Fluorescent acrylic acid hydrogel antifouling paint as well as preparation method and application thereof
The fluorescent acrylic hydrogel antifouling coating prepared through polymerization reaction uses the aggregation effect between polymer molecules to achieve cluster fluorescence, solving the problem of poor antifouling performance after the introduction of fluorescent agents, simplifying the process and improving the antifouling effect , suitable for industrial applications.
Patent Information
- Application Number
- CN202411244619.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-06
AI Technical Summary
The introduction of existing fluorescent agents into marine antifouling coatings leads to an increase in the surface roughness of the coating, poor antifouling performance, and may have an impact on the ecological environment. At the same time, the preparation process is cumbersome, which is not conducive to industrial application.
Through polymerization reaction, fluorescent acrylic hydrogel antifouling coating is prepared by using the aggregation effect between polymer molecules without using fluorescent agents, so as to achieve the cluster fluorescence and antifouling effect of the coating, combined with the water absorption characteristics of the hydrogel. Form a multiple anti-fouling mechanism.
A hydrogel antifouling coating that emits fluorescence at multiple excitation wavelengths is realized, which synergizes in the fluorescence and hydrogel characteristics, improves antifouling performance, simplifies the process flow, avoids the impact of fluorescent agents on the environment, and is suitable for scale. Chemical production.
Smart Images

Figure BDA0005030293110000041 
Figure BDA0005030293110000111 
Figure FDA0005030293100000031
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of marine fouling biological control. More specifically, the present invention relates to a fluorescent acrylic hydrogel antifouling coating, a preparation method of the hydrogel fluorescent acrylic hydrogel antifouling coating, and a use of the fluorescent acrylic hydrogel antifouling coating. Background Art
[0002] Fouling such as molecules, algae, and bacteria attached to the surface of equipment and ships in marine operations will cause serious economic losses and environmental damage. Therefore, it is crucial to study marine antifouling materials that can prevent biological fouling. It has been found that hydrogels, as a typical environmentally friendly antifouling material, have great application potential in the field of marine antifouling. However, due to the wide variety of fouling in the ocean, the antifouling strategy of only relying on the original properties of hydrogels is simple and it is difficult to achieve broad-spectrum and long-term antifouling. Therefore, giving hydrogels more antifouling strategies is an effective means to enhance antifouling performance.
[0003] Inspired by the antifouling mechanism of corals, corals emit fluorescence, providing weak light for algae to photosynthesize, which can inhibit the settlement and adhesion of algae. As a result, a large number of fluorescent agents are combined with various coatings to give the coatings fluorescent properties, thereby enhancing the antifouling performance of the coatings. For example, Xiong et al. described in the document "Effect of the properties of long afterglowphosphors on the antifouling performance of silicone fouling-release coating", "Progress in Organic Coatings", Vol. 170, 2022, p. 106965 that a fluorescent agent was added to a polydimethylsiloxane coating to give it fluorescent properties, but the introduction of the fluorescent agent made the surface rougher, which was not conducive to improving the antifouling performance. Mao et al. described in the document “Advanced Marine Antifouling Hydrogels Based on 7-Amino-4-methylcoumarin Fluorescence Driven by Rare-Earth Phosphorescence”, ACS Applied Materials & Interfaces, Vol. 15, 2023, pp. 57582-57592, the preparation of a fluorescent agent that can emit light, and complexing it with polyvinyl alcohol to prepare fluorescent polyvinyl alcohol hydrogel, but compared with the polyvinyl alcohol hydrogel without adding a fluorescent agent, its water content has decreased, which has a certain effect on the antifouling effect of the hydrogel hydration layer. Therefore, the current method of using a fluorescent agent to give the coating fluorescent properties will destroy the original characteristics of the coating, and the coating properties and fluorescent properties cannot achieve a better effect of synergistic antifouling. At the same time, the combination of the above-mentioned fluorescent agent and the coating will cause the fluorescent agent in the coating to be released into the seawater, which has a certain impact on the ecological environment. In addition, in order to give the coating fluorescent properties, the steps of preparing the fluorescent agent first are cumbersome, which is not conducive to the process of industrial application. In summary, imparting fluorescent properties to antifouling coatings without using fluorescent agents is a technical challenge in imparting fluorescent properties to antifouling coatings.
[0004] Based on this, the inventors propose to prepare a fluorescent acrylic hydrogel antifouling coating by a simple polymerization reaction without using a fluorescent agent and utilizing the aggregation effect between polymer molecules. The fluorescent acrylic hydrogel antifouling coating can emit fluorescence at multiple wavelengths, thereby achieving synergistic antifouling properties of fluorescence and acrylic hydrogel antifouling coating. Summary of the invention
[0005] [Technical issues to be solved]
[0006] The invention aims to provide a fluorescent acrylic acid hydrogel antifouling coating.
[0007] Another object of the present invention is to provide a method for preparing the fluorescent acrylic hydrogel antifouling coating.
[0008] Another object of the present invention is to provide the use of the fluorescent acrylic hydrogel antifouling coating obtained by the preparation method.
[0009] [Technical solution]
[0010] The present invention is achieved through the following technical solutions.
[0011] The invention also relates to a method for preparing the fluorescent acrylic acid hydrogel antifouling coating.
[0012] The preparation steps of the preparation method are as follows:
[0013] A. Preparation of Monomer Mixture
[0014] The oily acrylate monomer, acrylic acid monomer, acrylamide monomer, acrylate amino ester monomer and water-based acrylate monomer are mixed uniformly in a molar ratio of 20-85:5-20:0-20:0-50:0-40, and then 0.4-2.0% of an initiator based on the total weight of the monomers is added and mixed uniformly to obtain the monomer mixture;
[0015] B. Synthesis of fluorescent acrylic hydrogel antifouling coating prepolymer
[0016] Under nitrogen protection, 50-200% of the mixed organic solvent and 5-15% of the monomer mixture obtained in step A are added to a four-necked flask equipped with a stirrer, a condenser and a thermometer, and then the reaction system is heated to a temperature of 65-95° C.; at the same time, the temperature is maintained for 10-30 minutes, and then the remaining monomer mixture is evenly divided into 3-10 parts, and one part is added every 10-30 minutes; after the monomer mixture is added, the temperature is kept for 1 hour, and then 0.01-0.1% of the above-mentioned initiator is added based on the total mass of the monomer mixture, and the reaction is continued for 1-3 hours to obtain the fluorescent acrylic hydrogel antifouling coating prepolymer;
[0017] C. Preparation of fluorescent acrylic hydrogel antifouling coating
[0018] According to the crosslinking agent being 5-50% of the molar amount of the acrylic monomer, the fluorescent acrylic hydrogel antifouling coating prepolymer obtained in step B is mixed with the crosslinking agent at a temperature of 10-40° C., then coated on a substrate for full crosslinking, and dried to obtain the fluorescent acrylic hydrogel antifouling coating.
[0019] According to a preferred embodiment of the present invention, in step A, the oily acrylic acid ester monomer is one or more oily acrylic acid ester monomers selected from methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, butyl acrylate, butyl methacrylate, isobutyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, dodecyl acrylate, dodecyl methacrylate, myristyl acrylate, myristyl methacrylate, hexadecyl acrylate, octadecyl acrylate or octadecyl methacrylate.
[0020] According to another preferred embodiment of the present invention, in step A and step C, the acrylic acid monomer is one or more acrylic acid monomers selected from acrylic acid, methacrylic acid or itaconic acid.
[0021] According to another preferred embodiment of the present invention, in step A, the acrylamide monomer is one or more acrylamide monomers selected from acrylamide, N-hydroxymethyl acrylamide, N-hydroxyethyl acrylamide, N,N-methylenebisacrylamide, N,N-dimethyl acrylamide, N,N-diethyl acrylamide, N-isopropyl acrylamide or N-tert-butyl acrylamide; the amino acrylate monomer is one or more amino acrylate monomers selected from dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate or 3-(dimethylamino)propyl acrylate; the water-based acrylate monomer is one or more water-based acrylate monomers selected from hydroxymethyl acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 2-(hydroxymethyl)methyl acrylate or 2-(hydroxymethyl)ethyl acrylate.
[0022] According to another preferred embodiment of the present invention, in step A, the initiator is one or more initiators selected from azobisisobutyronitrile, azobisisoheptylnitrile, dibenzoyl peroxide, di(2-ethylhexyl) peroxydicarbonate, di-tert-butyl peroxide, dodecyl peroxide, tert-butyl perbenzoate, potassium persulfate or ammonium persulfate.
[0023] According to another preferred embodiment of the present invention, in step B, the organic solvent is one or more organic solvents selected from xylene, methyl isobutyl ketone, butyl acetate, n-butanol, ethanol or cyclohexanone.
[0024] According to another preferred embodiment of the present invention, in step B, the fluorescent acrylic hydrogel antifouling coating prepolymer has the following chemical structural formula (I):
[0025]
[0026] Where:
[0027] R1, R5 and R8 represent H or CH3;
[0028] R2 represents CH3, CH2CH3, CH2CH2CH3, CH2CH2CH2CH3, CH2CH(CH3)2, C(CH3)3, CH2CH(CH2CH3)(CH2)3CH3, (CH2)7CH3, (CH2) 11 CH3, (CH2) 13 CH3, (CH2) 15 CH3 or (CH2) 17 CH3;
[0029] R3 represents H, CH3 or CH2COOH;
[0030] R4 represents H, CH2OH, (CH2)2OH, CH2NHCOCHCH2, (CH3)2, (CH2CH3)2, CH(CH3)2 or C(CH3)3;
[0031] R6 represents CH2CH2 or CH2CH2CH2;
[0032] R7 and R 10 represents CH3 or CH2CH3;
[0033] R9 represents CH2, CH2CH2, CH2CH2CH2, CH2CHCH3 or CH2CH2CH2CH2;
[0034] a, b are positive integers, i, o, u, n are 0 or positive integers, i and o cannot be 0 at the same time;
[0035] Its number average molecular weight is 10,000 to 1,000,000, and its molecular weight distribution is 1.0 to 3.5.
[0036] According to another preferred embodiment of the present invention, in step C, the crosslinking agent is one or more crosslinking agents selected from aziridine crosslinker XR-100, aziridine crosslinker CX-100, aziridine crosslinker CX-300, aziridine crosslinker XC-103, acrylic crosslinker CX-A10 or silicone crosslinker Silicone-9301.
[0037] The invention also relates to a fluorescent acrylic acid hydrogel antifouling coating prepared by the preparation method.
[0038] The invention also relates to the use of the fluorescent acrylic hydrogel antifouling paint in preventing the formation of marine biofouling.
[0039] The present invention will be described in more detail below.
[0040] Acrylic hydrogel is a typical environmentally friendly antifouling material. It can be modified to introduce other antifouling structures to give it more antifouling properties. It has great application potential in preventing the formation of marine biofouling. Therefore, the present invention introduces hydrophilic groups to construct a water-absorbing acrylic hydrogel antifouling coating, and constructs different monomer compositions. Cluster fluorescence is achieved without introducing a fluorescent agent through the intermolecular interaction inside the polymer, thereby realizing the multiple antifouling mechanisms of the acrylic hydrogel antifouling coating's hydrophilic properties and fluorescence.
[0041] The invention relates to a method for preparing a fluorescent acrylic acid hydrogel antifouling coating.
[0042] A. Preparation of Monomer Mixture
[0043] The oily acrylate monomer, acrylic acid monomer, acrylamide monomer, acrylate amino ester monomer and water-based acrylate monomer are mixed uniformly in a molar ratio of 20-85:5-20:0-20:0-50:0-40, and then 0.4-2.0% of an initiator based on the total weight of the monomers is added and mixed uniformly to obtain the monomer mixture;
[0044] In the present invention, the oily acrylate monomer should be understood as an acrylate monomer that does not contain a hydrophilic group. Its main function in preparing the fluorescent acrylic hydrogel antifouling coating is to improve the solubility of the prepolymer in the organic solvent system to obtain a uniform fluorescent acrylic antifouling coating prepolymer.
[0045] The oily acrylic acid ester monomer used in the present invention is one or more oily acrylic acid ester monomers selected from methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, butyl acrylate, butyl methacrylate, isobutyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, dodecyl acrylate, dodecyl methacrylate, tetradecyl acrylate, tetradecyl methacrylate, hexadecyl acrylate, octadecyl acrylate or octadecyl methacrylate, all of which are products currently sold on the market, such as butyl acrylate sold by Tianjin Tianjiao Chemical Co., Ltd. under the trade name of butyl acrylate.
[0046] The main function of acrylic acid monomer in the preparation of fluorescent acrylic acid hydrogel antifouling coating is to provide cross-linking groups that can react with cross-linking agents, construct cross-linking networks, and promote the formation of fluorescent acrylic acid hydrogel antifouling coating from fluorescent acrylic acid hydrogel antifouling coating prepolymers.
[0047] The acrylic acid monomer used in the present invention is one or more acrylic acid monomers selected from acrylic acid, methacrylic acid or itaconic acid, which are all products currently sold on the market, such as acrylic acid sold by Tianjin Damao Chemical Reagent Company under the trade name of acrylic acid.
[0048] The main function of acrylamide monomer in the preparation of fluorescent acrylic hydrogel antifouling coating is to provide fluorescent chromophores and hydrophilic groups, so that the fluorescent hydrogel antifouling coating emits fluorescence and absorbs water to form a hydrogel.
[0049] The acrylamide monomers used in the present invention are one or more acrylamide monomers selected from acrylamide, N-hydroxymethyl acrylamide, N-hydroxyethyl acrylamide, N,N-methylenebisacrylamide, N,N-dimethyl acrylamide, N,N-diethyl acrylamide, N-isopropyl acrylamide or N-tert-butyl acrylamide, all of which are products currently sold on the market, such as acrylamide sold by Jiangxi Jiuchang Agricultural Science and Chemical Co., Ltd. under the trade name of acrylamide.
[0050] The main role of the acrylic amino ester monomer in the preparation of the fluorescent acrylic hydrogel antifouling coating is to provide the fluorescent chromophore and hydrophilic group of the fluorescent acrylic hydrogel antifouling coating, and promote the coating to emit fluorescence and absorb water.
[0051] The amino acrylate used in the present invention is one or more amino acrylate monomers selected from dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate or 3-(dimethylamino)propyl acrylate, all of which are products currently sold on the market, such as dimethylaminoethyl methacrylate sold by Aladdin Reagent Co., Ltd. under the trade name dimethylaminoethyl methacrylate.
[0052] In the present invention, the water-based acrylate monomer should be understood as an acrylate monomer with a hydrophilic group. Its main function in preparing the fluorescent acrylic hydrogel antifouling coating is to provide a hydrophilic group that combines with water molecules and promote the hydrogel to play the antifouling role of the hydration layer.
[0053] The aqueous acrylate monomers used in the present invention are one or more aqueous acrylate monomers selected from hydroxymethyl acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, methyl 2-(hydroxymethyl)acrylate or ethyl 2-(hydroxymethyl)acrylate, all of which are products currently sold on the market, such as the hydroxypropyl acrylate sold by Aladdin Reagent Co., Ltd. under the trade name hydroxypropyl acrylate.
[0054] In this step, when the amount of acrylic acid monomer, acrylamide monomer, amino acrylate monomer and water-based acrylic acid monomer is within the above range, if the amount of oily acrylic acid monomer is less than 20, the prepolymer and the solvent are easily separated, which is not conducive to forming a uniform prepolymer and solvent system; if the amount of oily acrylic acid monomer is higher than 85, it cannot provide enough fluorescent chromophores and hydrophilic groups, which is not conducive to the preparation of fluorescent acrylic acid hydrogel antifouling coatings. Therefore, it is reasonable to use an amount of oily acrylic acid monomer of 20 to 85, preferably 30 to 70, and more preferably 35 to 60.
[0055] When the amount of oily acrylic ester monomer, acrylamide monomer, amino acrylic ester monomer and water-based acrylic ester monomer is within the above range, if the amount of acrylic monomer is less than 5, it is not conducive to their reaction with the cross-linking agent to form a sufficient cross-linking structure, and the hydrogel properties are reduced; if the amount of acrylic monomer is higher than 20, it is easy to cause the prepolymer to form a gel, which is not conducive to the smooth progress of the polymerization reaction, and causes the cross-linking structure to be too tight, resulting in cracking of the coating. Therefore, the amount of acrylic monomer is appropriately 5 to 20, preferably 8 to 18, and more preferably 10 to 15.
[0056] When the amount of oily acrylate monomer, acrylic acid monomer, amino acrylate monomer and water-based acrylate monomer is within the range, when the amount of amino acrylate monomer is not 0, and the fluorescent acrylic hydrogel antifouling coating can emit fluorescence and absorb water, the amount of acrylamide monomer can be 0; if the amount of acrylamide monomer is higher than 20, it will cause gelation during the polymerization reaction, which is not conducive to the smooth progress of the polymerization reaction and is not conducive to obtaining a uniform prepolymer and solvent system. Therefore, the amount of acrylamide monomer is appropriately 0 to 20, preferably 5 to 15, and more preferably 8 to 12.
[0057] When the amount of oily acrylate monomer, acrylic acid monomer, acrylamide monomer and water-based acrylate monomer is within the range, when the amount of acrylamide monomer is not 0, and the fluorescent acrylic hydrogel antifouling coating can emit fluorescence and combine with water molecules, the amount of acrylate amino ester monomer can be zero; if the amount of acrylate amino ester monomer is higher than 50, the viscosity of the prepolymer and the solvent system will be too high, which is not conducive to subsequent processing, and the acrylic hydrogel antifouling coating will easily absorb too much water and be over-swollen and destroyed. Therefore, the amount of acrylate amino ester monomer is suitable to be 0 to 50, preferably 10 to 40, and more preferably 12 to 30.
[0058] When the amount of oily acrylate monomer, acrylic acid monomer, acrylamide monomer and acrylate amino ester monomer is within the above range, when the fluorescent acrylic hydrogel antifouling coating can combine with sufficient water molecules to form a hydration layer to play an antifouling role, the amount of water-based acrylate monomer can be 0; if the amount of water-based acrylate monomer is higher than 40, a large number of hydroxyl groups will form hydrogen bonds between polymers, and gel and phase separation will occur during the polymerization reaction, which is not conducive to the subsequent reaction. Therefore, it is reasonable to use 0 to 40 water-based acrylate monomers, preferably 10 to 30, and more preferably 12 to 25.
[0059] Preferably, the molar ratio of oily acrylate monomer, acrylic acid monomer, acrylamide monomer, amino acrylate monomer and water-based acrylate monomer is 30-70:8-18:5-15:10-40:10-30, more preferably 35-60:10-15:8-12:12-30:12-25.
[0060] According to the present invention, the main function of the initiator in the preparation of the fluorescent acrylic hydrogel antifouling coating is that the initiator will decompose into free radicals, thereby initiating the polymerization reaction of the monomers to generate polymers.
[0061] The initiator used in the present invention is an initiator selected from azobisisobutyronitrile, azobisisoheptanenitrile, dibenzoyl peroxide, di(2-ethylhexyl) peroxydicarbonate, di-tert-butyl peroxide, dodecyl peroxide, tert-butyl perbenzoate, potassium persulfate or ammonium persulfate, all of which are products currently sold on the market, such as the azobisisobutyronitrile sold by Tianjin Damao Chemical Reagent Factory under the trade name azobisisobutyronitrile.
[0062] The same initiator is used in the subsequent steps of preparing the fluorescent acrylic hydrogel antifouling coating of the present invention, so it is not described in detail.
[0063] In this step, if the amount of initiator is higher than 2.0%, the molecular weight of the fluorescent acrylic hydrogel antifouling coating will be too low, which is not conducive to the improvement of its mechanical properties, and the dispersion coefficient of its molecular weight will be too large, which is not conducive to process stability; if the amount of initiator is lower than 0.4%, the polymerization reaction will be unstable or not initiated, and the molecular weight of the prepolymer will be too large, so the polymerization reaction cannot proceed smoothly. Therefore, it is reasonable to use 0.4-2.0% of the initiator, preferably 0.6-1.5%.
[0064] B. Synthesis of fluorescent acrylic hydrogel antifouling coating prepolymer
[0065] Under nitrogen protection, 50-200% of the mixed organic solvent and 5-15% of the monomer mixture are added to a four-necked flask equipped with a stirrer, a condenser and a thermometer, based on the total mass of the monomer mixture obtained in step A, and then the reaction system is heated to a temperature of 65-90° C.; at the same time, the temperature is maintained for 10-30 minutes, and then the remaining monomer mixture is evenly divided into 3-10 parts, and one part is added every 10-30 minutes; after the monomer mixture is added, the temperature is kept for 1 hour, and then 0.01-0.1% of the above-mentioned initiator is added based on the total mass of the monomer mixture, and the reaction is continued for 1-3 hours to obtain the fluorescent acrylic hydrogel antifouling coating prepolymer;
[0066] The organic solvent used in this step is one or more organic solvents selected from xylene, methyl isobutyl ketone, butyl acetate, n-butanol, ethanol or cyclohexanone, all of which are products currently sold on the market, such as the xylene sold by Qingdao Datang Chemical Co., Ltd. under the trade name xylene.
[0067] The mixed organic solvent used in this step should be understood to be a solvent formed by mixing one or more of the above-mentioned organic solvents in any proportion.
[0068] In this step, 50-200% of the mixed organic solvent and 5-15% of the monomer mixture are maintained at a temperature of 65° C. to 95° C. for 10 to 30 minutes.
[0069] When the amount of the monomer mixture is within the range, if the amount of the mixed organic solvent is less than 50%, the viscosity of the prepolymer will be high in the later stage of the reaction, the reaction will be uneven, and it will be not conducive to the later use; if the amount of the mixed organic solvent is higher than 200%, a large amount of volatile organic matter will be volatilized during the later use, polluting the environment and causing waste of resources. Therefore, it is appropriate to use 50-200% of the mixed organic solvent, preferably 80-150%. When the amount of the mixed organic solvent is within the range, if the amount of the monomer mixture is lower than 5%, the early stage reaction will be insufficient, which is not conducive to the stable progress of the later reaction; if the amount of the monomer mixture is higher than 15%, the reaction will be violent in the initial stage, the temperature of the reaction system will be difficult to control, and it will bring safety hazards. Therefore, it is appropriate to use 5-15% of the monomer mixture, preferably 8-12%.
[0070] In this step, when the holding time is within the range, if the temperature is lower than 65°C, it is not conducive to the decomposition of the initiator and the smooth progress of the reaction; if the temperature is higher than 90°C, it will cause the reaction to be too violent, there will be potential safety hazards, and the distribution coefficient of the polymer molecular weight will be too large, and the process will be unstable. Therefore, the temperature is suitable for 65 to 95°C, preferably 70 to 90°C. When the temperature is within the range, if the holding time is shorter than 10 minutes, the initiation reaction is insufficient, which is not conducive to the stable progress of the later reaction; if the holding time is longer than 30 minutes, it is easy to cause dead-end polymerization and is not conducive to the improvement of process efficiency. Therefore, it is suitable to hold the time for 10 to 30 minutes, preferably 15 to 25 minutes.
[0071] In this step, the remaining monomer mixture is divided into 3 to 10 portions, and one portion is added every 30 minutes. The main purpose is to avoid adding too much monomer mixture at a single time, which cannot be dispersed into the reaction system in time. It can also avoid too violent reaction, causing the reaction temperature to be too high, causing safety problems and unstable reaction.
[0072] In this step, the purpose of adding initiator after keeping warm for 1 hour is to make the unreacted monomers in the system participate in the reaction and polymerization. The reaction is continued for 1 to 3 hours after adding initiator, and its basic function is to ensure that the unreacted monomers are fully reacted and polymerized.
[0073] The product obtained in this step is a fluorescent acrylic hydrogel antifouling coating prepolymer, which is determined by conventional analytical methods using a Fourier transform infrared spectrometer manufactured by Bruker, Germany, and has the chemical structure:
[0074]
[0075] Where:
[0076] R1, R3, R5 and R8 represent H or CH3;
[0077] R2 represents CH3, CH2CH3, CH2CH2CH3, CH2CH2CH2CH3, CH2CH(CH3)2, C(CH3)3, CH2CH(CH2CH3)(CH2)3CH3, (CH2)7CH3, (CH2) 11 CH3, (CH2) 13 CH3, (CH2) 15 CH3 or (CH2) 17 CH3;
[0078] R4 represents H, CH2OH, (CH2)2OH, CH2NHCOCHCH2, (CH3)2, (CH2CH3)2, CH(CH3)2 or C(CH3)3;
[0079] R6 represents CH2CH2 or CH2CH2CH2;
[0080] R7 and R 10 represents CH3 or CH2CH3;
[0081] R9 represents CH2, CH2CH2, CH2CH2CH2 or CH2CH2CH2CH2
[0082] a, b are positive integers, i, o, u, n are 0 or positive integers, i and o cannot be 0 at the same time;
[0083] Its number average molecular weight is 10,000 to 1,000,000, and its molecular weight distribution is 1.0 to 3.5.
[0084] C. Preparation of fluorescent acrylic hydrogel antifouling coating
[0085] According to the crosslinking agent being 5-50% of the molar amount of the acrylic monomer, the fluorescent acrylic hydrogel antifouling coating prepolymer obtained in step B is mixed with the crosslinking agent at a temperature of 10-40° C., then coated on a substrate for full crosslinking, and dried to obtain the fluorescent acrylic hydrogel antifouling coating.
[0086] According to the present invention, the main function of the cross-linking agent in the preparation of the fluorescent acrylic hydrogel antifouling coating is to react with the carboxyl group in the fluorescent acrylic hydrogel antifouling coating prepolymer to form a cross-linked network structure of the prepolymer. When the coating contacts water, the hydrophilic groups in the coating combine with water molecules and absorb water molecules, so that the water molecules fill the three-dimensional network to form a hydrogel coating with a three-dimensional structure.
[0087] The crosslinking agent used in the present invention is one or more crosslinking agents selected from aziridine crosslinking agent XR-100, aziridine crosslinking agent CX-100, aziridine crosslinking agent CX-300, aziridine crosslinking agent XC-103, acrylic acid crosslinking agent CX-A10 or silicone crosslinking agent Silicone-9301.
[0088] In this step, the amount of the crosslinking agent is 5-50% of the molar amount of the acrylic acid monomer. If the amount of the crosslinking agent is higher than 50%, the crosslinking agent that does not participate in the crosslinking will appear in the system, resulting in waste; if the amount of the crosslinking agent is lower than 5%, the number of crosslinking structures of the hydrogel coating will be insufficient, and it will be easily destroyed after absorbing water, and the mechanical properties will be too poor. Therefore, it is desirable to use 5-50% of the crosslinking agent, preferably 10-40%.
[0089] The fluorescent acrylic hydrogel antifouling coating prepolymer and the crosslinking agent are mixed uniformly at a temperature of 10 to 40°C. If the temperature at which the fluorescent acrylic hydrogel antifouling coating prepolymer and the crosslinking agent are mixed is lower than 10°C, the crosslinking activity will be reduced, and it will take longer to fully complete the crosslinking, which is not conducive to the efficient construction process and increases the production cost; if the temperature at which the fluorescent acrylic hydrogel antifouling coating prepolymer and the crosslinking agent are mixed is higher than 40°C, the activity of the crosslinking agent will increase, causing too many bubbles to appear in the coating, affecting the performance of the coating. Therefore, the temperature at which the fluorescent acrylic hydrogel antifouling coating prepolymer and the crosslinking agent are mixed is suitable to be 10 to 40°C, preferably 15 to 35°C.
[0090] The reaction container, electric stirring device, oil bath pot, drying device, etc. used in the present invention are all chemical equipment or devices commonly used in the field of chemical technology.
[0091] The hydrogel acrylic acid metal salt antifouling resin prepared by the present invention was analyzed by conventional infrared spectroscopy analysis method, and the analysis results are listed in the attached Figure 1 middle.
[0092] The invention relates to a fluorescent acrylic acid hydrogel antifouling coating prepared by a preparation method.
[0093] The present invention also relates to the use of the fluorescent acrylic hydrogel antifouling coating in preventing marine biofouling. The present invention examines the adhesion performance of the fluorescent acrylic hydrogel antifouling coating through a static bubble board; observes the fluorescent luminescence of the coating through a fluorescence microscope; examines its indoor antifouling performance through an algae growth inhibition experiment, and examines its outdoor antifouling performance through a real sea hanging board experiment. These specific test results are shown in the specific implementation method section.
[0094] [Beneficial Effects]
[0095] The beneficial technical effects of the present invention are:
[0096] (1) The present invention does not require the separate preparation of fluorescent compounds or fluorescent agents having a fluorescent effect, which can shorten the process flow and time.
[0097] (2) The fluorescent acrylic hydrogel antifouling coating prepared by the preparation method of the present invention can emit fluorescence in multiple excitation wavelength ranges, combining the hydrogel properties and multiple antifouling mechanisms of fluorescence.
[0098] (3) The method of imparting fluorescent properties to the hydrogel is not to introduce a fluorescent agent, and the original properties of the hydrogel will not be affected, such as its water absorption properties will not be affected by the fluorescent agent. The two antifouling mechanisms can achieve a mutually reinforcing synergistic effect, which is beneficial to prevent the formation of marine biofouling, and will not cause the fluorescent agent to be released into the environment and affect the environment. This coating exhibits good adhesion performance and indoor and outdoor antifouling effects.
[0099] (4) The fluorescent acrylic hydrogel antifouling coating has good film-forming properties, storage stability, and construction performance. Its preparation method is simple, and the raw materials are cheap and easily available, so it can be used for large-scale production of antifouling applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0100] Attached Figure 1 is the infrared spectrum of the fluorescent acrylic hydrogel antifouling coating prepared in Example 1-5;
[0101] Attached Figure 2 It is a fluorescent imaging diagram of the fluorescent acrylic hydrogel antifouling coating prepared in Example 1-5;
[0102] Attached Figure 3 is a graph showing the adhesion performance test results of the fluorescent acrylic hydrogel antifouling coating prepared in Example 1-5;
[0103] Attached Figure 4 This is a graph showing the anti-algae adhesion test results of the fluorescent acrylic hydrogel antifouling coating prepared in Example 1-5;
[0104] Attached Figure 5 This is a picture of the actual sea hanging board result of preparing fluorescent acrylic hydrogel antifouling coating in Example 1-5; DETAILED DESCRIPTION
[0105] The present invention is described in detail below with reference to the embodiments.
[0106] Example 1: Preparation of fluorescent acrylic hydrogel antifouling coating of the present invention
[0107] The implementation steps of this embodiment are as follows:
[0108] A. Preparation of Monomer Mixture
[0109] Butyl acrylate oily acrylate monomer, acrylic acid acrylic acid monomer, acrylamide acrylamide monomer, dimethylaminoethyl methacrylate acrylate amino ester monomer and hydroxypropyl acrylate water-based acrylate monomer are mixed uniformly in a molar ratio of 85:20:20:50:40, and then 1.2% of the initiator based on the total mass of the monomer initiator is added and mixed uniformly to obtain the monomer mixture;
[0110] B. Synthesis of fluorescent acrylic hydrogel antifouling coating prepolymer
[0111] Under nitrogen protection, 200% of a mixed organic solvent of xylene, n-butanol and ethanol (mass ratio 2:1.5:1) based on the total mass of the monomer mixture obtained in step A and 10% of the monomer mixture are added to a four-necked flask equipped with a stirrer, a condenser and a thermometer, and then the reaction system is heated to a temperature of 80°C; at the same time, the temperature is maintained for 20 minutes, and then the remaining monomer mixture is evenly divided into 7 parts, and one part is added every 15 minutes; after the monomer mixture is added, the temperature is kept for 1 hour, and then 0.01% of the above-mentioned initiator based on the total mass of the monomer mixture is added, and the reaction is continued for 2 hours to obtain the fluorescent acrylic hydrogel antifouling coating prepolymer;
[0112] C. Preparation of fluorescent acrylic hydrogel antifouling coating
[0113] According to the cross-linking agent being 25% of the molar amount of the acrylic acid monomer, the fluorescent acrylic hydrogel antifouling coating prepolymer obtained in step B and the aziridine CX-100 cross-linking agent are mixed uniformly at a temperature of 20° C., and then coated on a substrate for sufficient cross-linking and drying, thereby obtaining the fluorescent acrylic hydrogel antifouling coating Y1.
[0114] Conventional infrared spectroscopy analysis was used to determine that the product prepared in this embodiment was the fluorescent acrylic hydrogel antifouling coating. The results are shown in the attached Figure 1 The fluorescent microscope was used to take fluorescence images of the coating at different excitation wavelengths. The photos clearly show that the fluorescent acrylic hydrogel coating can present different colors of fluorescence within different excitation light wavelengths. The photos are shown in the attached Figure 2 .
[0115] Example 2: Preparation of fluorescent acrylic hydrogel antifouling coating of the present invention
[0116] The implementation steps of this embodiment are as follows:
[0117] A. Preparation of Monomer Mixture
[0118] The butyl acrylate oily acrylate monomer, the itaconic acid acrylate monomer and the acrylamide acrylamide monomer are mixed uniformly in a molar ratio of 20:5:5, and then 2.0% of the initiator based on the total mass of the monomer initiator is added and mixed uniformly to obtain the monomer mixture;
[0119] B. Synthesis of fluorescent acrylic hydrogel antifouling coating prepolymer
[0120] Under nitrogen protection, 150% of a mixed organic solvent of xylene, n-butanol and ethanol (mass ratio 3:1.5:1) based on the total mass of the monomer mixture obtained in step A and 5% of the monomer mixture are added to a four-necked flask equipped with a stirrer, a condenser and a thermometer, and then the reaction system is heated to a temperature of 65°C; at the same time, the temperature is maintained for 30 minutes, and then the remaining monomer mixture is evenly divided into 10 parts, and one part is added every 10 minutes; after the monomer mixture is added, the temperature is kept for 1 hour, and then 0.05% of the above-mentioned initiator based on the total mass of the monomer mixture is added, and the reaction is continued for 3 hours to obtain the fluorescent acrylic hydrogel antifouling coating prepolymer;
[0121] C. Preparation of fluorescent acrylic hydrogel antifouling coating
[0122] According to the cross-linking agent being 50% of the molar amount of the acrylic acid monomer, the fluorescent acrylic hydrogel antifouling coating prepolymer obtained in step B and the aziridine cross-linking agent XR-100 cross-linking agent are mixed uniformly at a temperature of 10° C., and then coated on a substrate for sufficient cross-linking and drying, thereby obtaining the fluorescent acrylic hydrogel antifouling coating Y2.
[0123] Conventional infrared spectroscopy analysis was used to determine that the product prepared in this embodiment was the fluorescent acrylic hydrogel antifouling coating. The results are shown in the attached Figure 1 The fluorescent microscope was used to take fluorescence images of the coating at different excitation wavelengths. The photos clearly show that the fluorescent acrylic hydrogel coating can present different colors of fluorescence within different excitation light wavelengths. The photos are shown in the attached Figure 2 .
[0124] Example 3: Preparation of fluorescent acrylic hydrogel antifouling coating of the present invention
[0125] The implementation steps of this embodiment are as follows:
[0126] A. Preparation of Monomer Mixture
[0127] n-Butyl methacrylate oily acrylate monomer, acrylic acid acrylate monomer, dimethylaminoethyl methacrylate amino acrylate monomer and hydroxyethyl acrylate water-based acrylate monomer are mixed uniformly in a molar ratio of 50:15:15:20, and then 0.4% of initiator based on the total weight of the monomers is added and mixed uniformly to obtain the monomer mixture;
[0128] B. Synthesis of fluorescent acrylic hydrogel antifouling coating prepolymer
[0129] Under nitrogen protection, 120% of the mixed organic solvent and 15% of the monomer mixture obtained in step A were added to a four-necked flask equipped with a stirrer, a condenser and a thermometer, and then the reaction system was heated to 95° C. At the same time, the temperature was maintained for 10 minutes, and then the remaining monomer mixture was evenly divided into 8 parts, and one part was added every 12 minutes; after the monomer mixture was added, the temperature was kept for 1 hour, and then 0.1% of the initiator was added based on the total mass of the monomer mixture, and the reaction was continued for 1 hour to obtain the fluorescent acrylic hydrogel antifouling coating prepolymer;
[0130] C. Preparation of fluorescent acrylic hydrogel antifouling coating
[0131] According to the cross-linking agent being 15% of the molar amount of the acrylic acid monomer, the fluorescent acrylic hydrogel antifouling coating prepolymer obtained in step B and the aziridine cross-linking agent XR-100 cross-linking agent are mixed uniformly at a temperature of 40° C., and then coated on a substrate for sufficient cross-linking and drying, thereby obtaining the fluorescent acrylic hydrogel antifouling coating Y3.
[0132] Conventional infrared spectroscopy analysis was used to determine that the product prepared in this embodiment was the fluorescent acrylic hydrogel antifouling coating. The results are shown in the attached Figure 1 The fluorescent microscope was used to take fluorescence images of the coating at different excitation wavelengths. The photos clearly show that the fluorescent acrylic hydrogel coating can present different colors of fluorescence within different excitation light wavelengths. The photos are shown in the attached Figure 2 .
[0133] Example 4: Preparation of fluorescent acrylic hydrogel antifouling coating of the present invention
[0134] The implementation steps of this embodiment are as follows:
[0135] A. Preparation of Monomer Mixture
[0136] Lauryl acrylate oily acrylate monomer, acrylic acid acrylic acid monomer, acrylamide acrylamide monomer, dimethylaminoethyl methacrylate acrylate amino ester monomer and 4-hydroxybutyl acrylate water-based acrylate monomer are mixed uniformly in a molar ratio of 60:10:5:15:10, and then 1.0% of initiator based on the total weight of the monomers is added and mixed uniformly to obtain the monomer mixture;
[0137] B. Synthesis of fluorescent acrylic hydrogel antifouling coating prepolymer
[0138] Under nitrogen protection, 50% of the mixed organic solvent and 12% of the monomer mixture, based on the total mass of the monomer mixture obtained in step A, are added to a four-necked flask equipped with a stirrer, a condenser and a thermometer, and then the reaction system is heated to a temperature of 85° C. At the same time, the temperature is maintained for 15 minutes, and then the remaining monomer mixture is evenly divided into 5 parts, and one part is added every 15 minutes; after the monomer mixture is added, the temperature is kept for 1 hour, and then 0.06% of the above-mentioned initiator, based on the total mass of the monomer mixture, is added, and the reaction is continued for 1.5 hours to obtain the fluorescent acrylic hydrogel antifouling coating prepolymer;
[0139] C. Preparation of fluorescent acrylic hydrogel antifouling coating
[0140] According to the cross-linking agent being 30% of the molar amount of the acrylic acid monomer, the fluorescent acrylic hydrogel antifouling coating prepolymer obtained in step B and the aziridine cross-linking agent CX-300 cross-linking agent are mixed uniformly at a temperature of 15° C., and then coated on a substrate for sufficient cross-linking and drying, thereby obtaining the fluorescent acrylic hydrogel antifouling coating Y4.
[0141] Conventional infrared spectroscopy analysis was used to determine that the product prepared in this embodiment was the fluorescent acrylic hydrogel antifouling coating. The results are shown in the attached Figure 1 The fluorescent microscope was used to take fluorescence images of the coating at different excitation wavelengths. The photos clearly show that the fluorescent acrylic hydrogel coating can present different colors of fluorescence within different excitation light wavelengths. The photos are shown in the attached Figure 2 .
[0142] Example 5: Preparation of fluorescent acrylic hydrogel antifouling coating of the present invention
[0143] The implementation steps of this embodiment are as follows:
[0144] A. Preparation of Monomer Mixture
[0145] n-Butyl methacrylate oily acrylate monomer, methacrylate acrylic acid monomer, N-hydroxymethyl acrylamide acrylamide monomer, dimethylamino acrylate acrylate amino ester monomer and hydroxypropyl methacrylate water-based acrylate monomer are mixed uniformly in a molar ratio of 35:18:10:20:12, and then 0.8% of initiator based on the total weight of the monomers is added and mixed uniformly to obtain the monomer mixture;
[0146] B. Synthesis of fluorescent acrylic hydrogel antifouling coating prepolymer
[0147] Under nitrogen protection, 180% of the mixed organic solvent and 0.8% of the monomer mixture, based on the total mass of the monomer mixture obtained in step A, are added to a four-necked flask equipped with a stirrer, a condenser and a thermometer, and then the reaction system is heated to a temperature of 75° C. At the same time, the temperature is maintained for 12 minutes, and then the remaining monomer mixture is evenly divided into 3 parts, and one part is added every 30 minutes; after the monomer mixture is added, the temperature is kept for 1 hour, and then 0.06% of the above-mentioned initiator, based on the total mass of the monomer mixture, is added, and the reaction is continued for 2.5 hours to obtain the fluorescent acrylic hydrogel antifouling coating prepolymer;
[0148] C. Preparation of fluorescent acrylic hydrogel antifouling coating
[0149] According to the cross-linking agent being 5% of the molar amount of the acrylic monomer, the fluorescent acrylic hydrogel antifouling coating prepolymer obtained in step B and the acrylic cross-linking agent CX-A10 cross-linking agent are mixed uniformly at a temperature of 22° C., and then coated on a substrate for sufficient cross-linking and drying, thereby obtaining the fluorescent acrylic hydrogel antifouling coating Y5.
[0150] Conventional infrared spectroscopy analysis was used to determine that the product prepared in this embodiment was the fluorescent acrylic hydrogel antifouling coating. The results are shown in the attached Figure 1 The fluorescent microscope was used to take fluorescence images of the coating at different excitation wavelengths. The photos clearly show that the fluorescent acrylic hydrogel coating can present different colors of fluorescence within different excitation light wavelengths. The photos are shown in the attached Figure 2 .
[0151] Application Example 1: Adhesion Performance Test of the Fluorescent Acrylic Hydrogel Antifouling Coating of the Present Invention
[0152] The implementation method of this application example is as follows:
[0153] Test samples: fluorescent acrylic hydrogel antifouling coatings Y1, Y2, Y3, Y4 and Y5 prepared in Examples 1-5;
[0154] Test substrate: acrylonitrile / butadiene / styrene copolymer (ABS) board, ABS board size is 100×80×1mm 3 ;
[0155] Pretreatment of test substrate: The ABS board was evenly polished with 80-grit sandpaper, then cleaned with ethanol and purified water, and dried at room temperature to constant weight.
[0156] Coating method: Coating by conventional coating method
[0157] Adhesion performance test basis: "Determination of salt water resistance of ship coatings-salt water and hot salt water immersion method" (GB / T10834-2008);
[0158] Specifically, the adhesion performance of the hydrogel acrylate metal salt antifouling resin of the present invention was tested by the static seawater bubble board method, and the test results are listed in the attached Figure 3 middle.
[0159] By the attached Figure 3 It can be seen that the hydrogel acrylate metal salt antifouling resin prepared in Examples 1-5 did not fall off during the 50-day static bubble board experiment and had good adhesion performance.
[0160] Application Example 2: Anti-algae adhesion performance test of the fluorescent acrylic hydrogel antifouling coating of the present invention The implementation method of this application example is as follows:
[0161] Test samples: fluorescent acrylic hydrogel antifouling coatings Y1, Y2, Y3, Y4 and Y5 prepared in Examples 1-5;
[0162] The non-fluorescent acrylic hydrogel coating Y01 is a coating prepared by our laboratory according to the existing conventional preparation method;
[0163] The blank sample Y0 is a substrate without any coating on the surface;
[0164] Test substrate: Acrylonitrile / butadiene / styrene copolymer (ABS) board, ABS board size is 50×50×1mm 3 ;
[0165] Pretreatment of test substrate: The ABS board was evenly polished with 80-grit sandpaper, then cleaned with ethanol and purified water, and dried at room temperature to constant weight.
[0166] Coating method: Use conventional coating method;
[0167] The anti-algae adhesion test was based on the method described by Feng Kang et al. in the literature “Synthesis and antifouling evaluation of indole derivatives”, Ecotoxicology and Environmental Safety, Vol. 182, p. 109423;
[0168] The test steps of the anti-algae adhesion experiment are as follows: according to the method described in the literature on the comparison of algae cell counting methods in algae growth inhibition experiments, a nutrient solution is prepared with vitamins, sodium nitrate, sodium phosphate, sodium silicate and trace elements in the ratio of 50:100:100:100:50 (μL / 100mL seawater), and the nutrient solution is then prepared with crescent-shaped Nitzschia closterium cultured to the exponential growth cycle to form an algae solution with an absorbance of 0.09 at an ultraviolet absorption wavelength of 680nm.
[0169] Place the fluorescent acrylic hydrogel antifouling coating sample face up in a weighing bottle, add 40 mL of the algae solution, and then place the culture dish in an incubator with a light intensity of 4000 lux, a light-dark ratio of 14:10, and a temperature of 21°C. After 7 days, take out the coating sample and rinse its surface with the algae solution in the culture dish to remove the algae attached to the surface. Then use 20 mL of nutrient solution to rinse all the algae attached to the coating surface into another culture dish, and then use an ultraviolet spectrophotometer to measure the absorbance of the rinse solution at a wavelength of 680 nm. The concentration of algae is calculated according to the standard working curve of algae growth, and the number of algae per unit area is calculated according to the coating area. The seawater used is filtered through a sand core funnel and sterilized in a high-temperature sterilizer (121°C).
[0170] The results of the anti-algae attachment experiment are listed in the attached Figure 4 In, by the attached Figure 4 It can be seen that compared with the blank sample Y0 and the acrylic hydrogel coating Y01 without fluorescent properties, the algae density attached to the surface of the fluorescent acrylic hydrogel antifouling coating prepared in Examples 1-5 is significantly less, which proves that the fluorescent acrylic hydrogel antifouling coating of the present invention has good anti-algae adhesion ability and is significantly better than the acrylic hydrogel antifouling coating without fluorescent properties.
[0171] Application Example 3: Performance Test of the Fluorescent Acrylic Hydrogel Antifouling Coating of the Present Invention on a Real Sea Board This application example is implemented as follows:
[0172] Test samples: fluorescent acrylic hydrogel antifouling coatings Y1, Y2, Y3, Y4 and Y5 prepared in Examples 1-5;
[0173] The blank sample is a control PVC substrate without any coating on the surface;
[0174] Test substrate: PVC, size 900×300×3mm 3
[0175] Pretreatment of test substrate: The PVC board was evenly polished with 80-grit sandpaper, then cleaned with ethanol and purified water, and dried at room temperature to constant weight;
[0176] Coating method: conventional coating method;
[0177] Antifouling performance test basis: National standard "Antifouling paint sample shallow sea immersion test method" (GB / T 5370-2007);
[0178] Testing time: October 2023;
[0179] Antifouling performance test results:
[0180] The test results are shown in the attached Figure 5, wherein the blank represents the biological fouling test results of the control plate without any coating, and Y1, Y2, Y3, Y4 and Y5 respectively represent the biological fouling adhesion test results of the fluorescent acrylic hydrogel antifouling coating prepared in Examples 1-5 for 35 days.
[0181] By the attached Figure 5 It can be seen that when the blank plate was 35 days old, a thick biofilm and some algae were attached to the surface, while there was basically no biofilm and algae adhesion on the surface of Y1, Y2, Y3, Y4 and Y5 coatings. These results fully prove that the fluorescent acrylic hydrogel antifouling coating prepared by the present invention has good antifouling ability in real sea.
Claims
1. A method for preparing a fluorescent acrylic hydrogel antifouling coating, characterized in that The preparation steps of the preparation method are as follows: A. Preparation of Monomer Mixture The oily acrylate monomer, acrylic acid monomer, acrylamide monomer, acrylate amino ester monomer and water-based acrylate monomer are mixed uniformly in a molar ratio of 20-85:5-20:0-20:0-50:0-40, and then 0.4-2.0% of an initiator based on the total weight of the monomers is added and mixed uniformly to obtain the monomer mixture; B. Synthesis of fluorescent acrylic hydrogel antifouling coating prepolymer Under nitrogen protection, 50-200% of the mixed organic solvent and 5-15% of the monomer mixture obtained in step A are added to a four-necked flask equipped with a stirrer, a condenser and a thermometer, and then the reaction system is heated to a temperature of 65-95° C.; at the same time, the temperature is maintained for 10-30 minutes, and then the remaining monomer mixture is evenly divided into 3-10 parts, and one part is added every 10-30 minutes; after the monomer mixture is added, the temperature is kept for 1 hour, and then 0.01-0.1% of the above-mentioned initiator is added based on the total mass of the monomer mixture, and the reaction is continued for 1-3 hours to obtain the fluorescent acrylic hydrogel antifouling coating prepolymer; C. Preparation of fluorescent acrylic hydrogel antifouling coating According to the crosslinking agent being 5-50% of the molar amount of the acrylic monomer, the fluorescent acrylic hydrogel antifouling coating prepolymer obtained in step B is mixed with the crosslinking agent at a temperature of 10-40° C., and then coated on a substrate for full crosslinking and drying, thereby obtaining the fluorescent acrylic hydrogel antifouling coating.
2. The preparation method according to claim 1, characterized in that In step A, the oily acrylic acid ester monomer is one or more oily acrylic acid ester monomers selected from methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, butyl acrylate, butyl methacrylate, isobutyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, dodecyl acrylate, dodecyl methacrylate, myristyl acrylate, myristyl methacrylate, hexadecyl acrylate, octadecyl acrylate or octadecyl methacrylate.
3. The preparation method according to claim 1, characterized in that In step A and step C, the acrylic acid monomer is one or more acrylic acid monomers selected from acrylic acid, methacrylic acid or itaconic acid.
4. The preparation method according to claim 1, characterized in that In step A, the acrylamide monomer is one or more acrylamide monomers selected from acrylamide, N-hydroxymethyl acrylamide, N-hydroxyethyl acrylamide, N,N-methylenebisacrylamide, N,N-dimethyl acrylamide, N,N-diethyl acrylamide, N-isopropyl acrylamide or N-tert-butyl acrylamide; the amino acrylate monomer is one or more amino acrylate monomers selected from dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate or 3-(dimethylamino)propyl acrylate; the water-based acrylate monomer is one or more water-based acrylate monomers selected from hydroxymethyl acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 2-(hydroxymethyl)methyl acrylate or 2-(hydroxymethyl)ethyl acrylate.
5. The preparation method according to claim 1, characterized in that In step A, the initiator is one or more initiators selected from azobisisobutyronitrile, azobisisoheptanenitrile, dibenzoyl peroxide, di(2-ethylhexyl) peroxydicarbonate, di-tert-butyl peroxide, dodecyl peroxide, tert-butyl perbenzoate, potassium persulfate or ammonium persulfate.
6. The preparation method according to claim 1, characterized in that In step B, the organic solvent is one or more organic solvents selected from xylene, methyl isobutyl ketone, butyl acetate, n-butanol, ethanol or cyclohexanone.
7. The preparation method according to claim 1, characterized in that In step B, the fluorescent acrylic hydrogel antifouling coating prepolymer has the following chemical structural formula (I): Where: R1, R5 and R8 represent H or CH3; R2 represents CH3, CH2CH3, CH2CH2CH3, CH2CH2CH2CH3, CH2CH(CH3)2, C(CH3)3, CH2CH(CH2CH3)(CH2)3CH3, (CH2)7CH3, (CH2) 11 CH3, (CH2) 13 CH3, (CH2) 15 CH3 or (CH2) 17 CH3; R3 represents H, CH3 or CH2COOH; R4 represents H, CH2OH, (CH2)2OH, CH2NHCOCHCH2, (CH3)2, (CH2CH3)2, CH(CH3)2 or C(CH3)3; R6 represents CH2CH2 or CH2CH2CH2; R7 and R 10 represents CH3 or CH2CH3; R9 represents CH2, CH2CH2, CH2CH2CH2, CH2CHCH3 or CH2CH2CH2CH2; a, b are positive integers, i, o, u, n are 0 or positive integers, i and o cannot be 0 at the same time; Its number average molecular weight is 10,000 to 1,000,000, and its molecular weight distribution is 1.0 to 3.
5.
8. The preparation method according to claim 1, characterized in that In step C, the crosslinking agent is one or more crosslinking agents selected from aziridine crosslinking agent XR-100, aziridine crosslinking agent CX-100, aziridine crosslinking agent CX-300, aziridine crosslinking agent XC-103, acrylic crosslinking agent CX-A10 or silicone crosslinking agent Silicone-9301.
9. The fluorescent acrylic hydrogel antifouling coating prepared according to the preparation method according to any one of claims 1 to 8.
10. Use of the fluorescent acrylic hydrogel antifouling coating according to claim 9 in preventing the formation of marine biofouling.
Citation Information
Patent Citations
Hydrogel capable of being used for marine antifouling, preparation method and uses thereof
CN110358006A
Surface micro-structure self-polishing antifouling coating and preparation method thereof
CN110684421A
Preparation method and application of acrylic-based hydrogel anti-fouling material
CN113881069A
Near-infrared photoluminescence gradient hydrogel as well as preparation method and application thereof
CN118165176A
Silicone hydrogels with amino surface groups
US20090103045A1
Cited By
Isobornyl acrylate polymer hydrogel material and synthesis method thereof
CN122381241A
Eugenol carbon dot fluoride-free acrylate polymer antifouling material and synthesis method thereof