A TPO coated board and preparation method thereof
By using an adhesive layer made of phenolic resin and other materials in the TPO film-coated board, the problem of peeling off of the traditional metal plate roof waterproof layer in high temperature and rain environments is solved, and the bonding strength and service life are significantly improved.
Patent Information
- Application Number
- CN202410493123.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-23
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-04-23
AI Technical Summary
Traditional metal plate roofs are difficult to renovate after installing photovoltaic modules and have poor waterproof and weather resistance. As a result, TPO film-coated panels are prone to peeling or blistering in high temperature and rainy environments, affecting their service life.
Adopting an adhesive layer made of phenolic resin, silane-modified polyester, polyolefin adhesive and maleic anhydride-grafted POE to enhance the bonding strength between the TPO waterproof layer and the metal plate, and through a high-temperature hot pressing process Optimize the heat resistance of the bonding layer.
It improves the bonding strength of TPO film-coated panels in high temperature and rain environments, extends its service life, avoids bulging and detachment, and significantly improves waterproof performance.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the field of building materials, and more specifically, to a TPO film-coated board and a preparation method thereof. Background Art
[0002] Solar photovoltaic power generation can provide clean electricity for enterprises and residents, and is recognized as a clean energy source in the world. With the continuous development of photovoltaic technology, the application benefits of photovoltaic technology have been significantly improved, and large idle roofs of factory buildings have become the best choice for installing photovoltaic modules. At present, the roof structure of large-area factories and public facilities buildings, which are the main carriers of rooftop solar power generation, is mainly traditional metal sheet roofs. Considering that once the rooftop solar energy system is installed and put into use, it is difficult to renovate the roof in use, which puts forward higher requirements for the waterproof and weather-resistant functions of the building roof. Conventional metal sheet roofs have poor waterproof, corrosion and weather resistance. Once corroded and damaged, the photovoltaic modules need to be removed and the metal sheet needs to be replaced as a whole, which is very expensive.
[0003] Film-coated panels for construction are a type of material widely used in the construction industry. By covering the surface of the substrate with one or more layers of functional films, the purpose of protection, decoration, and enhancement can be achieved. Compounding TPO waterproofing membranes onto metal plates can greatly increase the corrosion resistance and waterproof properties of metal plates, making TPO film-coated panels play an important role in the field of building waterproofing. However, since the surface of the metal plate is usually relatively smooth, the interfacial tension between the metal plate and the TPO material is large, and the bonding force is insufficient, it is easy for the TPO film layer to peel off or blister between the metal plate. In particular, the current preparation of TPO film-coated panels is mainly made by high-temperature hot pressing technology. Under high temperature conditions, the structural changes of the TPO waterproof layer lead to a decrease in the bonding strength between the metal plate and TPO. When the film-coated panels are exposed outdoors for a long time, they are prone to cracking in high temperature, rain and other environments for a long time, which affects the service life of the film-coated panels. Therefore, improving the bonding strength between the TPO film layer and the metal plate is important for TPO film-coated panels in the field of building waterproof materials. Summary of the invention
[0004] In order to improve the bonding strength between a TPO coating layer and a metal plate, the present application provides a TPO coating plate and a preparation method thereof.
[0005] In the first aspect, the present application provides a TPO coated board, which adopts the following technical solution:
[0006] A TPO coated board comprises, from bottom to top, a metal plate, an adhesive layer and a TPO waterproof layer, wherein the adhesive layer comprises the following raw materials in parts by weight:
[0007] 8-15 parts of phenolic resin, 5-10 parts of triphenylmethane triisocyanate, 15-25 parts of silane-modified polyester, 20-30 parts of polyolefin adhesive and 30-40 parts of maleic anhydride grafted POE. The silane-modified polyester is obtained by polymerizing silane monomer, versatate and vinyl benzoate in a mass ratio of 1: (0.3-0.5): (0.8-1.2).
[0008] By adopting the above technical scheme, the metal plate and the TPO waterproof layer in the present application are bonded by an adhesive layer, and the adhesive layer is mainly composed of maleic anhydride grafted POE binder resin and polyolefin adhesive, which has excellent bonding properties to metal and can enhance the bonding effect between the metal and the TPO waterproof layer. The TPO waterproof layer is polymerized from ethylene propylene rubber and polypropylene, and then prepared by adding antioxidants, anti-aging agents and other additives. Triphenylmethane triisocyanate is also added in the present application, which has excellent bonding properties between the rubber and the metal plate in the TPO waterproof layer, and the phenolic resin contains a large amount of hydroxymethyl and phenolic hydroxyl groups, which has good bonding strength between the metal plate and the TPO waterproof layer, and it has good heat resistance, which makes up for the damage to the bonding strength between the TPO waterproof layer and the metal plate when the two are formed by a high-temperature hot pressing process, and improves the bonding strength between the TPO waterproof layer and the metal plate in the final laminate.
[0009] Silane-modified polyester is obtained by polymerization of silane monomer, versatate vinyl ester and vinyl benzoate. The adhesive obtained by copolymerization of versatate vinyl ester and vinyl benzoate has excellent bonding effect on metal and TPO waterproof layer. Moreover, versatate vinyl ester has rich alkyl groups, which forms a steric hindrance effect and has a protective effect on itself, so that the obtained polyester has excellent self-cohesion and high bonding strength. The introduction of benzene ring groups in vinyl benzoate greatly improves the heat resistance of polyester. Combined with the introduction of siloxane groups in silane monomers, the heat resistance is further improved, so that the bonding layer has excellent heat resistance, reduces the damage to the adhesive structure in the subsequent high-temperature hot pressing process, resulting in a decrease in bonding strength, improves the bonding strength of the final laminated board, and will not bulge or fall off when it is exposed to high temperature, rain and other environments outdoors for a long time, thereby extending its service life.
[0010] Optionally, the silane-modified polyester is prepared by the following method:
[0011] Add vinyl benzoate and vinyl versatate to ethyl acetate, then add initiator, react at 75-85°C for 4-6h, then add silane monomer and catalyst when the temperature is lowered to 60-70°C, react at 90-110°C for 2-3h, then filter, wash and dry to obtain silane-modified polyester.
[0012] By adopting the above technical scheme, versatate vinyl carbonate and vinyl benzoate are first added to a solvent to undergo a polymerization reaction under the presence of an initiator to obtain polyester, and then a silane monomer is added. Under the action of a catalyst and an initiator, the silane monomer and the polyester are condensed, thereby introducing a silane group into the polyester molecular chain, achieving silane modification of the polyester, improving the heat resistance of the polyester, and having excellent bonding properties.
[0013] Optionally, the silane monomer includes one or both of 3-methacryloxypropyltrimethoxysilane and 3-methacryloxypropyldiethoxysilane.
[0014] Optionally, the adhesive layer is prepared by the following steps: mixing the raw materials of the adhesive layer at 60-70° C. for 40-60 min, and then calendering and extruding to obtain the adhesive layer.
[0015] Optionally, the TPO waterproof layer comprises the following raw materials in parts by weight:
[0016] 40-50 parts of TPO resin, 10-18 parts of modified ethylene-propylene rubber, 20-30 parts of polypropylene, 5-10 parts of styrene, 1-3 parts of peroxide crosslinking agent, 0.5-1.5 parts of antioxidant, 0.5-1.5 parts of anti-aging agent, 1-5 parts of filler and 0.2-0.5 parts of anti-ultraviolet agent;
[0017] The modified EPDM rubber is prepared by modifying EPDM rubber with 2-methyl fluoroacrylate and 2-vinylpyridine.
[0018] By adopting the above technical scheme, the TPO waterproof layer in the present application is mainly made of TPO resin and polypropylene, and modified ethylene propylene rubber and styrene are also added. The modified ethylene propylene rubber is made of 2-fluoromethyl acrylate and 2-vinylpyridine modified ethylene propylene rubber. The 2-fluoromethyl acrylate introduces a fluorocarbon group, which significantly improves the high temperature resistance of the TPO waterproof layer. The introduction of the pyridine group in 2-vinylpyridine forms a π-π stacking effect with the benzene ring introduced in the adhesive layer, thereby strengthening the bonding strength between the adhesive layer and the TPO waterproof layer, and further enhancing the bonding strength between the waterproof layer and the metal plate. The TPO film-coated board will not bulge or crack under long-term outdoor high temperature and rain conditions, thereby extending the service life of the film-coated board.
[0019] Optionally, 3-5 parts by weight of trimethylolpropane triacrylate are also added to the adhesive layer raw material.
[0020] By adopting the above technical scheme, trimethylolpropane triacrylate in the adhesive layer can form precipitation graft polymerization with styrene in the TPO waterproof layer, thereby strengthening the chemical reaction between the TPO waterproof layer and the adhesive layer, enhancing the bonding strength, and further enhancing the bonding strength between the metal plate and the waterproof layer.
[0021] Optionally, the modified ethylene-propylene rubber is prepared by the following method:
[0022] In parts by weight, 30-40 parts of EPDM rubber are melted at 200-220° C., and then 5-10 parts of methyl 2-fluoroacrylate and 8-15 parts of 2-vinyl pyridine are added, and then 3-5 parts of initiator are added and blended to prepare modified EPDM rubber.
[0023] By adopting the above technical scheme, under the action of an initiator, 2-fluoromethyl acrylate and 2-vinylpyridine are polymerized with unsaturated functional groups in EPDM rubber through unsaturated functional groups to obtain modified EPDM rubber, which significantly improves its high temperature resistance and bonding strength with the adhesive layer.
[0024] Optionally, the peroxide cross-linking agent in the TPO waterproof layer is selected from one or more of diisopropylbenzene peroxide, di-tert-butyl diisopropylbenzene peroxide, and 2,4-dichlorobenzoyl peroxide;
[0025] The filler is a mixture of titanium dioxide and talcum powder or titanium dioxide and calcium carbonate.
[0026] Optionally, the TPO waterproof layer is prepared by the following method:
[0027] The modified EPDM rubber is processed at 150-180°C for 10-15 minutes, and then TPO resin, peroxide crosslinking agent, polypropylene, antioxidant and filler are added and mixed for 20-30 minutes. The temperature is lowered to 60-70°C, antioxidant and anti-ultraviolet agent are added, and then styrene is added. After mixing for 10-20 minutes, it is extruded to obtain a TPO waterproof layer.
[0028] In a second aspect, the present application provides a method for preparing a TPO coated board, which adopts the following technical solution:
[0029] A method for preparing a TPO coated board comprises the following steps:
[0030] One side of the adhesive layer and the TPO waterproof layer are preheated and laminated at 120-140°C, and then the metal plate and the other side of the adhesive layer are hot-pressed and laminated at 140-160°C to obtain a TPO laminated board having a metal plate, an adhesive layer and a TPO waterproof structure from bottom to top.
[0031] By adopting the above technical scheme, the TPO waterproof layer and the metal plate in the TPO coated board prepared in the present application are firmly bonded by the adhesive layer, have excellent bonding strength, will not fall off or bulge in long-term outdoor high temperature and rain environments, and extend the service life of the TPO coated board.
[0032] In summary, this application has the following beneficial effects:
[0033] 1. In the present application, the metal plate and the TPO waterproof layer are bonded by an adhesive layer, and the adhesive layer is mainly composed of maleic anhydride grafted POE adhesive resin and polyolefin adhesive, which can enhance the bonding effect between the metal and the TPO waterproof layer. The addition of triphenylmethane triisocyanate enhances the bonding strength between the TPO waterproof layer and the metal plate, and the phenolic resin contains a large amount of hydroxymethyl and phenolic hydroxyl groups, which has good bonding strength for the metal plate and the TPO waterproof layer, and has good heat resistance, which makes up for the damage to the bonding strength of the TPO waterproof layer and the metal plate when the TPO waterproof layer and the metal plate are formed by a high-temperature hot pressing process, and improves the bonding strength between the TPO waterproof layer and the metal plate in the final laminated board;
[0034] 2. In the present application, the adhesive layer is added with silane monomer, tert-butyl vinyl ester and vinyl benzoate polymerized to obtain silane-modified polyester. The adhesive obtained by copolymerization of tert-butyl vinyl ester and vinyl benzoate has excellent bonding effect on metal and TPO waterproof layer. Moreover, tert-butyl vinyl ester has abundant alkyl groups, which forms a steric hindrance effect and has a protective effect on itself, so that the obtained polyester has excellent self-cohesion and high bonding strength. The introduction of benzene ring groups in vinyl benzoate greatly improves the heat resistance of polyester. The introduction of siloxane groups in silane monomer further improves the heat resistance, so that the adhesive layer has excellent heat resistance, reduces the damage to the adhesive structure in the subsequent high-temperature hot pressing process, and causes the decrease in bonding strength, improves the bonding strength of the final laminated board, and does not cause bulging, detachment, etc. when it is placed outdoors in high temperature, rain and other environments for a long time, thereby extending its service life.
[0035] 3. In the present application, the TPO waterproof layer is mainly made of TPO resin and polypropylene, and modified ethylene propylene rubber and styrene are also added. The modified ethylene propylene rubber is modified from ethylene propylene diene monomer rubber by 2-fluoromethyl acrylate and 2-vinyl pyridine. The fluorocarbon group is introduced into 2-fluoromethyl acrylate, which significantly improves the high temperature resistance of the TPO waterproof layer. The introduction of the pyridine group in 2-vinyl pyridine forms a π-π stacking effect with the benzene ring introduced in the adhesive layer, thereby strengthening the bonding strength between the adhesive layer and the TPO waterproof layer, and further enhancing the bonding strength between the waterproof layer and the metal plate. The TPO coated board will not bulge or crack under long-term outdoor high temperature and rain conditions, thereby extending the service life of the coated board. DETAILED DESCRIPTION
[0036] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.
[0037] In the following examples, maleic anhydride grafted POE is selected from Dow's maleic anhydride grafted POE, with a grade of TY1052H;
[0038] The phenolic resin is a liquid phenolic resin of model 2130 purchased from Wuxi Jiunai Anticorrosion Materials Co., Ltd.
[0039] Versatile vinyl carbonate was selected from Hubei Xingyan New Material Technology Co., Ltd., with a CAS number of 51000-52-3;
[0040] The polyolefin adhesive uses the polypropylene PP special glue model 11680 produced by Bezos Polymer New Materials (Dongguan) Co., Ltd.
[0041] The TPO resin is manufactured by ExxonMobil Chemical Co., Ltd. and is branded as TPO American ExxonMobil BMV301;
[0042] EPDM was purchased from Shanghai Sutong Industrial Co., Ltd., with the brand name 3072EM;
[0043] The antioxidant is antioxidant 4010;
[0044] The anti-ultraviolet agent is ultraviolet absorber UV-P;
[0045] The antioxidant used is antioxidant 1010.
[0046] Example 1
[0047] A method for preparing a TPO coated board comprises the following steps:
[0048] S1. Preparation of TPO waterproof layer: specifically comprising the following steps:
[0049] S1-1: preparing modified EPDM rubber, taking 35 kg of EPDM rubber and melting it at 210° C., then adding 8 kg of 2-fluoromethyl acrylate and 12 kg of 2-vinyl pyridine, and then adding 4 kg of initiator potassium persulfate and blending for 1.5 hours to obtain modified EPDM rubber;
[0050] S1-2: Preparation of TPO waterproof layer: 10 kg of the modified ethylene-propylene rubber prepared in step S1-1 was mixed at 160°C for 15 min, and then 45 kg of TPO resin, 2 kg of peroxide crosslinking agent, 25 kg of polypropylene, 1 kg of antioxidant 4010 and 3 kg of filler were added, and mixed for 25 min, the temperature was lowered to 65°C, 1 kg of antioxidant 1010 and 0.3 kg of ultraviolet absorber UV-P were added, and then 8 kg of styrene was added. After mixing for 15 min, the mixture was extruded to obtain a TPO waterproof layer with a thickness of 0.3 mm;
[0051] The filler is a mixture of titanium dioxide and talcum powder in a mass ratio of 1:0.5; the peroxide cross-linking agent is diisopropylbenzene peroxide;
[0052] S2, preparing the bonding layer: specifically comprising the following steps:
[0053] S2-1, preparation of silane-modified polyester: based on 1 kg of vinyl benzoate, vinyl benzoate and vinyl versatate are added to ethyl acetate, and then an initiator dibenzoyl peroxide is added, and the mixture is reacted at 80° C. for 5 h, and then the silane monomer and catalyst dibutyltin dilaurate are added when the temperature is lowered to 65° C., and the mixture is reacted at 100° C. for 2.5 h, and then filtered, washed and dried to obtain the silane-modified polyester;
[0054] The mass ratio of silane monomer, versatate vinyl ester and vinyl benzoate is 1:0.4:1, and the silane monomer is 3-methacryloxypropyltrimethoxysilane, the amount of ethyl acetate added is 4 times the mass of vinyl benzoate, the amount of initiator added is 4wt% of the amount of vinyl benzoate added, and the amount of catalyst added is 2wt% of the amount of vinyl benzoate added;
[0055] S2-2, preparing an adhesive layer: 12 kg of phenolic resin, 8 kg of triphenylmethane triisocyanate, 20 kg of the silane-modified polyester prepared in step S2-1, 25 kg of polyolefin adhesive, 4 kg of trimethylolpropane triacrylate and 35 kg of maleic anhydride-grafted POE were mixed at 65° C. for 50 min, and then rolled and extruded to obtain an adhesive layer with a thickness of 90 μm;
[0056] S3, preparing TPO film-coated board: preheating and compounding one side of the adhesive layer prepared in step S2-2 and the TPO waterproof layer prepared in step S1-2 at 130°C, and then hot-pressing and compounding the metal plate and the other side of the adhesive layer prepared in step S2-2 at 150°C to obtain a TPO film-coated board having a metal plate, an adhesive layer and a TPO waterproof structure from bottom to top.
[0057] Example 2
[0058] A method for preparing a TPO coated board comprises the following steps:
[0059] S1. Preparation of TPO waterproof layer: specifically comprising the following steps:
[0060] S1-1: preparing modified EPDM rubber, taking 30 kg of EPDM rubber and melting it at 200°C, then adding 5 kg of 2-fluoromethyl acrylate and 8 kg of 2-vinyl pyridine, and then adding 3 kg of initiator potassium persulfate and blending for 1 hour to obtain modified EPDM rubber;
[0061] S1-2: Preparation of TPO waterproof layer: 10 kg of the modified ethylene-propylene rubber prepared in step S1-1 was mixed at 150°C for 15 min, and then 40 kg of TPO resin, 1 kg of peroxide crosslinking agent, 20 kg of polypropylene, 0.5 kg of antioxidant 4010 and 1 kg of filler were added, and mixed for 20 min, the temperature was lowered to 60°C, 0.5 kg of antioxidant 1010 and 0.2 kg of ultraviolet absorber UV-P were added, and then 5 kg of styrene was added. After mixing for 10 min, the mixture was extruded to obtain a TPO waterproof layer with a thickness of 0.2 mm;
[0062] The filler is a mixture of titanium dioxide and talcum powder in a mass ratio of 1:0.5; the peroxide cross-linking agent is diisopropylbenzene peroxide;
[0063] S2, preparing the bonding layer: specifically comprising the following steps:
[0064] S2-1, preparation of silane-modified polyester: based on 1000g of vinyl benzoate, vinyl benzoate and vinyl versatate are added to ethyl acetate, and then an initiator dibenzoyl peroxide is added, and the mixture is reacted at 75°C for 6h, and then the silane monomer and catalyst dibutyltin dilaurate are added when the temperature is lowered to 60°C, and the mixture is reacted at 90°C for 3h, and then filtered, washed and dried to obtain the silane-modified polyester;
[0065] The mass ratio of silane monomer, vinyl ester and vinyl benzoate is 1:0.3:0.8, and the silane monomer is 3-methacryloxypropyltrimethoxysilane, the amount of ethyl acetate added is 3 times the mass of vinyl benzoate, the amount of initiator added is 3wt% of the amount of vinyl benzoate added, and the amount of catalyst added is 1wt% of the amount of vinyl benzoate added;
[0066] S2-2, preparing an adhesive layer: 8 kg of phenolic resin, 5 kg of triphenylmethane triisocyanate, 15 kg of the silane-modified polyester prepared in step S2-1, 20 kg of polyolefin adhesive, 3 kg of trimethylolpropane triacrylate and 30 kg of maleic anhydride-grafted POE were mixed at 60° C. for 60 min, and then rolled and extruded to obtain an adhesive layer with a thickness of 80 μm;
[0067] S3, preparing TPO film-coated board: preheating and compounding one side of the adhesive layer prepared in step S2-2 and the TPO waterproof layer prepared in step S1-2 at 120°C, and then hot-pressing and compounding the metal plate and the other side of the adhesive layer prepared in step S2-2 at 140°C to obtain a TPO film-coated board having a metal plate, an adhesive layer and a TPO waterproof structure from bottom to top.
[0068] Example 3
[0069] A method for preparing a TPO coated board comprises the following steps:
[0070] S1. Preparation of TPO waterproof layer: specifically comprising the following steps:
[0071] S1-1: preparing modified EPDM rubber, taking 40 kg of EPDM rubber and melting it at 220° C., then adding 10 kg of methyl 2-fluoroacrylate and 15 kg of 2-vinyl pyridine, and then adding 5 kg of initiator potassium persulfate and blending for 2 hours to obtain modified EPDM rubber;
[0072] S1-2: Preparation of TPO waterproof layer: 18 kg of the modified ethylene-propylene rubber prepared in step S1-1 was mixed at 180°C for 10 min, and then 50 kg of TPO resin, 3 kg of peroxide crosslinking agent, 30 kg of polypropylene, 1.5 kg of antioxidant 4010 and 5 kg of filler were added, and mixed for 30 min, the temperature was lowered to 70°C, 1.5 kg of antioxidant 1010 and 0.5 kg of ultraviolet absorber UV-P were added, and then 10 kg of styrene was added, mixed for 20 min, and extruded to obtain a TPO waterproof layer with a thickness of 0.5 mm;
[0073] The filler is a mixture of titanium dioxide and talcum powder in a mass ratio of 1:0.5; the peroxide cross-linking agent is diisopropylbenzene peroxide;
[0074] S2, preparing the bonding layer: specifically comprising the following steps:
[0075] S2-1, preparation of silane-modified polyester: based on 1000g of vinyl benzoate, vinyl benzoate and vinyl versatate are added to ethyl acetate, and then an initiator dibenzoyl peroxide is added, and the mixture is reacted at 85°C for 4h, and then the silane monomer and catalyst dibutyltin dilaurate are added when the temperature is lowered to 70°C, and the mixture is reacted at 110°C for 2h, and then filtered, washed and dried to obtain the silane-modified polyester;
[0076] The mass ratio of silane monomer, vinyl ester and vinyl benzoate is 1: 0.5: 1.2, and the silane monomer is 3-methacryloxypropyltrimethoxysilane, the amount of ethyl acetate added is 4 times the mass of vinyl benzoate, the amount of initiator added is 5wt% of the amount of vinyl benzoate added, and the amount of catalyst added is 3wt% of the amount of vinyl benzoate added;
[0077] S2-2, preparing an adhesive layer: 15 kg of phenolic resin, 10 kg of triphenylmethane triisocyanate, 25 kg of the silane-modified polyester prepared in step S2-1, 30 kg of polyolefin adhesive, 5 kg of trimethylolpropane triacrylate and 40 kg of maleic anhydride-grafted POE were mixed at 70° C. for 40 min, and then rolled and extruded to obtain an adhesive layer with a thickness of 100 μm;
[0078] S3, preparing TPO film-coated board: preheating and compounding one side of the adhesive layer prepared in step S2-2 and the TPO waterproof layer prepared in step S1-2 at 140°C, and then hot-pressing and compounding the metal plate and the other side of the adhesive layer prepared in step S2-2 at 160°C to obtain a TPO film-coated board having a metal plate, an adhesive layer and a TPO waterproof structure from bottom to top.
[0079] Example 4
[0080] A method for preparing a TPO coated board is carried out according to the method in Example 1, except that, when preparing the TPO waterproof layer in step S1, the EPDM rubber is not modified, and in step S2-2, the modified EPDM rubber is directly replaced with EPDM rubber in equal amounts.
[0081] Example 5
[0082] A method for preparing a TPO coated board is carried out according to the method in Example 1, except that when preparing the TPO waterproof layer in step S1, an equal amount of 2-vinylpyridine is replaced by methyl 2-fluoroacrylate in step S1-1.
[0083] Example 6
[0084] A method for preparing a TPO coated board is carried out according to the method in Example 1, except that when preparing the TPO waterproof layer in step S1, an equal amount of 2-fluoroacrylate is replaced by 2-vinylpyridine in step S1-1.
[0085] Example 7
[0086] A method for preparing a TPO coated board is carried out according to the method in Example 1, except that when preparing the adhesive layer in step S2-2, trimethylolpropane triacrylate is not added to the raw materials.
[0087] Comparative Example 1
[0088] A method for preparing a TPO film-coated board is carried out according to the method in Example 1, except that when preparing the adhesive layer in step S2-2, no silane-modified polyester is added to the raw material of the adhesive layer.
[0089] Comparative Example 2
[0090] A method for preparing a TPO coated board is carried out according to the method in Example 1, except that when preparing the adhesive layer in step S2-2, the silane-modified polyester in the adhesive layer raw material is directly replaced with versatate in equal amounts.
[0091] Comparative Example 3
[0092] A method for preparing a TPO coated board is carried out according to the method in Example 1, except that in step S2-1, no silane monomer is added, an initiator dibenzoyl peroxide is added, and after reacting at 80° C. for 5 hours, the mixture is directly filtered, washed and dried to obtain a silane-modified polyester.
[0093] Comparative Example 4
[0094] A method for preparing a TPO coated board is carried out according to the method in Example 1, except that in step S2-1, an equal amount of vinyl benzoate is replaced by versatate vinyl carbonate.
[0095] Comparative Example 5
[0096] A method for preparing a TPO coated board is carried out according to the method in Example 1, except that in step S2-1, an equal amount of versatate is replaced by vinyl benzoate.
[0097] Comparative Example 6
[0098] A method for preparing a TPO coated board is carried out according to the method in Example 1, except that maleic anhydride-grafted POE is not added in step S2-2.
[0099] Comparative Example 7
[0100] A method for preparing a TPO coated board is carried out according to the method in Example 1, except that triphenylmethane triisocyanate is not added in step S2-2.
[0101] Performance Testing
[0102] The TPO coated panels prepared in the above examples and comparative examples were cross-sectionalized according to the adhesion test method in T / CBMCA 017-2020 "Film-coated steel panels for construction". Both sides of the coated panels were cross-sectionalized to 3mm×3mm. The cross-sectional panels were then boiled in boiling water for 48 hours according to this standard to observe whether there was bulging or peeling. At the same time, the prepared TPO coated panel samples were aged in a standard oven at 115°C for 28 days, and then the peel strength of the coated panels was tested according to T / CBMCA 017-2020 "Film-coated steel panels for construction". The test results are shown in Table 1 below:
[0103] Table 1:
[0104]
[0105] After the TPO coated board is boiled in boiling water, the bubbling and shedding phenomena occur, and the severity of the phenomena decreases in order from severe bubbling / shedding, obvious bubbling / shedding, less bubbling / shedding, to slight bubbling / shedding.
[0106] Referring to the test results in Table 1 above, the TPO coated board prepared in the embodiment of the present application passed the test after boiling in water, and there was no bulging or falling off of the coating, and it had good bonding strength. Referring to the test results of Examples 1 and 4, when preparing the TPO waterproof layer, the ethylene-propylene rubber was not modified, and the peel strength of the TPO coated board after heat aging treatment was significantly reduced. The bonding strength between the metal plate of the TPO coated board and the TPO waterproof layer was high, and the bonding strength was still high even after high-temperature treatment. Referring to the test results of Examples 5 and 6, when the modified ethylene-propylene rubber only used 2-vinylpyridine or 2-methyl fluoroacrylate, the bonding strength was significantly reduced, especially when only 2-methyl fluoroacrylate was used for modification, the bonding strength was reduced more. The introduction of the pyridine group formed a chemical reaction with the benzene ring in the bonding layer to improve the bonding strength. Referring to the test results of Example 7, when trimethylolpropane triacrylate was not added to the raw material of the bonding layer, the bonding strength was also significantly reduced. The addition of trimethylolpropane triacrylate in the bonding layer formed a precipitation graft with styrene in the TPO waterproof layer, forming a chemical reaction, which significantly improved the bonding strength to the metal plate.
[0107] Referring to the test results of Comparative Examples 1 and 2, it can be seen that when silane-modified polyester is not added to the adhesive layer raw material in Comparative Example 1, the adhesive strength is low, and serious coating shedding occurs after boiling, while when silane-modified polyester is replaced with tert-butyl vinyl carbonate in an equal amount in Comparative Example 2, relatively obvious coating shedding also occurs after boiling, and the peeling strength is significantly reduced; combined with the test results of Comparative Example 3, when silane monomer is not added to the adhesive layer raw material, the coating bulges and shedding occurs after boiling, and the peeling strength is reduced, while when only tert-butyl vinyl carbonate or vinyl benzoate is added to the adhesive layer in Comparative Examples 4 and 5, the peeling strength is significantly reduced, and less coating bulging occurs after boiling. Combined with the test results of Comparative Examples 6 and 7, when maleic anhydride grafted POE or triphenylmethane triisocyanate is not added to the adhesive layer, less coating bulging occurs after boiling, and the peeling strength is low.
[0108] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.
Claims
1. A TPO film-faced board, characterized in that: The adhesive layer includes a metal plate, an adhesive layer and a TPO waterproof layer from bottom to top, wherein the adhesive layer includes the following raw materials in parts by weight: 8-15 parts of phenolic resin, 5-10 parts of triphenylmethane triisocyanate, 15-25 parts of silane-modified polyester, 20-30 parts of polyolefin adhesive and 30-40 parts of maleic anhydride grafted POE, wherein the silane-modified polyester is obtained by polymerizing a silane monomer, tert-butyl vinyl carbonate and vinyl benzoate in a mass ratio of 1: (0.3-0.5): (0.8-1.2); The silane monomer includes one or two of 3-methacryloxypropyltrimethoxysilane and 3-methacryloxypropyldiethoxysilane; The TPO waterproof layer comprises the following raw materials in parts by weight: 40-50 parts of TPO resin, 10-18 parts of modified ethylene-propylene rubber, 20-30 parts of polypropylene, 5-10 parts of styrene, 1-3 parts of peroxide crosslinking agent, 0.5-1.5 parts of antioxidant, 0.5-1.5 parts of anti-aging agent, 1-5 parts of filler and 0.2-0.5 parts of anti-ultraviolet agent; wherein the modified ethylene-propylene rubber is prepared from ethylene-propylene-diene rubber modified by 2-methyl fluoroacrylate and 2-vinylpyridine; 3-5 parts by weight of trimethylolpropane triacrylate are also added to the adhesive layer raw material.
2. A TPO film-faced board according to claim 1, characterized in that: The silane-modified polyester is prepared by the following method: vinyl benzoate and vinyl versatate are added to ethyl acetate, and then an initiator is added, and the reaction is carried out at 75-85°C for 4-6 hours, and then the silane monomer and the catalyst are added when the temperature is reduced to 60-70°C, and the reaction is carried out at 90-110°C for 2-3 hours, and then the silane-modified polyester is obtained by filtering, washing and drying.
3. The TPO film-faced board according to claim 1, characterized in that: The adhesive layer is prepared by the following steps: mixing the raw materials of the adhesive layer at 60-70° C. for 40-60 minutes, and then rolling and extruding to obtain the adhesive layer.
4. The TPO film-faced board according to claim 1, characterized in that: The modified EPDM rubber is prepared by the following method: 30-40 parts by weight of EPDM are melted at 200-220° C., 5-10 parts of methyl 2-fluoroacrylate and 8-15 parts of 2-vinylpyridine are added, and 3-5 parts of initiator are added for blending to prepare the modified EPDM rubber.
5. The TPO film-faced board according to claim 1, characterized in that: The peroxide crosslinking agent in the TPO waterproof layer is selected from one or more of dicumyl peroxide, di-tert-butyl dicumyl peroxide, and 2,4-dichlorobenzoyl peroxide; the filler is selected from a mixture of titanium dioxide and talcum powder or titanium dioxide and calcium carbonate.
6. The TPO film-faced board according to claim 1, characterized in that: The TPO waterproof layer is prepared by the following method: the modified ethylene-propylene rubber is kneaded at 150-180°C for 10-15 minutes, and then TPO resin, peroxide crosslinking agent, polypropylene, antioxidant and filler are added, kneaded for 20-30 minutes, the temperature is reduced to 60-70°C, antioxidant and anti-ultraviolet agent are added, and then styrene is added. After kneading for 10-20 minutes, it is extruded to obtain the TPO waterproof layer.
7. A method for preparing a TPO film-faced board according to any one of claims 1 to 6, characterized in that: The following steps are involved: One side of the adhesive layer and the TPO waterproof layer are preheated and laminated at 120-140°C, and then the metal plate and the other side of the adhesive layer are hot-pressed and laminated at 140-160°C to obtain a TPO laminated board having a metal plate, an adhesive layer and a TPO waterproof structure from bottom to top.
Citation Information
Cited By
TPO (thermoplastic polyolefin) film-coated plate and preparation method thereof
CN120116554A