH stretching vibration mode on the imidazole ring, and the 2800 cm-1~3000 cm-1 band is the saturated CH stretching vibration mode absorption peak. The absorption peak of the sample in the 600 cm-~1600 cm-band is mainly derived from the imidazole ring structure, of which the absorption peak at 1568 cm-1 comes from the imidazole ring C=N structure, and the absorption peaks at 995 cm-1 and 1145 cm-1 are related to the imidazole ring CN structure. The sample has a sharp peak at 422 cm-1, which is mainly derived from the Zn-N stretching vibration mode. The appearance of the above characteristic peaks indicates that the Zn2+ on the zinc salt is coordinated and bonded with the N atom on the imidazole ring, and the metal organic framework is successfully synthesized. Its spectrum characteristics are also consistent with the characteristics of ZIF-8 materials as a whole.
[0086] After the sample was etched with tannic acid, its spectral characteristics changed significantly. First, the relative intensity of the absorption peak at 3232 cm-1 increased significantly, which was caused by the introduction of a large number of hydroxyl structures on tannic acid. The absorption peak of the sample at 2927 cm-1 almost disappeared, indicating that the organic structure in ZIF-8 was significantly oxidized, and the change in the characteristics of the 800 cm-1~1400 cm-1 band was also caused by the introduction of a large number of oxygen-containing groups. It is worth noting that the absorption peaks of the sample at 1458 cm-1, 1423 cm-1 and 422 cm-1 were significantly weakened or even disappeared, indicating that the Zn-N and imidazole ring skeletons were broken, and more Zn2+ sites were exposed on the surface of the MOF material, and the dispersion increased.
[0087] The infrared spectrum of the carbonized single-atom material is relatively simple, showing only a broad peak near 1200 cm-1, which is the infrared absorption caused by the atomic phase change caused by the single-atom lattice vibration. The appearance of this peak indicates that the single-atom sample was successfully prepared.
[0088] like Figure 4 As shown in the embodiment Figure 4 A. Figure 4 B. Figure 4 C are the SEM images of ZIF8 HNCs, MnCl2-ZIF8 HNCs and MnSACs. Figure 4 D. Figure 4 E. Figure 4 F are the TEM images of ZIF8 HNCs, MnCl2-ZIF8 HNCs and Mn SACs, respectively. Figure 4 G is the spherical aberration electron microscope image of Mn SACs. The initial CN framework of the manganese single-atom enzyme is a standard hexahedral structure with a particle size of 80-200nm. Figure 4 D is the transmission image of the CN framework, proving the initial solid structure of the nanocube; Figure 4 B shows that the volume of the nanocube framework increases slightly after tannic acid etching, but it still has a regular hexahedron shape. Figure 4 E Transmission scan of the etched CN framework, proving that the hollow structure of the framework was successfully synthesized after tannic acid etching; Figure 4 C is a manganese-based single-atom enzyme after adding manganese through ion exchange and carbonization. Its surface morphology does not change significantly after tannic acid etching, but its transmission Figure 4 F shows that its framework portion is darker in color, demonstrating successful loading of manganese. Figure 4 G's spherical aberration electron microscopy proved that the manganese element in the material was dispersed in the material in the form of single atoms, proving the successful synthesis of manganese-based single-atom enzymes.
[0089] like Figure 5 The following are the mapping images of MnCl2-ZIF8 HNCs and Mn SACs. According to EDS element analysis, Figure 5 A is the uncarbonized MnCl2-ZIF8 HNCs containing oxygen. Figure 5 B shows that after carbonization at 900℃ for 4 hours, the oxygen in the manganese-based atomic enzyme flows out together with the combustion protection nitrogen during the carbonization process, and finally forms a single atomic structure of Mn-N3.
[0090] like Figure 6 to Figure 7The figure shows the synchrotron radiation spectrum of Mn-N3 (including Mn foil, Mn SACs, MnO, MnPc, MnO2, and MnO3). The coordination environment of manganese atoms was further characterized by X-ray absorption fine structure spectroscopy (XAFS). Figure 6 X-ray absorption near-edge structure (XANES) spectra of Mn SACs show that the absorption edge of Mn SACs is located between Mn foil and MnO2, indicating that the oxidation state of Mn in this Mn-based single-atom enzyme (Mn δ+ , 0﹤δ﹤4). Figure 7 Comparative analysis of the R-space spectrum of the extended X-ray absorption fine structure (EXAFS) of the manganese-based single-atom enzyme shows that it contains multiple shells, among which there is a main peak between 1-2 Å (unit: "angstrom"), which belongs to the Mn-N / C bond according to the comparison with MnPc and MnO2. The structure of this material contains Mn-N in the single-atom structure, with an average coordination number of 3 and a bond length of 2.00 Å, but no obvious Mn-Mn peak (2.3 Å) is found. The fitting data of the R-space spectrum proves the assumed coordination structure of Mn-N3.
[0091] like Figure 8 The figure shows the nitrogen adsorption-desorption isotherms of Mn SACs. Brunauer-Emmett-Teller (BET) measurements show that Mn SACs have a large surface area (708.012 m 2 / g), the total adsorption pore volume is 0.56586 (cm 3 / g), the average adsorption pore size is 3.2 (nm).
[0092] like Fig. 9 The figure below is a comparison of the adsorption capacity and Zeta potential of Mn SACs at different pH values. Generally, the higher the Zeta potential, the more obvious the repulsion between particles and the more stable the dispersion system. By measuring the Zeta potential of the material at different pH values, we can further obtain the zero point charge (pH ZPC ), that is, the pH of the solution when the particle Zeta potential is zero. Above this pH, the particle is positively charged in the solution, and vice versa. It can be seen that the zero charge point pH of Mn SACs ZPC The maximum adsorption capacity is between pH 8 and pH 9, and the maximum adsorption capacity is at pH 4, which means that the Mn SACs particles in the solution are negatively charged; under acidic conditions, tetracycline is usually in a positively charged form. Tetracycline molecules contain multiple electrophilic groups that can accept protons (h +), so that the whole molecule has a positive charge. The two bright rings and other functional groups in the tetracycline molecule can be protonated, resulting in an overall positive charge, which has a stronger electrostatic adsorption effect with the negatively charged Mn SACs particles, improving its adsorption capacity.
[0093] like Figures 10 to 12 Shown is the degradation rate spectrum of TC in Mn SACs under different conditions. Fig.10 The TC adsorption degradation experiment was conducted in a dark environment with the addition of ascorbic acid as an inhibitor, which demonstrated the in-situ adsorption capacity of the Mn SACs material. From the data, we can see that the use of 30 mg Mn SACs can achieve 50% adsorption degradation for 50 mg / mL TC solution within 10 minutes, and 28% adsorption degradation for 100 mg / mL TC solution within 10 minutes; Fig.11 The adsorption and enzyme-like degradation of TC by Mn SACs materials without adding inhibitors in a dark environment were studied. Using 30 mg of Mn SACs, a degradation level of 85% can be achieved for a 50 mg / mL TC solution within 10 minutes, and a degradation level of 50% can be achieved for a 100 mg / mL TC solution within 10 minutes. Fig.12 In order to investigate the adsorption, enzyme-like and photocatalytic degradation of TC by MnSACs materials without adding inhibitors under light environment, 30 mg Mn SACs can achieve a degradation level of 95% for a 50 mg / mL TC solution within 10 minutes, and a degradation level of 76% for a 100 mg / mL TC solution within 10 minutes.
[0094] like Fig.13 As shown, it is a stability experiment of the cyclic reaction in the application example of Mn SACs. After fully ultrasonically washing the materials for each experiment, they were re-frozen into powder by freeze-drying, collected and used again in the experiment; it was found that its photocatalytic ability did not decrease significantly during the four repeated experiments, and its enzyme-like catalytic ability fluctuated, which may be because some residual small molecule products were wrapped on the surface of the material and not completely washed, and its adsorption capacity showed a slight downward trend, which may be because of the hollow cubic structure, and small molecules could not be degraded and discharged. Overall, the degradation ability of the material itself did not change much in the four repeated experiments, proving the stability of the manganese single atom catalyst of this application.
[0095] It should be noted that, for the aforementioned method embodiments, for the sake of simplicity, they are all expressed as a series of action combinations, but those skilled in the art should be aware that the present application is not limited by the described order of actions, because according to the present application, certain steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also be aware that the embodiments described in the specification are all preferred embodiments, and the actions and modules involved are not necessarily required by the present application.
[0096] Through the description of the above implementation methods, those skilled in the art can clearly understand that the method according to the above embodiment can be implemented by means of software plus a necessary general hardware platform, and of course by hardware, but in many cases the former is a better implementation method. Based on this understanding, the technical solution of the present application, or the part that contributes to the prior art, can be embodied in the form of a software product, which is stored in a storage medium (such as ROM / RAM, magnetic disk, optical disk), and includes a number of instructions for a terminal device (which can be a mobile phone, computer, server, or network device, etc.) to execute the methods described in each embodiment of the present application.
[0097] A person of ordinary skill in the art can understand that all or part of the steps in the various methods of the above embodiments can be completed by instructing the hardware related to the terminal device through a program, and the program can be stored in a computer-readable storage medium, and the storage medium may include: a flash drive, a read-only memory (ROM), a random access memory (RAM), a magnetic disk or an optical disk, etc.
[0098] The embodiment of the present application further provides a storage medium. Optionally, in this embodiment, the storage medium can be used to execute the program code of the above method.
[0099] Optionally, in this embodiment, the storage medium may be located on at least one network device among a plurality of network devices in the network shown in the above embodiment.
[0100] Optionally, the specific examples in this embodiment may refer to the examples described in the above embodiments, and this embodiment will not be described in detail here.
[0101] Optionally, in this embodiment, the above-mentioned storage medium may include but is not limited to: a USB flash drive, a read-only memory (ROM), a random access memory (RAM), a mobile hard disk, a magnetic disk or an optical disk, and other media that can store program codes.
[0102] The serial numbers of the above-mentioned embodiments of the present application are for description only and do not represent the advantages or disadvantages of the embodiments.
[0103] If the integrated units in the above embodiments are implemented in the form of software functional units and sold or used as independent products, they can be stored in the above computer-readable storage medium. Based on this understanding, the technical solution of the present application, or the part that contributes to the prior art, or all or part of the technical solution can be embodied in the form of a software product, which is stored in a storage medium and includes several instructions for enabling one or more computer devices (which may be personal computers, servers or network devices, etc.) to execute all or part of the steps of the methods described in the various embodiments of the present application.
[0104] In the above embodiments of the present application, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, please refer to the relevant description of other embodiments.
[0105] In the several embodiments provided in the present application, it should be understood that the disclosed client can be implemented in other ways. Among them, the device embodiments described above are only schematic. For example, the division of the units is only a logical function division. There may be other division methods in actual implementation. For example, multiple units or components can be combined or integrated into another system, or some features can be ignored or not executed. Another point is that the mutual coupling or direct coupling or communication connection shown or discussed can be through some interfaces, indirect coupling or communication connection of units or modules, which can be electrical or other forms.
[0106] The units described as separate components may or may not be physically separated, and the components shown as units may or may not be physical units, that is, they may be located in one place or distributed on multiple network units. Some or all of the units may be selected according to actual needs to achieve the purpose of the solution of this embodiment.
[0107] In addition, each functional unit in each embodiment of the present application may be integrated into one processing unit, or each unit may exist physically separately, or two or more units may be integrated into one unit. The above-mentioned integrated unit may be implemented in the form of hardware or in the form of software functional units.
[0108] The above is only a preferred implementation of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application. These improvements and modifications should also be regarded as the scope of protection of the present application.
Claims
1. A method for preparing a manganese single-atom nanocatalyst, characterized in that: include: Synthesis of solid nanocubes: dissolving an organic ligand in deionized water and subjecting it to magnetic stirring to obtain solution A, dissolving a metal ion source and an activator in deionized water and dispersing them by ultrasonication to obtain solution B; While solution A is being magnetically stirred, solution B is poured into the solution for mixing and stirring to obtain a mixed solution; The solid obtained by centrifuging the mixed solution is vacuum dried, and then ground into powder to obtain the solid nanocube; Synthesizing hollow nanocubes: dissolving the solid nanocubes in deionized water to obtain solution C, and dissolving etching acid in deionized water to obtain solution D; While solution C is being magnetically stirred, solution D is poured into the solution to perform an etching reaction on the solid nanocubes, thereby obtaining a mixed solution; The obtained mixed solution is centrifuged and washed to obtain a solid; The obtained solid was dissolved in deionized water to obtain solution E; Adding metal salt: dissolving the metal salt in deionized water to obtain solution F; While solution E is being magnetically stirred, solution F is poured into the solution to obtain a mixed solution; The obtained mixed solution is centrifuged and washed to obtain a solid, and the solid is freeze-dried by a freeze dryer to obtain a powder; Tube furnace high temperature carbonization: The obtained powder is placed in a tube furnace for high temperature carbonization under the condition of passing inert gas to prevent oxidation, thereby obtaining a manganese single atom nanocatalyst; The organic ligand is any one of 2-methylimidazole or o-diazine; The metal ion source is any one of zinc sulfate, zinc chloride, zinc nitrite, zinc nitrate or zinc acetate; The activator is any one of hexadecyltrimethylammonium bromide or polyvinylpyrrolidone; The etching acid is any one of acetic acid, hydrofluoric acid or tannic acid; The metal salt is any one of manganese chloride tetrahydrate, manganese sulfate monohydrate, manganese nitrate or manganese nitrite.
2. The preparation method according to claim 1, characterized in that: The concentration of the organic ligand in the solution A is 0.05-0.1 g / mL, the concentration of the metal ion source in the solution B is 0.01-0.1 g / mL, and the concentration of the activator is 0.001-0.01 g / mL; When solution B is poured into solution A for mixing and stirring, the ratio of solution A to solution B is 1:
1.
3. The preparation method according to claim 1, characterized in that: The ratio of the solid nanocube powder to deionized water in the solution C is 1:(100-300); the ratio of the etching acid to deionized water in the solution D is (1-1.5):1; When the solution D is poured into the solution C, the ratio of the solution C to the solution D is 1:
1.
4. The preparation method according to claim 1, characterized in that: Dissolving the obtained solid in deionized water to obtain solution E, comprising: mixing the solid and deionized water in a ratio of (1-3):200, and mixing by ultrasonication to obtain solution E; Dissolving the metal salt in deionized water to obtain a solution F comprises: mixing the manganese metal salt and deionized water in a ratio of 1:(3-6) to obtain the solution F; Pouring solution F into solution E while magnetically stirring the solution to obtain a mixed solution includes: adding deionized water into solution E for dilution, and then pouring the diluted solution F into solution E while magnetically stirring the solution to obtain a mixed solution.
5. The preparation method according to claim 1, characterized in that: In the process of placing the obtained powder into a tubular furnace for high-temperature carbonization under the condition of passing inert gas to prevent oxidation, the heating rate of the tubular furnace is (1-10)°C / s, the reaction temperature is 800-1200°C, and the maintenance time is 120-360 minutes.
6. The preparation method according to claim 1, characterized in that: The zinc nitrate is zinc nitrate hexahydrate.