A kind of water-based epoxy insulating paint and preparation method thereof
By using water-based epoxy resin and functional modifier in water-based epoxy insulating paint, the wear resistance, adhesion and corrosion resistance of the paint film are improved, and the corrosion resistance and low temperature of the insulating paint in the prior art are solved. The problem of insufficient curing and storage stability has achieved high-performance, environmentally friendly insulating paint solutions.
Patent Information
- Application Number
- CN202410550275.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-06
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-05-06
AI Technical Summary
The existing water-based epoxy insulating paint has shortcomings in corrosion resistance, low-temperature curing, adhesion and storage stability, which is difficult to meet the multiple needs of insulating materials in electronic and electrical production.
Using aqueous epoxy resin as the main component, combining pigments, coupling agents, fillers, anti-flash rust agents, leveling agents, defoaming agents and thickening agents, improve the paint film through specific component ratios and processes. Wear resistance, adhesion, corrosion resistance and hardness, and the bonding strength and flexibility of the paint film are enhanced by dehydrating ricinoleic acid and maleic anhydride.
It realizes excellent electrical insulation performance, adhesion, corrosion resistance and hardness of water-based epoxy insulating paint, and has good storage stability, simple production process and low cost, and is suitable for insulating paint applications in multiple fields.
Smart Images

Figure BDA0004824064480000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of insulating coatings, and in particular to a water-based epoxy insulating varnish and a preparation method thereof. Background Art
[0002] Insulating varnish is an important insulating material in the production process of electronic and electrical components. It not only involves the production and processing of electronic and electrical appliances, but also involves the upstream materials of electronic and electrical products. Whether for environmental protection itself or for the occupational health and safety of operators, the safety and environmental protection improvement of insulating varnish has become an inevitable and irreversible trend.
[0003] At present, the traditional solvent-based insulating paints used by various domestic electronic and electrical appliance manufacturers all contain a large amount of flammable and explosive toxic solvents such as benzene, ketone esters, etc. After construction, a large amount of harmful substances are volatilized, threatening human health and polluting the environment, so they will gradually be replaced by water-based insulating paints. Water-based insulating paint refers to insulating paint that uses water as a solvent. It is a new alternative product to solvent-based insulating paint. Compared with traditional solvent-based insulating paints, water-based insulating paints do not use benzene and other toxic and harmful solvents that pollute the environment, so they are more environmentally friendly and can also ensure the health of related construction workers. It is an environmentally friendly, low-odor insulating coating with broad application prospects.
[0004] Water-based epoxy resin insulating varnish uses water as solvent and has no volatile organic solvents, which meets environmental protection requirements; after curing, epoxy resin has the advantages of excellent mechanical strength, chemical resistance, electrical properties, moisture resistance, low shrinkage, high cost performance, etc. However, it still has various shortcomings, such as corrosion resistance, low temperature curing, adhesion and storage stability, etc., which need to be improved. Summary of the invention
[0005] The purpose of this application is to provide a water-based epoxy insulating varnish and a preparation method thereof in view of the deficiencies in current technology.
[0006] In the first aspect, the present application provides a water-based epoxy insulating paint, which adopts the following technical solution:
[0007] A water-based epoxy insulating paint comprises a component A and a component B, wherein the mass ratio of the component A to the component B is 3-5:1; the component A comprises the following raw materials by mass: 22-26 parts of water-based epoxy resin, 3-5 parts of pigment, 1-1.3 parts of coupling agent, 6-10 parts of filler, 0.5-1 part of anti-flash rust agent, 0.4-0.6 part of leveling agent, 0.3-0.5 part of defoamer, 0.5-0.8 part of thickener, and 100-120 parts of deionized water; the component B comprises the following raw materials by mass: 75-80 parts of curing agent and 20-25 parts of deionized water.
[0008] By adopting the above technical scheme, waterborne epoxy resin: as the main component, provides the basic structure and curing performance of the paint film. Pigment: provides the color of the paint film and optimizes the appearance of the paint film. Coupling agent: enhances the adhesion between the filler and the resin, and improves the wear resistance and adhesion of the paint film. Filler: increases the thickness and impact strength of the paint film, while improving the rheological properties of the coating. Anti-flash rust agent: prevents the paint film from rusting in a humid environment. Leveling agent: improves the leveling of the paint film and reduces defects on the surface of the coating film. Defoaming agent: prevents bubbles from forming in the coating film. Thickener: adjusts the fluidity and viscosity of the paint film. Deionized water: used as a solvent and diluent to adjust the concentration and viscosity of component A. Curing agent: reacts with the waterborne epoxy resin in component A to cure the paint film. The synergistic effect between the components makes the waterborne epoxy insulating paint have excellent electrical insulation properties, adhesion, corrosion resistance and hardness. In addition, the paint has good storage stability, is not easy to sink to the bottom, has a simple production process, is easy to construct, and has low cost, and can meet the application needs of insulating paint in multiple fields.
[0009] Preferably, the preparation method of the water-based epoxy resin is as follows: according to the mass fractions, dehydrated ricinoleic acid, epoxy resin F-51 and tetraethylammonium bromide are added to a reaction bottle, nitrogen is passed through for 15-20 minutes, the temperature is raised to 80-85°C, the materials melt, and stirring is started; the temperature is continued to be raised to 220-225°C, and the temperature is maintained at 220-225°C to react until the acid value is 6 mgKOH / g, and then the temperature is lowered; when the temperature drops to 135-140°C, dipropylene glycol methyl ether and maleic anhydride are added, and the temperature is maintained at 135-140°C for reaction for 4-5 hours to obtain the water-based epoxy resin.
[0010] Preferably, the mass ratio of the dehydrated ricinoleic acid, epoxy resin F-51, tetraethylammonium bromide, dipropylene glycol methyl ether and maleic anhydride is 250:363:2.1:317:75.
[0011] By adopting the above technical scheme, the present application uses dehydrated castor oil acid and functional hydrophilic monomer maleic anhydride to modify epoxy resin at the same time to prepare water-based epoxy resin. Its preparation mechanism is as follows: dehydrated castor oil acid and epoxy resin are subjected to esterification reaction; after the acid value is qualified, dipropylene glycol methyl ether and maleic anhydride are added to continue the esterification reaction; after the acid value is qualified, a water-based epoxy resin is obtained. Dehydrated castor oil acid contains unsaturated carbon-carbon double bonds, which can be oxidatively cross-linked to improve the performance of the resin and is a natural cross-linking agent; at the same time, the long-chain non-polar fatty acid chain can make the coating have a good hydrophobic effect, and can give the coating good flexibility and flex resistance, which can improve the film-forming properties of the coating and improve the wettability to the substrate. Using dehydrated castor oil acid to modify waterborne epoxy resin can make waterborne epoxy resin have many excellent properties of epoxy resin and drying oil at the same time, which has a good promoting effect on improving the wettability of waterborne epoxy insulation paint and improving the bonding strength and flexibility of the paint film. The dehydrated castor oil acid of waterborne epoxy resin retains a large number of unsaturated double bonds, which improve the dryness and bonding strength of the paint film under the action of the drying agent; it has good storage stability; the functional hydrophilic monomer maleic anhydride is used to introduce carboxyl groups into the resin. These carboxyl groups have good water solubility, and only a small amount of addition is needed to make the resin have good water solubility. They can continue to dehydrate and condense during the high-temperature baking process of the subsequent insulation treatment, so that the resin can still maintain good electrical insulation performance and excellent salt spray resistance.
[0012] Preferably, the pigment is one of titanium dioxide, lithopone and toluidine red, and the titanium dioxide, lithopone and toluidine red are all modified by γ-aminopropyltriethoxysilane, and the mass of the γ-aminopropyltriethoxysilane is 1-1.5% of the mass of titanium dioxide, lithopone or toluidine red; the filler is composed of talcum powder and kaolin in a mass ratio of 1:3-5, and the talcum powder and kaolin are both modified by γ-aminopropyltriethoxysilane, and the mass of the γ-aminopropyltriethoxysilane is 1-1.5% of the total mass of the talcum powder and kaolin; the particle size of the kaolin is 5-10 microns, and the particle size of the talcum powder is 1-5 microns.
[0013] By adopting the above technical scheme, in the pigment, the modification of γ-aminopropyltriethoxysilane can improve the compatibility of the pigment with the waterborne epoxy resin and enhance the binding force between the pigment and the resin. This will improve the hardness and electrical insulation properties of the paint film. In the filler, talc and kaolin are composed in a mass fraction ratio of 1:3-5. They are also modified by γ-aminopropyltriethoxysilane, and the modified fillers have better compatibility and can improve the hardness and electrical insulation properties of the paint film. In addition, the particle size of kaolin is 5-10 microns, and the particle size of talc is 1-5 microns. The appropriate particle size of these fillers can improve the uniformity and smoothness of the paint film, while enhancing the scratch resistance of the coating film. In summary, by using pigments and fillers modified by γ-aminopropyltriethoxysilane, their compatibility with waterborne epoxy resin can be improved, and the hardness and electrical insulation properties of the paint film can be improved. At the same time, adjusting the particle size of pigments and fillers helps to improve the uniformity and scratch resistance of the paint film. A synergistic effect can be achieved through these methods to improve the performance of water-based epoxy insulating paint.
[0014] Preferably, the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltriethoxysilane and isocyanatemethyltriethoxysilane in a mass ratio of 3:(1-3):1.
[0015] By adopting the above technical scheme, γ-aminopropyltriethoxysilane has good hydrophilicity and bonding ability, which can enhance the bonding force between the paint film and the substrate and improve the adhesion. Vinyltriethoxysilane and isocyanatemethyltriethoxysilane have strong elasticity and flexibility, which can increase the toughness and impact resistance of the paint film. In summary, the composition of the coupling agent works synergistically with other ingredients to improve the adhesion, hardness, electrical insulation performance and impact resistance of water-based epoxy insulating paint.
[0016] Preferably, the curing agent is one or more of 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-phenylimidazole trimellitate and 2-phenyl-4-methyl-5-hydroxymethylimidazole.
[0017] Preferably, the anti-flash rust agent is one of ZT-708 and ZT-707 produced by Beijing Zhitu Chemical.
[0018] Preferably, the defoamer is one of the silicone defoamer BYK-018, the polyether defoamer BYK-019 and the polyether modified silicone defoamer TEGO-810; the leveling agent is one of the modified polyether leveling agent TEGO-450 and the modified silicone leveling agent BYK-306.
[0019] Preferably, the thickener is composed of a polyurethane thickener RM-8W from DOW and a hydrophobic fumed silica A-200 from Degussa in a mass ratio of 1:1.
[0020] By adopting the above technical solution, the role of the thickener is to increase the viscosity of the paint film, control the fluidity of the paint film, prevent the paint from flowing and dripping, and thus ensure uniform coating performance during construction. Polyurethane thickeners have efficient thickening ability, which can make the paint film have a higher viscosity, thereby increasing the thickness and weather resistance of the coating. Hydrophobic fumed silica can enhance the anti-settling performance of the paint film and increase the uniformity and smoothness of the coating. Through the combined use of polyurethane thickeners and hydrophobic fumed silica, the synergistic effect between them can improve the thickening effect and ensure the fluidity, construction performance and anti-settling performance of the coating.
[0021] In a second aspect, the present application provides a method for preparing a water-based epoxy insulating varnish, which adopts the following technical solution:
[0022] As a general technical concept, the present application also provides a method for preparing the above-mentioned water-based epoxy insulating paint, comprising the following steps: S101, preparation of component A: according to the mass fractions, respectively, water-based epoxy resin, pigment, coupling agent, filler, anti-flash rust agent, leveling agent, defoamer, thickener and deionized water are added to a stirring kettle, the speed is set to 1000rpm, stirred for 60-90min, and then sand-milled and dispersed until the slurry fineness is less than 20 microns, so as to obtain component A;
[0023] S102, preparation of component B: adding curing agent and deionized water into a stirring kettle according to the mass fraction, setting the speed to 300 rpm, stirring for 10-15 minutes, and obtaining component B;
[0024] S103, mixing the prepared A and B components in a mass ratio of 3-5:1 to obtain a water-based epoxy insulating paint.
[0025] In summary, the beneficial technical effects of this application are:
[0026] 1. Excellent electrical insulation properties: Water-based epoxy resin contains a large number of unsaturated double bonds, which can improve the dryness and bonding strength of the paint film, thus having excellent electrical insulation properties.
[0027] 2. Excellent adhesion: Coupling agent is added to water-based epoxy resin, which can improve the bonding strength between the coating and the substrate and enhance the adhesion.
[0028] 3. Outstanding anti-corrosion performance: Anti-flash rust agent is added to water-based epoxy resin, which can effectively prevent flash rust on the metal surface and improve the paint film's resistance to corrosive media.
[0029] 4. Excellent hardness: After modification, fillers and pigments can increase the hardness of the coating film and improve the wear resistance and scratch resistance of the coating.
[0030] 5. Good storage stability: Water-based epoxy insulating paint is not easy to sink to the bottom, can remain stable for a long time, and is easy to store and use.
[0031] 6. Simple production process and easy construction: The preparation of raw materials is simple, the production process is relatively easy, and the paint is easy to apply and has good leveling properties during construction. DETAILED DESCRIPTION
[0032] The implementation scheme of the present application will be described in detail below in conjunction with the examples, but those skilled in the art will understand that the following examples are only used to illustrate the present application and should not be considered to limit the scope of the present application. If the specific conditions are not specified in the examples, they are carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially. The silicone defoamer BYK-018, polyether defoamer BYK-019 and modified silicone leveling agent BYK-306 are all produced by BYK in Germany, and ZT-708 and ZT-707 are produced by Beijing Zhitu Chemical Company.
[0033] Preparation Example 1 Preparation of waterborne epoxy resin
[0034] The preparation method of the water-based epoxy resin is as follows: according to the mass fractions, 25 kg of dehydrated ricinoleic acid, 36.3 kg of epoxy resin F-51 and 0.21 kg of tetraethylammonium bromide are added to a reaction bottle, and after nitrogen is passed for 15 minutes, the temperature is raised to 80°C, the materials melt, and stirring is started; the temperature is continued to be raised to 220°C, and the temperature is maintained at 220°C to react until the acid value is 6 mgKOH / g, and then the temperature is lowered; when the temperature drops to 135°C, 31.7 kg of dipropylene glycol methyl ether and 7.5 kg of maleic anhydride are added, and the temperature is maintained at 135°C for reaction for 4 hours to obtain the water-based epoxy resin.
[0035] Preparation Example 2 Preparation of waterborne epoxy resin
[0036] The preparation method of the water-based epoxy resin is as follows: according to the mass fractions, 25 kg of dehydrated ricinoleic acid, 36.3 kg of epoxy resin F-51 and 0.21 kg of tetraethylammonium bromide are added to a reaction bottle, and after nitrogen is passed for 20 minutes, the temperature is raised to 85°C, the materials melt, and stirring is started; the temperature is continued to be raised to 225°C, and the temperature is maintained at 225°C to react until the acid value is 6 mgKOH / g, and then the temperature is lowered; when the temperature drops to 140°C, 31.7 kg of dipropylene glycol methyl ether and 7.5 kg of maleic anhydride are added, and the temperature is maintained at 140°C for reaction for 5 hours to obtain the water-based epoxy resin.
[0037] Preparation Example 3 Preparation of waterborne epoxy resin
[0038] The preparation method of the water-based epoxy resin is as follows: according to the mass fractions, 25 kg of dehydrated ricinoleic acid, 36.3 kg of epoxy resin F-51 and 0.21 kg of tetraethylammonium bromide are added to a reaction bottle, and after nitrogen is passed for 18 minutes, the temperature begins to rise to 82°C, the materials melt, and stirring begins; the temperature is continued to rise to 223°C, and the temperature is maintained at 223°C to react until the acid value is 6 mgKOH / g, and then the temperature is lowered; when the temperature drops to 138°C, 31.7 kg of dipropylene glycol methyl ether and 7.5 kg of maleic anhydride are added, and the temperature is maintained at 138°C for reaction for 4.6 hours to obtain the water-based epoxy resin.
[0039] Example 1
[0040] A water-based epoxy insulating varnish comprises a component A and a component B, wherein the mass ratio of the component A to the component B is 3:1; the component A comprises the following raw materials by mass: 22 kg of water-based epoxy resin, 3 kg of pigment, 1 kg of coupling agent, 6 kg of filler, 0.5 kg of anti-flash rust agent ZT-708, 0.4 kg of modified polyether leveling agent TEGO-450, 0.3 kg of silicone defoamer BYK-018, 0.5 kg of thickener, and 100 kg of deionized water; the component B comprises the following raw materials by mass: 75 kg of 1-benzyl-2-methylimidazole and 25 kg of deionized water. The pigment is titanium dioxide and is modified by γ-aminopropyltriethoxysilane, the mass of which is 1% of the mass of titanium dioxide; the filler is composed of talc and kaolin in a mass ratio of 1:3, the talc and kaolin are both modified by γ-aminopropyltriethoxysilane, the mass of which is 1% of the total mass of talc and kaolin; the particle size of the kaolin is 5-10 microns, the particle size of the talc is 1-5 microns, the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltriethoxysilane and isocyanatemethyltriethoxysilane in a mass ratio of 3:1:1, the thickener is composed of a polyurethane thickener RM-8W from DOW and a hydrophobic fumed silica A-200 from Degussa in a mass ratio of 1:1, and the water-based epoxy resin is the water-based epoxy resin prepared in Preparation Example 1.
[0041] The above-mentioned method for preparing a water-based epoxy insulating varnish comprises the following steps:
[0042] S101, preparation of component A: according to the mass fractions, respectively, water-based epoxy resin, pigment, coupling agent, filler, anti-flash rust agent ZT-708, modified polyether leveling agent Digao TEGO-450, silicone defoamer BYK-018, thickener and deionized water are added to a stirring kettle, the speed is set to 1000 rpm, stirred for 60 minutes, and then sand-milled and dispersed until the slurry fineness is less than 20 microns, to obtain component A;
[0043] S102, preparation of component B: add 1-benzyl-2-methylimidazole and deionized water into a stirring kettle according to their weight fractions, set the speed to 300 rpm, and stir for 10 minutes to obtain component B;
[0044] S103. Evenly mix the prepared components A and B in a mass ratio of 3:1 to obtain a water-based epoxy insulating paint.
[0045] Example 2
[0046] A water-based epoxy insulating varnish comprises a component A and a component B, wherein the mass ratio of the component A to the component B is 5:1; the component A comprises the following raw materials by mass: 26 kg of water-based epoxy resin, 5 kg of pigment, 1.3 kg of coupling agent, 10 kg of filler, 1 kg of anti-flash rust agent ZT-707, 0.6 kg of modified silicone leveling agent BYK-306, 0.5 kg of polyether defoamer BYK-019, 0.8 kg of thickener, and 120 kg of deionized water; the component B comprises the following raw materials by mass: 80 kg of 1-cyanoethyl-2-phenylimidazole trimellitate and 20 kg of deionized water. The pigment is lithopone and is modified by γ-aminopropyltriethoxysilane, the mass of which is 1.5% of the mass of lithopone; the filler is composed of talcum powder and kaolin in a mass ratio of 1:5, the talcum powder and kaolin are both modified by γ-aminopropyltriethoxysilane, the mass of which is 1.5% of the total mass of talcum powder and kaolin; the particle size of the kaolin is 5-10 microns, the particle size of the talcum powder is 1-5 microns, the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltriethoxysilane and isocyanatemethyltriethoxysilane in a mass ratio of 3:3:1, the thickener is composed of a polyurethane thickener RM-8W from DOW and a hydrophobic fumed silica A-200 from Degussa in a mass ratio of 1:1, and the water-based epoxy resin is the water-based epoxy resin prepared in Preparation Example 2.
[0047] The above-mentioned method for preparing a water-based epoxy insulating varnish comprises the following steps:
[0048] S101, preparation of component A: according to the mass fractions, respectively, water-based epoxy resin, pigment, coupling agent, filler, anti-flash rust agent ZT-707, modified silicone leveling agent BYK-306, polyether defoamer BYK-019, thickener and deionized water are added to a stirring kettle, the speed is set to 1000 rpm, stirred for 90 minutes, and then sand-milled to disperse the slurry to a fineness of less than 20 microns, to obtain component A;
[0049] S102, preparation of component B: according to the mass fractions, 1-cyanoethyl-2-phenylimidazole trimellitate and deionized water are added into a stirring kettle, the speed is set to 300 rpm, and the stirring is carried out for 15 minutes to obtain component B;
[0050] S103. Evenly mix the prepared components A and B in a mass ratio of 5:1 to obtain a water-based epoxy insulating varnish.
[0051] Example 3
[0052] A water-based epoxy insulating varnish comprises a component A and a component B, wherein the mass ratio of the component A to the component B is 4:1; the component A comprises the following raw materials, by mass: 24 kg of water-based epoxy resin, 4 kg of pigment, 1.2 kg of coupling agent, 8 kg of filler, 0.7 kg of anti-flash rust agent ZT-708, 0.5 kg of modified polyether leveling agent TEGO-450, 0.4 kg of polyether modified silicon defoamer TEGO-810, 0.6 kg of thickener, and 110 kg of deionized water; the component B comprises the following raw materials, by mass: 78 kg of 2-phenyl-4-methyl-5-hydroxymethylimidazole and 22 kg of deionized water. The pigment is toluidine red and is modified by γ-aminopropyltriethoxysilane, the mass of which is 1.2% of the mass of toluidine red; the filler is composed of talc and kaolin in a mass ratio of 1:4, the talc and kaolin are both modified by γ-aminopropyltriethoxysilane, the mass of which is 1.2% of the total mass of talc and kaolin; the particle size of the kaolin is 5-10 microns, the particle size of the talc is 1-5 microns, the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltriethoxysilane and isocyanatemethyltriethoxysilane in a mass ratio of 3:2:1, the thickener is composed of a polyurethane thickener RM-8W from DOW and a hydrophobic fumed silica A-200 from Degussa in a mass ratio of 1:1, and the water-based epoxy resin is the water-based epoxy resin prepared in Preparation Example 3.
[0053] The above-mentioned method for preparing a water-based epoxy insulating varnish comprises the following steps:
[0054] S101, preparation of component A: according to the mass fractions, respectively, water-based epoxy resin, pigment, coupling agent, filler, anti-flash rust agent ZT-708, modified polyether leveling agent TEGO-450, polyether modified silicon defoamer TEGO-810, thickener and deionized water are added to a stirring kettle, the speed is set to 1000 rpm, stirred for 70 minutes, and then dispersed by sand grinding until the slurry fineness is less than 20 microns, to obtain component A;
[0055] S102, preparation of component B: add 2-phenyl-4-methyl-5-hydroxymethylimidazole and deionized water into a stirring kettle according to their weight fractions, set the speed to 300 rpm, and stir for 13 minutes to obtain component B;
[0056] S103. Evenly mix the prepared components A and B in a mass ratio of 4:1 to obtain a water-based epoxy insulating varnish.
[0057] Example 4
[0058] The same as Example 3, except that an equal amount of γ-aminopropyltriethoxysilane is used instead of the coupling agent, and the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltriethoxysilane and isocyanatemethyltriethoxysilane in a mass ratio of 3:2:1.
[0059] Example 5
[0060] The same as Example 3, except that an equal amount of vinyl triethoxysilane is used instead of the coupling agent, and the coupling agent is composed of γ-aminopropyl triethoxysilane, vinyl triethoxysilane and isocyanate methyl triethoxysilane in a mass ratio of 3:2:1.
[0061] Example 6
[0062] The same as Example 3, except that an equal amount of isocyanate methyl triethoxy silane is used instead of the coupling agent, and the coupling agent is composed of γ-aminopropyl triethoxy silane, vinyl triethoxy silane and isocyanate methyl triethoxy silane in a mass ratio of 3:2:1.
[0063] Example 7
[0064] The same as Example 3, except that an equal amount of polyurethane thickener RM-8W of DOW Company is used instead of the thickener, and the thickener is composed of polyurethane thickener RM-8W of DOW Company and hydrophobic fumed silica A-200 of Degussa in a mass ratio of 1:1.
[0065] Example 8
[0066] The same as Example 3, except that an equal amount of Degussa's hydrophobic fumed silica A-200 is used to replace the thickener, and the thickener is composed of a polyurethane thickener RM-8W from DOW and Degussa's hydrophobic fumed silica A-200 in a mass ratio of 1:1.
[0067] Comparative Example 1
[0068] The same as Example 3, except that an equal amount of bisphenol A epoxy resin E-44 is used to replace the water-based epoxy resin prepared in Preparation Example 3 of the present application.
[0069] Comparative Example 2
[0070] The same as Example 3, except that an equal amount of talc (the particle size of the talc is 1-5 microns) is used instead of the filler composed of talc and kaolin in a mass ratio of 1:4, and the talc and kaolin are both modified by γ-aminopropyltriethoxysilane, and the mass of the γ-aminopropyltriethoxysilane is 1.2% of the total mass of the talc and kaolin; the particle size of the kaolin is 5-10 microns, and the particle size of the talc is 1-5 microns.
[0071] Comparative Example 3
[0072] The same as Example 3, except that an equal amount of kaolin (the particle size of kaolin is 5-10 microns) is used instead of the filler consisting of talc and kaolin in a mass ratio of 1:4, and the talc and kaolin are both modified by γ-aminopropyltriethoxysilane, and the mass of the γ-aminopropyltriethoxysilane is 1.2% of the total mass of the talc and kaolin; the particle size of the kaolin is 5-10 microns, and the particle size of the talc is 1-5 microns.
[0073] Performance Testing
[0074] 132 copper sheets with a size of 10cm×10cm×0.2cm were divided into 11 groups, with 12 sheets in each group, and immersed in the water-based epoxy insulating paint spray prepared in Example 1-Example 8 and Comparative Example 1-Comparative Example 3 for 30 seconds. The copper sheets were taken out and cured at 100°C for 2 hours to obtain a coating with a thickness controlled at 4060 microns. After aging for 7 days, the coating was tested. The test results are shown in Table 1.
[0075] Pencil hardness: tested according to GB / T 6739-2006 standard;
[0076] Adhesion test: Tested according to GB / T9286-1998 standard;
[0077] Storage stability: tested according to GB / T6735-1986 standard;
[0078] 5% H2SO4 resistance test: Tested according to GB / T9274 standard;
[0079] Breakdown strength: tested according to GB / T1981.2-2009 standard.
[0080] Table 1 Performance test
[0081]
[0082] As can be seen from Table 1, the water-based epoxy insulating varnishes prepared in Examples 1 to 3 have good hardness, excellent adhesion, excellent corrosion resistance and excellent electrical insulation performance, and at the same time have the advantages of stable storage, simple construction and low cost, and can meet the application requirements of insulating varnishes in the fields of automobiles, home appliances, industrial control, medical consumables, etc.
[0083] As can be seen from Table 1, the performance comparison analysis of the water-based epoxy insulating varnishes prepared in Example 3 and Example 4-Example 6 shows that the coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltriethoxysilane and isocyanatemethyltriethoxysilane in a mass ratio of 3:2:1. The synergistic effect between them can improve the comprehensive performance of the water-based epoxy insulating varnish.
[0084] As can be seen from Table 1, the performance comparison analysis of the water-based epoxy insulating varnishes prepared in Example 3 and Example 7-Example 8 uses a thickener composed of a polyurethane thickener RM-8W from DOW and a hydrophobic fumed silica A-200 from Degussa in a mass ratio of 1:1. The synergistic effect between them can improve the storage stability of the water-based epoxy insulating varnish.
[0085] As can be seen from Table 1, the performance comparison analysis of the water-based epoxy insulating varnish prepared in Example 3 and Comparative Example 1 shows that the water-based epoxy resin prepared in Preparation Example 3 retains a large number of unsaturated double bonds on the dehydrated ricinoleic acid in the water-based epoxy resin, and these unsaturated double bonds improve the dryness and bonding strength of the paint film under the action of the drying agent; it has good storage stability; the functional hydrophilic monomer maleic anhydride is used to introduce carboxyl groups into the resin, and these carboxyl groups have good water solubility, and only a small amount of addition is needed to make the resin have good water solubility. They can continue to dehydrate and condense during the high-temperature baking process of the subsequent insulation treatment, so that the resin can still maintain good electrical insulation performance and excellent salt spray resistance.
[0086] As can be seen from Table 1, the performance comparison analysis of the water-based epoxy insulating paints prepared in Example 3 and Comparative Examples 2-3 adopts a compound of talc powder and kaolin modified with γ-aminopropyltriethoxysilane, and utilizes the synergistic effect between them to improve the comprehensive performance of the water-based epoxy insulating paint.
[0087] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.
Claims
1. A water-based epoxy insulating varnish, characterized in that: The invention comprises component A and component B, wherein the mass ratio of component A to component B is 3-5:1; the component A comprises the following raw materials by mass: 22-26 parts of waterborne epoxy resin, 3-5 parts of pigment, 1-1.3 parts of coupling agent, 6-10 parts of filler, 0.5-1 parts of anti-flash rust agent, 0.4-0.6 parts of leveling agent, 0.3-0.5 parts of defoamer, 0.5-0.8 parts of thickener, and 100-120 parts of deionized water; the component B comprises the following raw materials by mass: 75-80 parts of curing agent and 20-25 parts of deionized water; The pigment is one of titanium dioxide, lithopone and toluidine red, and the titanium dioxide, lithopone and toluidine red are all modified by γ-aminopropyl triethoxysilane, and the mass of the γ-aminopropyl triethoxysilane is 1-1.5% of the mass of titanium dioxide, lithopone or toluidine red; the filler is composed of talcum powder and kaolin in a mass ratio of 1:3-5, and the talcum powder and kaolin are all modified by γ-aminopropyl triethoxysilane, and the mass of the γ-aminopropyl triethoxysilane is 1-1.5% of the total mass of the talcum powder and kaolin; the particle size of the kaolin is 5-10 microns, and the particle size of the talcum powder is 1-5 microns; The coupling agent is composed of γ-aminopropyltriethoxysilane, vinyltriethoxysilane and isocyanatemethyltriethoxysilane in a mass ratio of 3:(1-3):1; The thickener is composed of a polyurethane thickener RM-8W from DOW and a hydrophobic fumed silica A-200 from Degussa in a mass ratio of 1:1; The preparation method of the waterborne epoxy resin is as follows: according to the mass fractions, dehydrated ricinoleic acid, epoxy resin F-51 and tetraethylammonium bromide are added into a reaction bottle, nitrogen is passed through for 15-20 minutes, the temperature is raised to 80-85°C, the materials are melted, and stirring is started; the temperature is further raised to 220-225°C, and the temperature is maintained at 220-225°C to react until the acid value is 6mgKOH / g, and then the temperature is lowered; when the temperature drops to 135-140°C, dipropylene glycol methyl ether and maleic anhydride are added, and the temperature is maintained at 135-140°C for reaction for 4-5 hours, so as to obtain the waterborne epoxy resin; the mass fraction ratio of the dehydrated ricinoleic acid, epoxy resin F-51, tetraethylammonium bromide, dipropylene glycol methyl ether and maleic anhydride is 250:363:2.1:317:
75.
2. A water-based epoxy insulating varnish according to claim 1, characterized in that: The curing agent is one or more of 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-phenylimidazole trimellitate and 2-phenyl-4-methyl-5-hydroxymethylimidazole.
3. A water-based epoxy insulating varnish according to claim 1, characterized in that: The anti-flash rust agent is one of ZT-708 and ZT-707 produced by Beijing Zhitu Chemical.
4. A water-based epoxy insulating varnish according to claim 1, characterized in that: The defoamer is one of the silicone defoamer BYK-018, the polyether defoamer BYK-019 and the polyether modified silicone defoamer TEGO-810; the leveling agent is one of the modified polyether leveling agent TEGO-450 and the modified silicone leveling agent BYK-306.
5. A method for preparing a water-based epoxy insulating varnish according to any one of claims 1 to 4, characterized in that: The following steps are involved: S101, preparation of component A: according to the mass fractions, respectively, water-based epoxy resin, pigment, coupling agent, filler, anti-flash rust agent, leveling agent, defoamer, thickener and deionized water are placed in a stirring kettle, the speed is set to 1000 rpm, stirred for 60-90 minutes, and then sand-milled and dispersed until the slurry fineness is less than 20 microns, to obtain component A; S102, preparation of component B: adding curing agent and deionized water into a stirring kettle according to the mass fraction, setting the speed to 300 rpm, stirring for 10-15 minutes, and obtaining component B; S103. Evenly mix the prepared A and B components in a mass ratio of 3-5:1 to obtain a water-based epoxy insulating paint.