A production process for high-strength corrugated base paper recycled from waste paper

Through the waste paper recycling and regeneration process, the fibers are treated with biological enzymes and surfactants, and combined with composite additives to form a dense glue application, which solves the problem of the strength of corrugated base paper decreasing in high humidity environments, improves water resistance and mechanical strength, and ensures the Packaging stability and reduce resource consumption.

CN118345647BActive Publication Date: 2024-11-15SHANDONG PANGTUAN PAPER PROD CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410623436.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-20
Publication Date
2024-11-15
Estimated Expiration
2044-05-20

AI Technical Summary

Technical Problem

The strength of existing corrugated base paper decreases in high humidity environments and is prone to moisture, which affects the stability and load-bearing capacity of packaging, and the production process causes losses to natural resources and affects the ecological environment.

Method used

The waste paper recycling and regeneration high-strength corrugated base paper production process is adopted, and modified fibers are treated by biological enzymes, combined with surfactants and composite additives for ultrasonic treatment to form dense surface glue-sizing chemicals, enhancing the water resistance and mechanical strength of the paper.

Benefits of technology

It significantly improves the strength and water resistance of corrugated base paper under high humidity conditions, reduces the risk of softening and expansion caused by water absorption, ensures the safety and integrity of packaging items, and reduces resource consumption and environmental impact.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of recycled waste paper processing, and specifically relates to a production process for high-strength corrugated paper recycled from waste paper. The specific preparation process is as follows: S1, remove impurities from recycled waste paper, soak, pulp, and enzymolysis to obtain pretreated pulp; S2, add a surfactant to the pretreated pulp obtained in step S1, perform an ultrasonic treatment once, then add a composite auxiliary agent, and perform a second ultrasonic treatment; S3, remove slag from the pulp obtained in step S2 through a slag remover, then dilute with water, sheet form, press, and pre-dry; S4, double-side sizing the pre-dried corrugated paper obtained in step S3 with surface sizing chemicals, and dry to obtain. The process provided by the present invention effectively improves the strength and water resistance of corrugated paper under high humidity conditions, ensures that the carton can still maintain the stability of the structure in a high humidity environment, greatly reduces the risk of softening, swelling, and even rupture due to water absorption, and ensures the safety and integrity of the packaged items.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of recycled waste paper processing, and specifically relates to a production process for recycling high-strength corrugated base paper from waste paper. Background Art

[0002] Corrugated paper is an important part of corrugated board production. It is a specially designed and processed paper used to form the wavy core layer in the corrugated board structure. Corrugated paper has good fiber bonding strength, flatness, tightness and stiffness, as well as a certain elasticity, ensuring that the corrugated box has good shock and pressure resistance. Its main ingredients include wood pulp, waste paper pulp or other fiber raw materials, and chemical additives such as wet strength agent, retention aid, softener, etc. are added to optimize performance.

[0003] Corrugated paper is mainly used to produce various types of corrugated board, which can be used in food packaging, retail packaging, shockproof packaging and other fields after printing, cutting and other subsequent processing. Due to its excellent structural properties, corrugated paper plays an important role in the packaging industry, especially in the fields of food and beverage, daily chemical products, electronic products, etc.

[0004] However, although the existing corrugated paper has a certain strength, it may still be insufficient in some heavy packaging applications. It is also susceptible to moisture in the natural environment, which affects its strength. In a high humidity environment or long-term immersion, its strength will drop significantly, seriously affecting the stability and load-bearing capacity of the packaging. Traditional corrugated paper production relies on a large amount of wood and water resources, and wastewater and waste are generated during the production process, which will cause a great loss of natural resources and have a profound adverse impact on the ecological environment.

[0005] Therefore, it is necessary to provide a method for preparing corrugated paper with high strength and low water absorption by using waste paper. Summary of the invention

[0006] In order to solve the problems existing in the prior art, the purpose of the present invention is to provide a production process for high-strength corrugated paper recycled from waste paper. The process provided by the present invention effectively improves the strength and water resistance of corrugated paper under high humidity conditions, ensures that the carton can still maintain structural stability in a high humidity environment, greatly reduces the risk of softening, swelling and even rupture caused by water absorption, and ensures the safety and integrity of the packaged items.

[0007] The technical solution of the present invention is:

[0008] A production process for recycling high-strength corrugated paper from waste paper, comprising the following preparation steps:

[0009] S1. After removing impurities from the recycled waste paper, soak it in water, adjust the pulp concentration and process it with a high-concentration hydraulic pulper, then add biological enzymes, adjust the pH and perform enzymolysis to obtain pretreated pulp;

[0010] S2, adding a surfactant to the pretreated slurry obtained in step S1, performing an ultrasonic treatment once, then adding a composite auxiliary agent, stirring evenly, and performing a second ultrasonic treatment;

[0011] S3, the pulp obtained in step S2 is removed by a remover, then diluted with water, formed into sheets, pressed, and pre-dried to obtain pre-dried corrugated paper;

[0012] S4, applying sizing chemicals on both sides of the pre-dried corrugated paper obtained in step S3, and drying the paper.

[0013] Furthermore, the recycled waste paper in step S1 is domestic waste boxboard.

[0014] Furthermore, the surface sizing chemicals in step S4 are composed of the following components and their weight proportions: 25-35 parts of grafted butyl acrylate starch, 7-10 parts of guar gum, 3-5 parts of nano calcium carbonate, 8-10 parts of polyvinyl alcohol, and 150-200 parts of water.

[0015] Furthermore, the preparation method of the grafted butyl acrylate starch comprises the following steps:

[0016] Add 4 to 6 times the mass of distilled water to corn starch and mix evenly, heat to 85 to 95° C., and continue stirring until the starch paste is completely dissolved to form a uniform starch paste; add butyl acrylate, ammonium persulfate and N,N-dimethylformamide to the starch paste and mix well; then place the mixture in a constant temperature water bath, react for 4 to 6 hours at a temperature of 60 to 70° C. and a stirring speed of 80 to 100 r / min; after the reaction is completed, wash the product with deionized water, then centrifuge and dry to obtain the product.

[0017] Furthermore, the amount of butyl acrylate used is 22-26% of the mass of corn starch, the amount of ammonium persulfate added is 1.2-1.6% of the mass of corn starch, and the amount of N,N-dimethylformamide added is 7-12% of the mass of corn starch.

[0018] Furthermore, the amount of butyl acrylate used is 24% of the mass of corn starch, the amount of ammonium persulfate added is 1.5% of the mass of corn starch, and the amount of N,N-dimethylformamide added is 10% of the mass of corn starch.

[0019] Furthermore, in the step S1, the waste paper after impurities removal is soaked in water for 5 to 8 hours, the pulp concentration is adjusted to 10 to 15%, and the processing time in the high-consistency hydraulic pulper is 20 to 30 minutes.

[0020] Furthermore, the biological enzyme in step S1 is a combination of cellulase, xylanase and α-amylase; the biological enzyme is composed of cellulase, xylanase and α-amylase in a weight ratio of 1:1:2-3.

[0021] Furthermore, the amount of the biological enzyme added in step S1 is 0.2-0.3% of the absolute dry weight of the pulp, the enzymolysis temperature is 42-50° C., the enzymolysis time is 4-6 hours, the pH is adjusted to 6.5-7.5, and the stirring speed during the enzymolysis process is 200-300 r / min.

[0022] Furthermore, the amount of surfactant added in step S2 is 0.3-0.7% of the weight of the pretreated pulp obtained in step S1; the surfactant is composed of sodium xylene sulfonate and 1,3-propylene glycol in a weight ratio of 2-4:1.

[0023] Furthermore, the amount of surfactant added in step S2 is 0.5% of the weight of the pretreated pulp obtained in step S1; the surfactant is composed of sodium xylene sulfonate and 1,3-propylene glycol in a weight ratio of 3:1.

[0024] Furthermore, the composite auxiliary agent in step S2 is a combination of two or more of polyacrylamide, polyethyleneimine, alkyl ketene dimer, carboxymethyl starch, and carboxymethyl cellulose; the added amount of the composite auxiliary agent is 0.3-0.5% of the weight of the pretreated pulp in step S1.

[0025] Furthermore, in step S2, the frequency of the first ultrasonic treatment is 60-80 kHz, and the ultrasonic time is 20-30 min. The frequency of the second ultrasonic treatment is 30-50 kHz, and the ultrasonic time is 30-40 min.

[0026] Furthermore, the preparation method of the surface sizing chemical in step S4 comprises the following preparation steps:

[0027] Dissolve the grafted butyl acrylate starch in water, stir evenly, then add polyvinyl alcohol, guar gum and nano calcium carbonate while stirring, stir for 1 to 2 hours, and then leave for 2 to 3 hours to obtain the product.

[0028] Furthermore, in step S3, the pulp after deslagging is diluted to a pulp concentration of 0.8-1.5%; the sizing amount in step S4 is 8 g / m 2The drying temperature is 105-110℃, the moisture content of the corrugated paper after drying is 7.5wt%, and the basis weight is 110-165g / m 2 .

[0029] The corrugated paper prepared by the preparation process of the present invention has strong adaptability to high humidity environment, fundamentally overcoming the difficulties encountered in the traditional production process. Faced with the high temperature and high humidity conditions in summer, the strength performance of high-strength corrugated paper decreases and the water resistance weakens. The preparation process of high-strength corrugated paper of the present invention adopts a reasonable ratio of different raw materials. First, a specific composite biological enzyme is used to enzymolyze the recycled waste paper in the pulping process, and the fiber is appropriately modified, which can promote the separation of ink particles and fiber decomposition between fibers, improve the swelling of fibers, increase the swelling degree and interweaving degree of fibers, and promote the effective combination of surface sizing chemicals and fibers in subsequent steps, thereby strengthening the water resistance and mechanical strength of paper at the molecular level.

[0030] Furthermore, a surfactant composed of sodium xylene sulfonate and 1,3-propylene glycol in a weight ratio of 2 to 4:1 is added to the pretreated pulp after enzymatic hydrolysis, and an ultrasonic treatment is performed once, and then a composite additive is added for a second ultrasonic treatment. By combining the synergistic effect of the surfactant and the composite additive (two or more of polyacrylamide, polyethyleneimine, alkyl ketene dimer, carboxymethyl starch, and carboxymethyl cellulose), and using a segmented ultrasonic treatment process for treatment, the fiber and the composite additive can be dispersed more evenly in the water, reducing flocculation, thereby improving the uniformity and fluidity of the pulp. At the same time, it can also reduce the loss of fibers, improve the strength and uniformity of paper, thereby improving the uniformity of subsequent sizing and coating operations, and by adjusting the surface tension of the pulp, the surface sizing chemicals can be more evenly distributed on the paper sheet.

[0031] Finally, the present invention adopts the prepared specific surface sizing chemicals, which can form a dense protective layer on the surface of paper, effectively prevent moisture penetration, enhance the moisture and liquid resistance of paperboard, and significantly reduce the hygroscopic expansion of corrugated paper even in a high humidity environment, maintain the structural stability and strength of the carton, and effectively improve the ring crush strength of corrugated paper.

[0032] Compared with the prior art, the production process of high-strength corrugated paper recycled from waste paper provided by the present invention has the following advantages:

[0033] The present invention provides a production process for high-strength corrugated base paper recycled from waste paper. By adopting a reasonable ratio of different raw materials, high-efficiency wet-end chemicals, surface sizing chemicals, bio-enzyme products, etc. are combined and applied to the production of high-strength corrugated base paper. Through efficient synergistic effect, the strength and water resistance of the corrugated base paper under high humidity conditions are effectively improved, and the problem of high-strength corrugated base paper strength reduction and poor water resistance in high-temperature and high-humidity environments, which has troubled high-strength corrugated base paper manufacturers and carton manufacturers for many years, is solved. The problem that the high-strength corrugated base paper has a reduced strength and poor water resistance due to high temperature and high humidity environments, resulting in the rupture or collapse of packaging boxes, is solved. DETAILED DESCRIPTION

[0034] The present invention is further illustrated below through the description of specific implementation methods, but this is not a limitation of the present invention. Those skilled in the art can make various modifications or improvements based on the basic idea of ​​the present invention, but as long as they do not deviate from the basic idea of ​​the present invention, they are all within the protection scope of the present invention.

[0035] In the following examples and comparative examples, reagents not otherwise specified are conventional reagents and can be purchased from conventional reagent production and sales companies. The methods used, unless otherwise specified, are all existing technologies. Information on some raw material manufacturers is as follows:

[0036] Cellulase, CAS No.: 9012-54-8, Product No.: S10041; xylanase, CAS No.: 9025-57-4, Product No.: S10108; α-amylase, CAS No.: 9025-57-4, Product No.: S10108; polyacrylamide (PAM), CAS No.: 9003-05-8, Product No.: S31321; carboxymethyl cellulose, CAS No.: 9000-11-7, Product No.: S14019, guar gum, CAS No.: 9000-30-0, Product No.: S30550, were purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0037] Polyethyleneimine, CAS No.: 9002-98-6, was purchased from Shandong Haizhou Bioengineering Co., Ltd.;

[0038] Alkyl ketene dimer (AKD), CAS No.: 144245-85-2, purchased from Hubei Xinmingtai Chemical Co., Ltd.;

[0039] Carboxymethyl starch, CAS number: 9057-06-1, purchased from Zhengzhou Longsheng Chemical Products Co., Ltd.;

[0040] Polyvinyl alcohol, CAS No.: 9002-89-5, purchased from Shandong Xinheng Chemical Co., Ltd.;

[0041] Nano calcium carbonate, CAS number: 471-34-1, purchased from Shanghai Myrel Biochemical Technology Co., Ltd., catalog number M81760;

[0042] Acrylic acid grafted starch was purchased from Hubei Maidehao Chemical Co., Ltd.

[0043] Example 1

[0044] A production process for recycling high-strength corrugated paper from waste paper, comprising the following preparation steps:

[0045] S1. After removing impurities from 2 kg of domestic waste boxboard, soak it in water for 5 hours, adjust the pulp concentration to 10%, and then treat it with a high-concentration hydraulic pulper for 20 minutes, then add a biological enzyme composed of cellulase, xylanase and α-amylase in a weight ratio of 1:1:2, and the addition amount of the biological enzyme is 0.2% of the absolute dry weight of the pulp, adjust the pH to 6.5, and perform enzymolysis for 6 hours at a temperature of 42° C. and a stirring speed of 200 r / min to obtain a pretreated pulp;

[0046] S2. Add a surfactant composed of sodium xylene sulfonate and 1,3-propylene glycol in a weight ratio of 2:1 to the pretreated pulp obtained in step S1 (the amount of the surfactant added is 0.3% of the weight of the pretreated pulp obtained in step S1), perform an ultrasonic treatment, the frequency of the ultrasonic treatment is 60 kHz, and the ultrasonic time is 30 min. Then, add a composite auxiliary agent composed of polyacrylamide and alkyl ketene dimer in a weight ratio of 1:3 (the amount of the composite auxiliary agent added is 0.3% of the weight of the pretreated pulp obtained in step S1), stir evenly, and perform a second ultrasonic treatment; the frequency of the second ultrasonic treatment is 30 kHz, and the ultrasonic time is 40 min.

[0047] S3, the pulp obtained in step S2 is removed by a remover, and then diluted with water to a pulp concentration of 0.8%, formed into sheets, pressed, and dried to a moisture content of ≤10wt%, to obtain pre-dried corrugated paper;

[0048] S4, using surface sizing chemicals to double-side gluing the pre-dried corrugated paper obtained in step S3, with a gluing amount of 8g / m 2 , dried to a moisture content of 7.5wt%, quantitative 130g / m 2 You can get it.

[0049] The preparation method of the surface sizing chemical in step S4 comprises the following steps: dissolving 25g of grafted butyl acrylate starch in 150g of water, stirring evenly, then adding 8g of polyvinyl alcohol, 7g of guar gum and 3g of nano calcium carbonate while stirring, stirring for 1h, and then standing for 2h to obtain the product.

[0050] The preparation method of the grafted butyl acrylate starch comprises the following steps:

[0051] Add 800 g of distilled water to 200 g of corn starch and mix evenly, heat to 85° C., and continue stirring until the starch paste is completely dissolved to form a uniform starch paste; add 44 g of butyl acrylate, 2.4 g of ammonium persulfate and 14 g of N,N-dimethylformamide to the starch paste and mix well; then place the mixture in a constant temperature water bath, react for 6 hours at a temperature of 60° C. and a stirring speed of 80 r / min; after the reaction is completed, wash the product with deionized water, then centrifuge and dry to obtain.

[0052] Example 2

[0053] A production process for recycling high-strength corrugated paper from waste paper, comprising the following preparation steps:

[0054] S1. After removing impurities from 2 kg of domestic waste boxboard, soak it in water for 6 hours, adjust the pulp concentration to 12%, and then treat it with a high-concentration hydraulic pulper for 25 minutes, then add a biological enzyme composed of cellulase, xylanase and α-amylase in a weight ratio of 1:1:2.5, and the addition amount of the biological enzyme is 0.25% of the absolute dry weight of the pulp, adjust the pH to 7.0, and perform enzymolysis for 5 hours at a temperature of 45°C and a stirring speed of 250 r / min to obtain a pretreated pulp;

[0055] S2. Add a surfactant composed of sodium xylene sulfonate and 1,3-propylene glycol in a weight ratio of 3:1 to the pretreated pulp obtained in step S1 (the amount of the surfactant added is 0.5% of the weight of the pretreated pulp in step S1), perform an ultrasonic treatment, the frequency of the ultrasonic treatment is 70kHz, and the ultrasonic time is 25min, then add a composite auxiliary agent composed of polyacrylamide, alkyl ketene dimer and carboxymethyl starch in a weight ratio of 1:2:1 (the amount of the composite auxiliary agent added is 0.4% of the weight of the pretreated pulp obtained in step S1), stir evenly, and perform a second ultrasonic treatment; the frequency of the second ultrasonic treatment is 40kHz, and the ultrasonic time is 35min;

[0056] S3, the pulp obtained in step S2 is removed by a remover, and then diluted with water to a pulp concentration of 1.2%, sheeted into shape, pressed, and dried to a moisture content of ≤10wt%, to obtain pre-dried corrugated base paper;

[0057] S4, using surface sizing chemicals to double-side gluing the pre-dried corrugated paper obtained in step S3, with a gluing amount of 8g / m 2 , dried to a moisture content of 7.5wt%, quantitative 140g / m 2 , you will get it.

[0058] The preparation method of the surface sizing chemical in step S4 comprises the following steps: dissolving 20 g of grafted butyl acrylate starch in 180 g of water, stirring evenly, then adding 9 g of polyvinyl alcohol, 8 g of guar gum and 4 g of nano calcium carbonate while stirring, stirring for 1.5 h, and then standing for 2.5 h to obtain the product.

[0059] The preparation method of the grafted butyl acrylate starch comprises the following steps:

[0060] Add 1000 g of distilled water to 200 g of corn starch and mix evenly, heat to 90° C., and continue stirring until the starch paste is completely dissolved to form a uniform starch paste; add 48 g of butyl acrylate, 3 g of ammonium persulfate and 20 g of N,N-dimethylformamide to the starch paste and mix well; then place the mixture in a constant temperature water bath, react for 5 hours at a temperature of 65° C. and a stirring speed of 90 r / min; after the reaction is completed, wash the product with deionized water, then centrifuge and dry to obtain.

[0061] Example 3

[0062] A production process for recycling high-strength corrugated paper from waste paper, comprising the following preparation steps:

[0063] S1. After removing impurities from 2 kg of domestic waste boxboard, soak it in water for 8 hours, adjust the pulp concentration to 15%, and then treat it with a high-concentration hydraulic pulper for 30 minutes, then add a biological enzyme composed of cellulase, xylanase and α-amylase in a weight ratio of 1:1:3, and the addition amount of the biological enzyme is 0.3% of the absolute dry weight of the pulp, adjust the pH to 7.5, and perform enzymolysis for 4 hours at a temperature of 50°C and a stirring speed of 300 r / min to obtain a pretreated pulp;

[0064] S2. Add a surfactant composed of sodium xylene sulfonate and 1,3-propylene glycol in a weight ratio of 4:1 to the pretreated pulp obtained in step S1 (the amount of the surfactant added is 0.7% of the weight of the pretreated pulp obtained in step S1), perform an ultrasonic treatment, the frequency of the ultrasonic treatment is 80 kHz, and the ultrasonic time is 20 min. Then, add a composite auxiliary agent composed of polyacrylamide, polyethyleneimine, alkyl ketene dimer, and carboxymethyl cellulose in a weight ratio of 1:1:1:1 (the amount of the composite auxiliary agent added is 0.5% of the weight of the pretreated pulp obtained in step S1), stir evenly, and perform a second ultrasonic treatment; the frequency of the second ultrasonic treatment is 50 kHz, and the ultrasonic time is 30 min.

[0065] S3, the pulp obtained in step S2 is removed by a remover, and then diluted with water to a pulp concentration of 1.5%, sheeted into shape, pressed, and dried to a moisture content of ≤10wt%, to obtain pre-dried corrugated paper;

[0066] S4, using surface sizing chemicals to double-side gluing the pre-dried corrugated paper obtained in step S3, with a gluing amount of 8g / m 2 , dried to a moisture content of 7.5wt%, quantitative 165g / m 2 , you will get it.

[0067] The preparation method of the surface sizing chemical in step S4 comprises the following steps: dissolving 35g of grafted butyl acrylate starch in 200g of water, stirring evenly, then adding 10g of polyvinyl alcohol, 10g of guar gum and 5g of nano calcium carbonate while stirring, stirring for 2h, and then standing for 3h to obtain the product.

[0068] The preparation method of the grafted butyl acrylate starch comprises the following steps:

[0069] Add 1200 g of distilled water to 200 g of corn starch and mix evenly, heat to 95° C., and continue stirring until the starch paste is completely dissolved to form a uniform starch paste; add 52 g of butyl acrylate, 3.2 g of ammonium persulfate and 24 g of N,N-dimethylformamide to the starch paste and mix well; then place the mixture in a constant temperature water bath, react for 4 hours at a temperature of 70° C. and a stirring speed of 100 r / min; after the reaction is completed, wash the product with deionized water, then centrifuge and dry to obtain.

[0070] Comparative Example 1

[0071] Compared with Example 2, the difference of Comparative Example 1 is that the xylene sulfonic acid in the surfactant of step S2 is replaced by sodium dodecylbenzene sulfonate, and the other production processes and parameters are the same as those of Example 2.

[0072] Comparative Example 2

[0073] Compared with Example 2, the difference of Comparative Example 2 is that only one ultrasonic treatment is performed in step S2. That is, the specific process of step S2 is: a surfactant composed of sodium xylene sulfonate and 1,3-propylene glycol in a weight ratio of 2:1 is added to the pretreated pulp obtained in step S1 (the amount of the surfactant added is 0.3% of the weight of the pretreated pulp in step S1), and then a composite auxiliary agent composed of polyacrylamide and alkyl ketene dimer in a weight ratio of 1:3 is added (the amount of the composite auxiliary agent added is 0.3% of the weight of the pretreated pulp obtained in step S1), stirred evenly, and ultrasonic treatment is performed, the ultrasonic frequency is 70kHz, and the ultrasonic time is 1h.

[0074] Other production processes and parameters are the same as those in Example 2.

[0075] Comparative Example 3

[0076] Compared with Example 2, the difference of Comparative Example 3 is that the grafted butyl acrylate starch in the surface sizing chemical of step S4 is replaced by commercially available acrylic acid grafted starch, and other production processes and parameters are the same as those of Example 2.

[0077] Comparative Example 4

[0078] Compared with Example 2, the difference of Comparative Example 4 is that guar gum is not added in step S4, the amount of grafted butyl acrylate starch is increased accordingly to 28 g, and other production processes and parameters are the same as those of Example 2.

[0079] Test Example 1: Performance test of corrugated paper prepared by the present invention

[0080] 1. Test object: corrugated paper prepared in Examples 1 to 3 and Comparative Examples 1 to 4 of the present invention.

[0081] 2. Test methods:

[0082] (1) The quantitative weight (g / m2) of the corrugated base paper prepared in Examples 1 to 3 and Comparative Examples 1 to 4 was measured according to the relevant method in GB 13023-1991 Corrugated Base Paper Standard. 2 ), lateral ring pressure index (N·m / g).

[0083] (2) The water absorption values ​​(g / m2) of the corrugated base papers prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were measured according to the relevant methods in GB / T 1540-2002 Determination of water absorption of paper and paperboard - Cobber method. 2 ).

[0084] The test results are shown in Table 1.

[0085] Table 1

[0086] Group <![CDATA[Quantitative (g / m 2 )]]> Transverse ring pressure index (N·m / g) <![CDATA[Water absorption value (g / m 2 )]]> Example 1 130 8.9 23.4 Example 2 140 9.2 21.6 Example 3 165 9.6 21.2 Comparative Example 1 140 7.1 24.6 Comparative Example 2 140 6.8 27.2 Comparative Example 3 140 7.7 35.3 Comparative Example 4 140 8.1 33.7

[0087] As shown in Table 1, the high-strength corrugated paper prepared by Examples 1 to 3 of the present invention has a basis weight of 130 to 165 g / m 2 It has high ring crush strength, the transverse ring crush index is between 8.9 and 9.6 N·m / g, and the water absorption value is less than 24g / m 2 , far exceeding the national standard, with excellent overall performance. The corrugated cardboard produced is not easy to deform and break when under pressure, and has a low water absorption value, which can prevent the corrugated cardboard from softening or losing strength in a high humidity environment, which is beneficial to maintaining the structural integrity of the packaging.

[0088] In Comparative Examples 1 to 4, when the raw materials and preparation parameters in the preparation process of the present invention were changed, the ring crush strength of the obtained corrugated paper decreased, the water absorption value increased, and the overall performance decreased to varying degrees.

[0089] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A production process for recycling high-strength corrugated paper from waste paper, It is characterized in that The method comprises the following preparation steps: S1. After removing impurities from the recycled waste paper, soak it in water, adjust the pulp concentration and process it with a high-concentration hydraulic pulper, then add biological enzymes, adjust the pH and perform enzymolysis to obtain pretreated pulp; S2, adding a surfactant to the pretreated slurry obtained in step S1, performing an ultrasonic treatment once, then adding a composite auxiliary agent, stirring evenly, and performing a second ultrasonic treatment; S3, the pulp obtained in step S2 is removed by a remover, then diluted with water, formed into sheets, pressed, and pre-dried to obtain pre-dried corrugated paper; S4, applying double-sided sizing to the pre-dried corrugated paper obtained in step S3 with a surface sizing chemical, and drying the paper to obtain the corrugated paper; The surface sizing chemicals in step S4 are composed of the following components and their weight proportions: 25-35 parts of grafted butyl acrylate starch, 7-10 parts of guar gum, 3-5 parts of nano calcium carbonate, 8-10 parts of polyvinyl alcohol, and 150-200 parts of water; The preparation method of the grafted butyl acrylate starch comprises the following steps: Add 4-6 times the mass of distilled water to corn starch and mix evenly, heat to 85-95°C, and continue stirring until the starch paste is completely dissolved to form a uniform starch paste; add butyl acrylate, ammonium persulfate and N,N-dimethylformamide to the starch paste and mix well; then place the mixture in a constant temperature water bath, react for 4-6 hours at a temperature of 60-70°C and a stirring speed of 80-100 r / min; after the reaction is completed, wash the product with deionized water, then centrifuge and dry to obtain; The amount of butyl acrylate is 22-26% of the mass of corn starch, the amount of ammonium persulfate is 1.2-1.6% of the mass of corn starch, and the amount of N,N-dimethylformamide is 7-12% of the mass of corn starch; The biological enzyme in step S1 is a combination of cellulase, xylanase and α-amylase; the amount of the biological enzyme added in step S1 is 0.2~0.3% of the absolute dry weight of the pulp, the enzymatic hydrolysis temperature is 42~50°C, the enzymatic hydrolysis time is 4~6 h, the pH is adjusted to 6.5~7.5, and the stirring speed during the enzymatic hydrolysis process is 200~300 r / min; The surfactant in step S2 is composed of sodium xylene sulfonate and 1,3-propylene glycol in a weight ratio of 2 to 4:1; The composite auxiliary agent in step S2 is a combination of two or more of polyacrylamide, polyethyleneimine, alkyl ketene dimer, carboxymethyl starch, and carboxymethyl cellulose; The frequency of the first ultrasonic treatment in step S2 is 60-80 kHz, and the ultrasonic time is 20-30 min. The frequency of the second ultrasonic treatment is 30-50 kHz, and the ultrasonic time is 30-40 min.

2. The production process of high-strength corrugated paper recycled from waste paper according to claim 1, It is characterized in that In the step S1, the waste paper after impurities removal is soaked in water for 5-8 hours, the pulp concentration is adjusted to 10-15%, and the processing time in the high-consistency hydraulic pulper is 20-30 minutes.

3. The production process of high-strength corrugated paper recycled from waste paper according to claim 1, It is characterized in that The amount of surfactant added in step S2 is 0.3-0.7% of the weight of the pretreated pulp obtained in step S1.

4. The production process of high-strength corrugated paper recycled from waste paper according to claim 1, It is characterized in that The added amount of the composite auxiliary agent is 0.3-0.5% of the weight of the pretreated pulp in step S1.

5. The production process of high-strength corrugated paper recycled from waste paper according to claim 1, It is characterized in that The preparation method of the surface sizing chemical in step S4 comprises the following preparation steps: Dissolve the grafted butyl acrylate starch in water, stir evenly, then add polyvinyl alcohol, guar gum and nano calcium carbonate while stirring, stir for 1 to 2 hours, and then leave for 2 to 3 hours to obtain the product.

6. The production process of high-strength corrugated paper recycled from waste paper according to claim 1, It is characterized in that In step S3, the pulp after deslagging is diluted to a pulp concentration of 0.8-1.5%; the sizing amount in step S4 is 8 g / m 2 The drying temperature is 105~110℃, and the moisture content of the corrugated paper after drying is 7.5 wt%.

Citation Information

Patent Citations

  • Method for preparing starch-based water-resistant adhesive for corrugated board production

    CN102533182A

  • Paper making method with pulp and product of high-surface-intensity offset printing paper

    CN103526630A

  • Method for preparing regenerated corrugated paper base paper through rosin modified starch surface sizing

    CN107354788A

  • Preparation method of sizing agent for corrugated paper

    CN108824077A

  • Ultra-low quantitative flame-retardant corrugated isolation paper and preparation method thereof

    CN109811577A